    Passive daytime radiative cooling coatings with renewable self-cleaning functions

    2024-04-05 02:28:16QinWuYuoCuiGuifengXiJinlongYngShumingDuXinhongXiongLiYngDongXuXuDengJixiCui
    Chinese Chemical Letters 2024年2期

    Qin Wu ,Yuo Cui, ,Guifeng Xi, ,Jinlong Yng ,Shuming Du ,Xinhong Xiong ,Li Yng,Dong Xu,Xu Deng,Jixi Cui,,*

    a Institute of Fundamental and Frontier Sciences,University of Electronic Science and Technology of China,Chengdu 610054,China

    b Yangtze Delta Region Institute (Huzhou),University of Electronic Science and Technology of China,Huzhou 313001,China

    c Beijing Key Laboratory of Power Generation System Functional Material,CHN Energy New Energy Technology Research Institute Ltd.,Beijing 102209,China

    d Institute for Advanced Study,Chengdu University,Chengdu 610106,China

    Keywords: Superhydrophobic Passive radiative cooling Wearing Regeneration Glass resin armor

    ABSTRACT Passive daytime radiative cooling (PDRC) technology is emerging as one of the most promising solutions to the global problem of spacing cooling,but its practical application is limited due to reduced cooling effectiveness caused by daily wear and tear,as well as dirt contamination.To tackle this problem,we report a novel strategy by introducing a renewable armor structure for prolonging the anti-fouling and cooling effectiveness properties of the PDRC coatings.The armor structure is designed by decorating fluorinated hollow glass microspheres (HGM) inside rigid resin composite matrices.The HGM serve triple purposes,including providing isolated cavities for enhanced solar reflectance,reinforcing the matrices to form robust armored structures,and increasing thermal emittance.When the coatings are worn,the HGM on the surface expose their concave cavities with numerous hydrophobic fragments,generating a highly rough surface that guarantee the superhydrophobic function.The coatings show a high sunlight reflectance (0.93) and thermal emittance (0.94) in the long-wave infrared window,leading to a cooling of 5 °C below ambient temperature under high solar flux (~900 W/m2).When anti-fouling functions are reduced,they can be regenerated more than 100 cycles without compromising the PDRC function by simple wearing treatment.Furthermore,these coatings can be easily prepared using a one-pot spray method with low-cost materials,exhibit strong adhesion to a variety of substrates,and demonstrate exceptional environmental stability.Therefore,we anticipate their immediate application opportunities for spacing cooling.

    Space cooling has become a global concern as it consumes 15% of global electricity and yields 10% greenhouse gas emissions[1].Many measures are being pursued to address this issue,and one of the most promising approaches is passive daytime radiative cooling (PDRC) technology.This green technology is usually based on coatings that reflect sunlight in the wavelength range of 0.3-2.5 μm and radiate heat to the cold outer space through the atmosphere’s long-wave infrared (LWIR) transmission window(wavelength range of 8-13 μm) [2-12].Recently,such a combination has been achieved in cheap and scalable polymer paints by introducing cavities or particles into coating matrices to induce light scattering [4,9,13-18].These coatings show excellent spectroscopic results,but their practical applications are still rare.It is mainly due to their poor longevity in PDRC function as a consequence of solid contaminants (dust or other microparticles) or daily wear and tear.Solid contaminants will quickly accumulate on coatings surfaces to decrease the sunlight reflectance and thermal-infrared emission [19],while inevitable daily wear and tear would damage the delicate structures.Besides longevity,weak mechanical properties,low adhesion on substrates,and poor water-repellency may also constitute the determinate reasons for disenabling the practical use of these materials.Therefore,it is still desirable to develop robust PDRC coatings with a mechanism to prevent contamination.

    Lotus leaf-like superhydrophobicity represents one of the most powerful self-cleaning strategies [20-22].Recently,it has been integrated into PDRC coatings for elongating surface cooling performance.Two strategies have been developed to this end,including covering superhydrophobic structures/layers on PDRC coatings [23-25] or utilizing the intrinsic porous/heterogeneous nature of PDRC coatings to create rough surfaces [26-32].The former frequently involves complicated fabrication and interfacial issues due to the bilayer structures.Introducing new layers/components would also reduce the PDRC function due to their sunlight absorption or low sunlight reflectance.In contrast,the latter mainly depend on the porous structures that provide PDRC matrices and superhydrophobic rough surfaces.Although this class of coatings can be prepared by facile one-pot methods,the balance of two functions often leads to compromise in cooling performance.Moreover,only modest robustness in superhydrophobicity can be achieved in these systems.Since preparing superhydrophobic surfaces mechanically robust enough for practical use is already an endless task for materials scientists,it is challenging to design PDRC coatings combining excellent radiative cooling effect and robust superhydrophobicity without tradeoffs in other performance of a paint required for practical applications.

    Herein,we propose an alternative strategy to address this issue.Rather than preventing mechanical wearing,we utilize this inevitable phenomenon to renew superhydrophobicity.Fig.1a shows our design to realize this concept.The polymer-composite coatings consist of hollow glass microspheres (HGM) and resins.HGM are introduced for three purposes,i.e.,providing isolated cavities to induce sunlight reflectance,reinforcing the coatings,and forming wearing-renewed rough surfaces.Sunlight reflectance occurs on interfaces generated by media with different reflection indices(RI).Although both cavities and particles can induce such heterogeneities,cavities could be the preferable option because of two reasons: (1) The RI difference between air and solid matrices is large (0.4-0.5) in comparison to typical particle-based coatings(0.1-0.2,such as typical BaSO4-acylate paints);(2) Cavities would not show any absorption of sunlight while particles fillers (e.g.,TiO2) typically exhibit weak absorption.This advantage has been proved by highly porous polymer systems [11].However,high cavity content would make the substrates brittle or fluffy.In contrast,the use of HGM not only allows for tunable porosity but would also reinforce the coatings because of their rigid nature.More importantly,the structures of HGM-containing composites allow for(re)generation of superhydrophobic surfaces with enhanced sunlight reflectance performance when daily wear and tear occurs.Briefly,the composite coatings are typically robust.After severe abrasion strong enough to remove the resin,the HGM fixed in the resin would be broken to reveal their highly concave cavities and form strong glass armor.The fragments generated in the wearing would deposit into the cavities,creating highly rough surfaces.The surfaces would also provide more interfaces for sunlight reflectance.With this design,we get a high sunlight reflectance of 0.93 and a high emittance of 0.94 at the LWIR window as well as renewable,robust superhydrophobicity.The coatings can be prepared by one-pot spray from cheap materials,showing good adhesion to various substrates (3 MPa),high compression strength(26 MPa),and excellent environmental stability.

    Fig.1.Design and preparation of HGM-FHA coatings.(a) Diagrammatic representation of the design concept for the HGM-FHA coatings.(b) Photograph of a HGM-FHA coating on a 30 cm × 30 cm glass plate (inset,water contact angle image).(c) SEM image of the surface of a raw coating.SEM vertical cross-section (d) and surface (e)images of a HGM-FHA coating.All HGM-FHA coatings contain 80 wt% HGM and have an average HGM size of~8 μm.

    Fluorinated hydroxy acrylic resin (FHA,one of the most common resins used for paints,see Experimental Section 3.1 and Table S1 in Supporting information for their synthesis and characterization) were selected as polymer matrices because of their excellent adhesion and hydrophobic nature (Fig.S1 in Supporting information).HGM were modified with perfluoroalkyl chains to provide hydrophobic surfaces (Fig.S2 and Experimental Section 3.2 in Supporting information).The mixture of FHA,HGM,curing agent,and solvent in a mass ratio of 1:4:0.2:11 was used as the typical precursor suspension to show our idea.This suspension could be coated on various substratesviafacile spraying,rolling,or brushing(Movie S1 in Supporting information).After drying in air for 2 d,raw HGM-FHA coatings were obtained.A scraper was used in our case to control the thickness of the coatings for study,and sandpapers were employed to wear the raw coatings to (re)generate superhydrophobic surfaces (Fig.S3 in Supporting information).This simple method allowed us to prepare large coatings on different substrates,such as a 30 cm × 30 cm coating on glass (Fig.1b).

    We monitored the forming process of the rough structures using scanning electron microscopy (SEM).As shown in Fig.1c,the raw coatings display moderately rough surfaces made from polymer-covered HGM.The surfaces were hydrophobic,showing a water contact angle (WCA) of 116° and a water rolling angle (WRA)of>20°.Sandpaper-wearing treatment would break the HGM on the surfaces,exposing their hollow structures (Fig.1d).Fine fragments were observed in the concave cavities (Fig.1e).These fragments felled with the hydrophobic side up (Fig.S4 in Supporting information).As a result of such highly rough structures,the surfaces display a high WCA of 154° and a low WRA of 3°,indicating superhydrophobicity.The coatings also exhibit exceptional dynamic wettability,as evidenced by the complete bouncing off of water droplets from the surface captured by a high-speed video camera(Fig.S5 and Movie S2 in Supporting information).

    With the coatings in our hands,we first evaluated their optical properties.Fig.2a shows the typical reflection of the HGM-FHA coatings (80% HGM mass fraction) in the sunlight spectrum (0.3-2.5 μm) and LWIR transmission window (8-13 μm).The typical samples contained spherical HGM with an average size of~8 μm and a wide distribution (1.44,Fig.S6 in Supporting information).They provided a broad-spectrum scattering efficiency across the entire solar wavelengths due to the high-order Mie resonance excitations,which resulted in a high reflection of sunlight (~93% for a 0.8-mm-thick film).

    Fig.2.Characterization of the HGM-FHA coatings.(a) Measured reflectance spectra of the HGM-FHA coatings with 80 wt% HGM (average HGM size of~8 μm) from the ultraviolet to the mid-infrared (Inset,comparison of the light scattering behavior between raw coatings and HGM-FHA coatings).(b) Average reflectance and emittance of the HGM-FHA coatings with different HGM (average HGM size of~8 μm) mass fractions.All the coatings have thicknesses of 0.8 mm.(c) Reflectance and emittance of HGM-FHA coatings with different thicknesses.The samples contain 80 wt% HGM with an average size of~8 μm.(d) The optical properties of the HGM-FHA coatings with different diameters of HGM.The samples contain 80 wt% HGM and have thicknesses of 0.8 mm.(e) The wetting properties of the HGM-FHA coatings with different HGM(average HGM size of~8 μm) mass fractions.(f) The wetting properties of the HGM-FHA coatings with different diameters of HGM.The samples contain 80 wt% HGM and have thicknesses of 0.8 mm.

    Interestingly,the wearing treatment enhanced the reflection of sunlight (1% higher).It was attributed to the extra light scattering induced by these fine fragments in the concaves created by wear (inset in Fig.2a).The sample also possessed a nearly saturated emissivity of>0.94 in the LWIR transmission window.We had employed attenuated total reflectance-Fourier transform infrared spectroscopy (ATR-FTIR) to study the absorption of the pristine materials and composite coatings in the LWIR transmission window.The composite coatings exhibit strong emittances in the atmospheric transparency window due to the stretching vibrations of Si-O-Si (HGM) and C-O-C (FHA) bonds (Fig.S7 in Supporting information).Furthermore,the HGM were mainly composed of alkali lime borosilicate with inherent absorption at the phonon-polariton resonance wavelength of 9.7 μm.As a result of these absorption,the obtained hybrid coating showed highly broadband near-normal emissions across the LWIR transparency window.

    The optical properties of the composite coatings were influenced by different factors,including the fraction of HGM in the coatings,coating thickness,HGM sizes,and the type of polymers used.As shown in Fig.2b and Fig.S8a (Supporting information),increasing HGM fraction promotes sunlight reflection,while only a minor enhancement in emissivity in the LWIR window is observed.It was because HGM determined the system’s porosity.Besides HGM fraction,increasing coating thickness also favors sunlight reflection and thermal emittance in the range of 8-13 μm until a value of>0.6 mm (Fig.2c and Fig.S8b in Supporting information).To investigate the influence of HGM sizes,we fabricated a series of composite coatings using HGM with average sizes ranging from 8 μm to 20 μm and compared their optical properties (Fig.S6).The sunlight reflectance of these coatings drops with increasing the HGM size (Fig.2d and Fig.S9 in Supporting information).In our system,the sunlight was reflected mainlyviaMie scattering.Increasing particle sizes beyond the sunlight wavelength would reduce the reflection [33,34].In contrast to these changes,tested three polymer matrices display similar sunlight reflectance and thermal emittance (Fig.S10 in Supporting information).We theoretically analyzed the relationship between sunlight reflectance and cooling power [3] by setting the average thermal emittance asE=0.94.It was found that the coatings could achieve a passive cooling effect when the average sunlight reflectance of the HGM-FHA coatings was greater than 0.9 (Fig.S11 in Supporting information).

    We then investigated the surface properties of these coatings with different structure parameters.At first,the surface roughness of the raw coatings increases with the HGM content (Fig.S12 Supporting information).These surfaces were not superhydrophobic yet until treated by wear in the case of>40% HGM were used (Fig.2e).We also change the HGM size to get different roughness surfaces (Fig.S13 in Supporting information).Larger HGM size would lead to slightly lower WCA and higher WRA(Fig.2f).The sandpaper mesh was critical for forming surface micro/nanostructures when these coatings were treated with sandpaper.Large mesh favored the formation of small fragments and thus high WCA.In particular,sandpaper with a mesh of>120 was required to get stable superhydrophobicity (Fig.S14 in Supporting information).Furthermore,we conducted washing experiment to prove the stability of these fragments (Fig.S15 in Supporting information).It was found that the surface maintained its superhydrophobicity for 10-min washing.We attributed to the small size of the cavities in the broken glass sphere which stored the fragments,and the fragments surface contained the low-surfaceenergy fluorinated polymer leading to the extremely low adhesion of the fragments to water droplets when in contact.

    In our design,rigid polymer matrices were used to ensure the occurrence of wearing-induced fracture.The obtained coatings show a high compression modulus of 26 MPa (Fig.S16 in Supporting information).The rigid shell of HGM,serving as a skeleton structure,significantly increased the compression strength of the material,making it resistant to abrasion and able to withstand external forces without collapsing.Furthermore,the rigid nature of the matrices was expected to favor energy absorption for HGM fragmentation.To confirm this hypothesis,we replaced the stiff polymers with elastic silicone,i.e.,the copolymer of polydimethylsiloxane and urea (uPDMS),to prepare the HGM-uPDMS composite coatings (Fig.S17a in Supporting information).Under the same wearing treatment,no HGM were broken since the elastic matrices could dissipate the shearing force by deformation.As a result of the absence of the fragment-based nanostructure,the HGMuPDMS coatings only reached a WCA of 148°,and their surfaces were even sticky to water droplets.We also found that using simple hydrophobic polymers as matrices might lead to other issues,such as low adhesion to the substrates.For example,polyvinylidene fluoride (PVDF) is a typical low-surface energy polymer often used to design PDRC coatings.It usually shows poor adhesion to the substrates.We prepared an HGM-PVDF composite coating to confirm this idea.Both the as-prepared and wearing-treated composite coatings were superhydrophobic.However,the adhesion of the coating was so weak that it directly peeled off from the glass substrate during drying (Fig.S17b in Supporting information).Such poor adhesion would significantly limit its application as a coating.Based on these studies,the HGM-FHA coatings with 80% HGM(average HGM size of~8 μm) mass fraction were selected as optimized samples for further investigation.

    Surface superhydrophobicity would be inevitably reduced in daily use,resulting in a remarkable decrease in the cooling effect of PDRC coatings.In our design,we proposed to utilize daily wearing to regenerate the self-cleaning function of the coatings.To probe the regeneration ability,we subjectively destroyed the structure of the HGM-FHA coatings by 3M tape peeling treatment.Briefly,a 3M tape was pasted on the coatings and peeled.It was found that the coatings were robust to suffer 40 peeling cycles without significant reduction in surface superhydrophobicity (low WRA).An evident increase in WRA occurred after 60 cycles of peeling (Fig.3a).Such decline was attributed to the removal of fragments (Fig.S18 in Supporting information),indicating the importance of fragments in surface properties.Besides structure damage,we also evaluated the deterioration of surface chemistry on coatings properties,using plasma to change surface chemistry.After 5 min irradiation,the coatings would change from superhydrophobic to hydrophilic (Fig.3b).The failure coatings could recover their surface properties by a simple sandpaper-wearing treatment (Movie S3 in Supporting information).In the treatment,the rigid polymer matrices were worn to expose the embedded HGM,which were then broken to regenerate the similar fragmentcontaining rough structure.As a demo of the regeneration process,we took a HGM-FHA coating with a thickness of 1.5 mm on a glass(2.5 cm × 2.5 cm) as an example.A weight of 100 g was attached to the back face of the sample with tape to form the test specimen.The coating surface was placed facing downwards on standard 800 mesh sandpaper and the test specimen was moved a distance of 3 cm for one regeneration cycle (Fig.S19 in Supporting information).After 100 regeneration cycles,the coating still retained its micro-nanostructure surface (Fig.3c).We plotted the regeneration cycle with the thickness of the coating as well as the WCA,WRC,and reflectance (Fig.3d).The coating thickness decreases with the regeneration cycle (4.3 μm/cycle).However,no apparent change occurs in either surface or optical properties.Based on the thickness-reflectance result (Fig.2c),we did not expect any change in optical properties until the coating thickness was reduced to<600 μm.

    Fig.3.Regeneration and mechanical properties of the HGM-FHA coatings.(a) Structure damage and regeneration: WCA and WRA of HGM-FHA coatings treated with 3M tape.(b) Chemical damage and regeneration: The photo of water drops on a sample at different states.(c) SEM images of a HGM-FHA coating before and after wearing treatment (100 regeneration cycles).(d) WCA,WRA,thickness and reflectance values of HGM-FHA coatings with regeneration cycle.(e) Adhesion strength of the HGM-FHA coatings on different kinds of substrate.The data were obtained by PosiTest Pull-off adhesion testing.All HGM-FHA coatings contain 80 wt% HGM and have an average HGM size of~8 μm.

    We systematically evaluated the practical applicability of our coatings by testing their adhesion stability with various substrates in different environments.Fig.3e shows the adhesion strengths of the coatings on ceramic,stainless steel,aluminum,and glass.The adhesion typically exceeded 3 MPa.This firm attachment was attributed to the formation of strong covalent bonds between coatings and substrates due to abundant functional groups(-NH-CO-O-,-COO-) in the matrices (Fig.S7) [35,36].For outdoor building applications,coating surfaces inevitably suffer from rain flushing,sun burning,and dust settling.To further evaluate the environmental stability of the coatings,we performed accelerated weathering tests based on the protocols of GB/T 9755-2014.As shown in Table S2 (Supporting information),the coatings met the standards of first-grade products,indicating their excellent practicability for use on external walls of buildings.

    To further demonstrate the potential of our HGM-FHA coatings,we conducted long-time outdoor experiments.The coatings were placed outside for one month in Chengdu,China,in a humid and hot climate,using a hydrophobic coating (WCA: 109°) made from similar compositions (fluorinated hydroxy acrylic resin and hollow glass beads) as a control.The HGM-FHA coatings maintain their optical properties while the sunlight reflectance of the control was significantly reduced after one month of outdoor exposure (reduced 23%,Figs.4a and b).The HGM-FHA coatings also retained a high WCA of>150° during the exposure period,suggesting excellent weather resistance.This stable superhydrophobicity also improved the antifouling property by making it easier to remove dust from the coating surfaces (Fig.4c).The stable superhydrophobicity increases the antifouling property,leading to much easier removal of dust deposited on the coating surfaces by wind and rain.In contrast,the control coating was easily contaminated and showed a decrease in reflectance,resulting in lower cooling performance than the HGM-FHA coatings (Fig.4d).The HGM-FHA coatings also had a superior self-cleaning property,as demonstrated by pouring carbon black on the coatings and observing how the water droplets cleaned the surfaces (Fig.S20 and Movie S4 in Supporting information).Outdoor tests under a condition with an average solar intensity of~900 W/m2,a relative humidity of~40% at noon,and an average wind speed of~1.0 m/s indicated that the HGM-FHA coatings could maintain an average temperature reduction of~5 °C below the ambient under direct sunlight (Fig.4e and Fig.S21 in Supporting information).Furthermore,in the hot summer weather(an average solar intensity of~1000 W/m2,a relative humidity of~41% at noon),the HGM-FHA coatings could show the temperature reduction of~10 °C at noon (Fig.S22 in Supporting information).This value corresponded to a theoretical net cooling power of 81.76 W/m2below the ambient under direct sunlight (Fig.S23 in Supporting information).Additionally,the coatings have a low thermal conductivity of 0.113 W m-1K-1,which helped to suppress heat exchange with the ambient atmosphere (Fig.S24 in Supporting information).In contrast,the cooling performance of the control decreased significantly after being contaminated due to its lack of efficient self-cleaning function (an average temperature elevation of~2.6 °C was observed compared to the initial state).

    Fig.4.The practical outdoor performance of HGM-FHA coatings.(a) The reflectance spectra of different coatings were compared to show the effect of outdoor exposure for one month.(b) Change in the average reflectance and emittance with time in outdoor exposure.(c) Change in the WCA and WRA with time in outdoor exposure.(d) The IR images and photos of coatings at 1:30 pm under direct solar radiation.(e) Temporal temperature data of the air and the hybrid coating under direct sunlight in Chengdu(date,7 May 2022,UTC+8) and solar irradiance measured in the experiment.HGM-FHA coatings contain 80 wt% HGM with average size of~8 μm and have thicknesses of 0.8 mm.Control coating also contain 80 wt% hollow glass beads with average size of~8 μm and have thicknesses of 0.8 mm.

    In summary,we have presented a class of robust PDRC coatings with regenerable superhydrophobicity.The typical HGM-FHA coatings display a remarkable 93% sunlight reflectance and 94%mid-infrared emissivity and can effectively reduce the temperature below ambient by~5 °C in direct sunlight.More importantly,they can regenerate their self-cleaning properties through a wear-induced reformation of superhydrophobic surfaces without any tradeoff in optical properties.We have demonstrated that this function can ensure long-lasting cooling efficiency in the outdoor environment.Since the coatings can be prepared by a simple spraying process and display good adhesion to various surfaces and excellent environmental stability,we envision their immediate application opportunities in different outdoor objects.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgments

    This work was supported by the National Natural Science Foundation of China (Nos.52003035,52203135 and 51973023) and the CHN Energy Group Project (No.GJNY-21-183).

    Supplementary materials

    Supplementary material associated with this article can be found,in the online version,at doi:10.1016/j.cclet.2023.108687.

    国产高潮美女av| 九九热线精品视视频播放| 欧美日本亚洲视频在线播放| 亚洲国产精品合色在线| 日本三级黄在线观看| 别揉我奶头~嗯~啊~动态视频| 男女之事视频高清在线观看| 国产av不卡久久| 国产免费av片在线观看野外av| 久久精品91蜜桃| 日日摸夜夜添夜夜添小说| 级片在线观看| 欧美色视频一区免费| 亚洲精华国产精华精| 精品免费久久久久久久清纯| 长腿黑丝高跟| 亚洲美女视频黄频| av在线蜜桃| 曰老女人黄片| 欧美高清成人免费视频www| 99久久成人亚洲精品观看| 欧美3d第一页| 亚洲国产色片| 十八禁人妻一区二区| 69av精品久久久久久| 舔av片在线| 一二三四社区在线视频社区8| 香蕉av资源在线| 97人妻精品一区二区三区麻豆| 一区二区三区高清视频在线| 久久久久免费精品人妻一区二区| 欧美大码av| 欧美黄色淫秽网站| 男人和女人高潮做爰伦理| 国产一区二区在线av高清观看| 一级a爱片免费观看的视频| 午夜福利在线在线| 一级黄色大片毛片| 中文资源天堂在线| 啦啦啦韩国在线观看视频| www.精华液| 欧美丝袜亚洲另类 | 在线视频色国产色| 精品福利观看| 国产aⅴ精品一区二区三区波| 夜夜夜夜夜久久久久| 免费人成视频x8x8入口观看| 99国产综合亚洲精品| 国产免费av片在线观看野外av| 亚洲专区中文字幕在线| 欧美绝顶高潮抽搐喷水| 啦啦啦观看免费观看视频高清| 欧美国产日韩亚洲一区| 女人被狂操c到高潮| 午夜精品久久久久久毛片777| 最近最新免费中文字幕在线| 狠狠狠狠99中文字幕| 制服丝袜大香蕉在线| 香蕉av资源在线| 日本免费一区二区三区高清不卡| 天堂影院成人在线观看| 国产精品精品国产色婷婷| 男人舔女人下体高潮全视频| 欧美中文日本在线观看视频| 国产黄色小视频在线观看| 国产精品日韩av在线免费观看| 美女黄网站色视频| 久久久水蜜桃国产精品网| 九九久久精品国产亚洲av麻豆 | 日韩成人在线观看一区二区三区| 成人国产一区最新在线观看| 亚洲中文字幕一区二区三区有码在线看 | 成年免费大片在线观看| 久久亚洲真实| 亚洲精华国产精华精| 听说在线观看完整版免费高清| 国产91精品成人一区二区三区| 五月伊人婷婷丁香| 97碰自拍视频| 人妻夜夜爽99麻豆av| 日韩精品中文字幕看吧| 亚洲一区二区三区不卡视频| 国产av麻豆久久久久久久| 一级毛片女人18水好多| 级片在线观看| 久久午夜综合久久蜜桃| 国产精品亚洲av一区麻豆| 一进一出抽搐gif免费好疼| 熟女少妇亚洲综合色aaa.| 精品久久久久久久久久久久久| 丰满人妻熟妇乱又伦精品不卡| 欧美另类亚洲清纯唯美| 色视频www国产| 非洲黑人性xxxx精品又粗又长| 一本一本综合久久| 久久午夜亚洲精品久久| 精品久久久久久久末码| 亚洲五月天丁香| 国产伦人伦偷精品视频| 舔av片在线| 亚洲av熟女| 亚洲黑人精品在线| 国产高清有码在线观看视频| 久久久精品欧美日韩精品| 最近视频中文字幕2019在线8| 中文字幕熟女人妻在线| 久久久水蜜桃国产精品网| 九色成人免费人妻av| 天堂动漫精品| 哪里可以看免费的av片| 国产三级黄色录像| 久久久国产精品麻豆| 九色成人免费人妻av| 俄罗斯特黄特色一大片| 一夜夜www| 偷拍熟女少妇极品色| 一个人免费在线观看电影 | 成人18禁在线播放| 精品久久久久久久久久久久久| 久久午夜综合久久蜜桃| 亚洲在线自拍视频| 久久人妻av系列| 男女那种视频在线观看| 99久久精品一区二区三区| 免费一级毛片在线播放高清视频| 亚洲 欧美一区二区三区| 好看av亚洲va欧美ⅴa在| 亚洲国产欧美网| 亚洲自偷自拍图片 自拍| 国产精品国产高清国产av| www日本在线高清视频| 日本熟妇午夜| 757午夜福利合集在线观看| 亚洲午夜理论影院| 久久精品亚洲精品国产色婷小说| 国产熟女xx| 亚洲最大成人中文| 欧美不卡视频在线免费观看| 婷婷亚洲欧美| 熟女电影av网| 嫩草影视91久久| 久久欧美精品欧美久久欧美| 午夜福利18| 欧美av亚洲av综合av国产av| 丁香欧美五月| 国产精品久久久av美女十八| 欧美在线黄色| 国产欧美日韩一区二区三| 久久99热这里只有精品18| 日韩欧美三级三区| 淫秽高清视频在线观看| 婷婷精品国产亚洲av| 国产av麻豆久久久久久久| 免费在线观看日本一区| 麻豆一二三区av精品| 欧美绝顶高潮抽搐喷水| 成人特级黄色片久久久久久久| 18禁观看日本| 国产男靠女视频免费网站| 欧美在线黄色| 色吧在线观看| 黄色女人牲交| 国产成年人精品一区二区| 久久久久久国产a免费观看| 我要搜黄色片| 午夜福利视频1000在线观看| 亚洲人成伊人成综合网2020| 国产高清三级在线| 成人精品一区二区免费| 亚洲专区字幕在线| 亚洲国产高清在线一区二区三| 国内精品美女久久久久久| 日韩欧美精品v在线| 黄色女人牲交| 日韩三级视频一区二区三区| 少妇裸体淫交视频免费看高清| 丝袜人妻中文字幕| 少妇的丰满在线观看| 欧美大码av| 亚洲专区字幕在线| 动漫黄色视频在线观看| 亚洲精品在线观看二区| 少妇人妻一区二区三区视频| 国产真人三级小视频在线观看| 欧美黑人欧美精品刺激| 黄色视频,在线免费观看| 久久精品91无色码中文字幕| 99热6这里只有精品| 在线播放国产精品三级| 丁香六月欧美| 国产精品国产高清国产av| 97碰自拍视频| 国产免费av片在线观看野外av| 欧美成人性av电影在线观看| 又大又爽又粗| 国产麻豆成人av免费视频| 老司机午夜福利在线观看视频| 欧美一级a爱片免费观看看| 精品福利观看| 亚洲av成人不卡在线观看播放网| 少妇丰满av| 88av欧美| 俄罗斯特黄特色一大片| 久久久久九九精品影院| xxxwww97欧美| 日韩欧美国产在线观看| 99久久精品一区二区三区| 亚洲专区国产一区二区| 麻豆久久精品国产亚洲av| 日韩成人在线观看一区二区三区| 最新中文字幕久久久久 | 免费大片18禁| a级毛片在线看网站| 亚洲人成电影免费在线| 日韩欧美在线二视频| 香蕉久久夜色| 欧美日韩综合久久久久久 | 一区二区三区国产精品乱码| 亚洲国产精品合色在线| 精品电影一区二区在线| 精品国产三级普通话版| 久久久久久久午夜电影| 最近最新中文字幕大全免费视频| 成人av在线播放网站| 色尼玛亚洲综合影院| 真人做人爱边吃奶动态| 一区二区三区激情视频| 色噜噜av男人的天堂激情| 国产午夜精品久久久久久| 久久久久九九精品影院| 精品久久蜜臀av无| 一区二区三区国产精品乱码| 亚洲专区国产一区二区| 女人高潮潮喷娇喘18禁视频| 丰满人妻一区二区三区视频av | 国产爱豆传媒在线观看| 久久中文看片网| 嫩草影院入口| 亚洲第一欧美日韩一区二区三区| 日日夜夜操网爽| 精品不卡国产一区二区三区| 一级a爱片免费观看的视频| 欧美一区二区国产精品久久精品| 亚洲五月婷婷丁香| 美女扒开内裤让男人捅视频| 免费在线观看视频国产中文字幕亚洲| 黄色 视频免费看| 日韩欧美一区二区三区在线观看| 我要搜黄色片| 久久这里只有精品19| 看免费av毛片| 免费无遮挡裸体视频| 亚洲美女黄片视频| 90打野战视频偷拍视频| 两性夫妻黄色片| 国产av一区在线观看免费| 久久久久国产精品人妻aⅴ院| 又粗又爽又猛毛片免费看| 亚洲av美国av| 午夜福利在线观看吧| 男女床上黄色一级片免费看| АⅤ资源中文在线天堂| 亚洲七黄色美女视频| 美女高潮的动态| 免费一级毛片在线播放高清视频| 日韩中文字幕欧美一区二区| 国产精品久久久av美女十八| 国产一区二区三区在线臀色熟女| 日韩有码中文字幕| 精品久久久久久久久久免费视频| 在线十欧美十亚洲十日本专区| 欧美一区二区精品小视频在线| 国产精品,欧美在线| 一夜夜www| 久久久国产成人精品二区| 国产亚洲精品一区二区www| 999久久久国产精品视频| 欧美黄色片欧美黄色片| 久久亚洲真实| 欧美另类亚洲清纯唯美| 黑人操中国人逼视频| 999久久久国产精品视频| 国产欧美日韩精品亚洲av| 日韩欧美免费精品| 日日干狠狠操夜夜爽| 亚洲成a人片在线一区二区| 成人精品一区二区免费| 一本综合久久免费| 在线观看免费视频日本深夜| av天堂中文字幕网| 999精品在线视频| 黄片小视频在线播放| 69av精品久久久久久| 久久久久国产一级毛片高清牌| 精品久久久久久久人妻蜜臀av| 一区二区三区激情视频| 亚洲片人在线观看| 搡老妇女老女人老熟妇| 成年免费大片在线观看| 亚洲成av人片在线播放无| 此物有八面人人有两片| 久久精品影院6| 日本一二三区视频观看| 国产aⅴ精品一区二区三区波| 亚洲精品一卡2卡三卡4卡5卡| www日本黄色视频网| 噜噜噜噜噜久久久久久91| 欧美色欧美亚洲另类二区| 国产激情欧美一区二区| 每晚都被弄得嗷嗷叫到高潮| АⅤ资源中文在线天堂| 久久精品91无色码中文字幕| 欧洲精品卡2卡3卡4卡5卡区| 国产精品乱码一区二三区的特点| 国产一级毛片七仙女欲春2| 91麻豆精品激情在线观看国产| 免费搜索国产男女视频| 欧美一级毛片孕妇| 亚洲专区字幕在线| 天天躁狠狠躁夜夜躁狠狠躁| 嫩草影院精品99| 久久这里只有精品19| 精品久久久久久久人妻蜜臀av| 黄色 视频免费看| 一二三四社区在线视频社区8| 最近在线观看免费完整版| 人妻丰满熟妇av一区二区三区| 在线a可以看的网站| 国产高清激情床上av| 啪啪无遮挡十八禁网站| 桃色一区二区三区在线观看| 久久久久久久久中文| www.自偷自拍.com| 露出奶头的视频| 中文字幕精品亚洲无线码一区| 国产伦精品一区二区三区四那| 黄色 视频免费看| 波多野结衣高清作品| 欧美日韩一级在线毛片| 真人做人爱边吃奶动态| 人妻夜夜爽99麻豆av| АⅤ资源中文在线天堂| bbb黄色大片| 日韩欧美在线乱码| 午夜福利18| 一个人免费在线观看电影 | 国内精品美女久久久久久| 亚洲精品美女久久av网站| 可以在线观看的亚洲视频| 欧美高清成人免费视频www| 村上凉子中文字幕在线| 欧美成人性av电影在线观看| www.熟女人妻精品国产| 亚洲成人免费电影在线观看| 国产免费av片在线观看野外av| 久久久国产成人免费| 99精品在免费线老司机午夜| 日韩欧美国产一区二区入口| 国产精品精品国产色婷婷| 老司机福利观看| 在线a可以看的网站| 床上黄色一级片| 在线观看免费午夜福利视频| 免费一级毛片在线播放高清视频| 伊人久久大香线蕉亚洲五| 制服丝袜大香蕉在线| 日本三级黄在线观看| 三级男女做爰猛烈吃奶摸视频| 欧美黑人欧美精品刺激| 真人一进一出gif抽搐免费| 可以在线观看毛片的网站| 91字幕亚洲| 欧美性猛交黑人性爽| 国产日本99.免费观看| 91在线观看av| 成人三级黄色视频| 亚洲黑人精品在线| 观看免费一级毛片| 国产高潮美女av| 午夜亚洲福利在线播放| 蜜桃久久精品国产亚洲av| 精品国产超薄肉色丝袜足j| 成年女人永久免费观看视频| 亚洲欧美精品综合久久99| 婷婷精品国产亚洲av| 97超视频在线观看视频| 一级作爱视频免费观看| 黑人操中国人逼视频| 亚洲片人在线观看| 好男人在线观看高清免费视频| 在线观看舔阴道视频| www日本在线高清视频| 美女黄网站色视频| 亚洲欧美精品综合久久99| 国产高清视频在线播放一区| 国产精品久久久久久人妻精品电影| xxx96com| 欧美日本亚洲视频在线播放| 国产精品久久久久久人妻精品电影| 人妻丰满熟妇av一区二区三区| 日韩欧美精品v在线| 久久亚洲真实| 人人妻人人看人人澡| 最近最新免费中文字幕在线| 在线观看一区二区三区| 美女免费视频网站| 中文字幕熟女人妻在线| 91麻豆av在线| 亚洲精品在线美女| 舔av片在线| 在线播放国产精品三级| 国产午夜福利久久久久久| 一个人免费在线观看的高清视频| 精品午夜福利视频在线观看一区| 亚洲精品在线美女| 精品国产乱码久久久久久男人| 丰满人妻熟妇乱又伦精品不卡| 伊人久久大香线蕉亚洲五| 日韩av在线大香蕉| 精品国产乱子伦一区二区三区| 人人妻人人澡欧美一区二区| 免费搜索国产男女视频| 一级毛片女人18水好多| 免费看a级黄色片| 久久九九热精品免费| 国产精品亚洲美女久久久| 国产蜜桃级精品一区二区三区| 在线观看免费午夜福利视频| 国产精品国产高清国产av| 国产一区二区激情短视频| 欧美成人免费av一区二区三区| av福利片在线观看| 亚洲av日韩精品久久久久久密| www国产在线视频色| 身体一侧抽搐| 一夜夜www| 精品久久久久久久人妻蜜臀av| 国产精品久久久久久精品电影| av女优亚洲男人天堂 | 草草在线视频免费看| 日本撒尿小便嘘嘘汇集6| 亚洲成人免费电影在线观看| 天天添夜夜摸| 久久人妻av系列| 久久国产乱子伦精品免费另类| 性色avwww在线观看| 亚洲国产日韩欧美精品在线观看 | 国产主播在线观看一区二区| 久9热在线精品视频| 曰老女人黄片| 国产精品九九99| 蜜桃久久精品国产亚洲av| 97碰自拍视频| 久久久久国内视频| 国产精品亚洲美女久久久| 国产精品一区二区三区四区久久| 午夜两性在线视频| 最好的美女福利视频网| 欧美日韩精品网址| 午夜福利18| 亚洲欧美日韩高清专用| 超碰成人久久| 久久久久久大精品| av黄色大香蕉| 日韩欧美精品v在线| 亚洲欧美日韩高清专用| www日本在线高清视频| 国产一区二区激情短视频| 成人亚洲精品av一区二区| 伊人久久大香线蕉亚洲五| 性色avwww在线观看| 欧美绝顶高潮抽搐喷水| 亚洲无线在线观看| 亚洲欧洲精品一区二区精品久久久| 午夜影院日韩av| 欧美成狂野欧美在线观看| 免费av不卡在线播放| 国产三级黄色录像| 国产精品 欧美亚洲| 亚洲美女黄片视频| bbb黄色大片| 精品一区二区三区视频在线观看免费| 成人午夜高清在线视频| 久久久久久久久中文| 国产成年人精品一区二区| 久久伊人香网站| 一级a爱片免费观看的视频| 午夜激情欧美在线| 精品一区二区三区视频在线观看免费| 欧美成人性av电影在线观看| 亚洲国产日韩欧美精品在线观看 | 精品国产三级普通话版| 最新在线观看一区二区三区| 亚洲成人久久性| 中亚洲国语对白在线视频| 亚洲无线观看免费| 国产一区二区激情短视频| 国产aⅴ精品一区二区三区波| 午夜福利18| 男插女下体视频免费在线播放| 亚洲欧美日韩东京热| 综合色av麻豆| 天堂网av新在线| 国产精品av视频在线免费观看| 成年免费大片在线观看| 午夜视频精品福利| 18禁裸乳无遮挡免费网站照片| 欧美不卡视频在线免费观看| 免费看美女性在线毛片视频| 国产1区2区3区精品| 波多野结衣高清作品| 国产久久久一区二区三区| 精华霜和精华液先用哪个| 99热6这里只有精品| 亚洲中文字幕一区二区三区有码在线看 | av黄色大香蕉| 亚洲成人中文字幕在线播放| 亚洲人成伊人成综合网2020| 精品国产超薄肉色丝袜足j| 两个人视频免费观看高清| 国产亚洲精品综合一区在线观看| 天堂√8在线中文| 久久热在线av| 亚洲精品色激情综合| www国产在线视频色| 久久欧美精品欧美久久欧美| 毛片女人毛片| 免费av不卡在线播放| 岛国在线免费视频观看| 国产午夜精品论理片| 90打野战视频偷拍视频| 国产探花在线观看一区二区| 国产91精品成人一区二区三区| 国产久久久一区二区三区| 午夜福利欧美成人| 国产视频内射| 99国产极品粉嫩在线观看| 欧美色视频一区免费| 亚洲 欧美 日韩 在线 免费| 国模一区二区三区四区视频 | 偷拍熟女少妇极品色| 国产激情偷乱视频一区二区| 九色成人免费人妻av| 啦啦啦观看免费观看视频高清| 国产私拍福利视频在线观看| 亚洲国产精品久久男人天堂| 国产一区二区在线观看日韩 | 老鸭窝网址在线观看| 国产精品国产高清国产av| 久久中文字幕人妻熟女| 亚洲国产日韩欧美精品在线观看 | 琪琪午夜伦伦电影理论片6080| 亚洲在线自拍视频| 免费av毛片视频| 观看免费一级毛片| 国产精品免费一区二区三区在线| 久久久久精品国产欧美久久久| 日韩欧美一区二区三区在线观看| 精品久久久久久久久久久久久| 黄色女人牲交| 国内久久婷婷六月综合欲色啪| 99久久精品热视频| www.熟女人妻精品国产| 草草在线视频免费看| 国产精品久久电影中文字幕| 国产伦精品一区二区三区视频9 | a级毛片在线看网站| 变态另类成人亚洲欧美熟女| 日本 欧美在线| 亚洲精品一卡2卡三卡4卡5卡| 国产精品 国内视频| h日本视频在线播放| 一个人观看的视频www高清免费观看 | 成年免费大片在线观看| 波多野结衣高清无吗| x7x7x7水蜜桃| 国产av在哪里看| 国产亚洲欧美98| 亚洲欧美日韩无卡精品| 成年女人毛片免费观看观看9| 亚洲成人中文字幕在线播放| 91麻豆av在线| 久久这里只有精品中国| 国内久久婷婷六月综合欲色啪| 一进一出好大好爽视频| 真实男女啪啪啪动态图| 亚洲18禁久久av| 精品国产乱子伦一区二区三区| 亚洲国产欧美人成| 日日夜夜操网爽| 亚洲熟妇熟女久久| 一级毛片精品| 亚洲av日韩精品久久久久久密| 国产亚洲精品av在线| 亚洲九九香蕉| 国内精品一区二区在线观看| 老鸭窝网址在线观看| 在线a可以看的网站| 日本一二三区视频观看| 1000部很黄的大片| bbb黄色大片| 久久欧美精品欧美久久欧美| 中文字幕精品亚洲无线码一区| 男人舔奶头视频| 美女高潮的动态| 色噜噜av男人的天堂激情| 亚洲国产精品久久男人天堂| 91麻豆精品激情在线观看国产| 久久久精品大字幕| 欧美日韩中文字幕国产精品一区二区三区| 成人精品一区二区免费| av在线天堂中文字幕| 中文资源天堂在线| 亚洲精品国产精品久久久不卡| 99久久99久久久精品蜜桃|