    Formation of L10-FeNi hard magnetic material from FeNi-based amorphous alloys

    2022-04-12 03:47:18YaocenWang汪姚岑ZiyanHao郝梓焱YanZhang張巖
    Chinese Physics B 2022年4期
    關(guān)鍵詞:張巖崇德

    Yaocen Wang(汪姚岑) Ziyan Hao(郝梓焱) Yan Zhang(張巖)

    Xiaoyu Liang(梁曉宇)4, Xiaojun Bai(白曉軍)1, and Chongde Cao(曹崇德)1,2,§

    1School of Physical Science and Technology,Northwestern Polytechnical University,Xi’an 710072,China

    2Innovation Center of Northwestern Polytechnical University in Chongqing,Chongqing 401135,China

    3Ningbo Institute of Materials Technology and Engineering,Chinese Academy of Sciences,Ningbo 315201,China

    4Institute of Multidisciplinary Research for Advanced Materials,Tohoku University,Sendai 980-8577,Japan

    Keywords: L10-FeNi,hard magnetic materials,amorphous alloys,ab initio simulation

    1. Introduction

    In recent years, hard magnetic materials, or commonly called hard magnets, are playing more and more important roles in many fields due to their high coercivities and large maximum magnetic energy products,such as magnetic recording media, motors, electronics, aerospace industry, etc.[1-4]The application of rare-earth hard magnets like Sm-Co[5,6]and Nd-Fe-B[7,8]causes the massive consumption of rareearth elements. This seriously affects the sustainability in future industry,and the costly raw materials also limit the application of high-performance hard magnets.

    Being a rare-earth free hard magnetic material,L10-FeNi has a chemically ordered structure, which is similar to facecentered-cubic (fcc) lattice with minor deformation alongcaxis and consists of alternating Fe and Ni atoms layers along the [001] direction. With excellent saturation magnetization(~1270 emu/cm3),[9]high uniaxial magnetic anisotropy (~1.3 J/cm3)and theoretically maximum magnetic energy product (~42 MGOe),[10,11]L10-FeNi appears to be a promising candidate to replace the rare-earth containing hard magnets.However, it was reported that L10-FeNi could be only stable below 320°C against the chemically disordered A1-FeNi phase, under which millions or billions of years are required for the atoms to be orderly arranged into L10-FeNi due to the lack of atomic diffusion ability, practically unacceptable for the industry.[12,13]Extreme conditions and modern fabrication techniques have been introduced for the artificial synthesis of L10-FeNi,such as high-energy particle irradiation,[9]alternate atom deposition,[14,15]pressure distortion,[16]and mechanical alloying,[17]but yet neither of them is promising for the mass production of materials with great application values. The small difference of free energy acting as phase transition driving force between A1-FeNi and L10-FeNi and the insufficient diffusion ability of Fe and Ni atoms below the order-disorder transition temperature, are always crucial problems for L10-FeNi fabrication,leaving almost no room for efficient fabrication of L10-FeNi.

    Recently, Makinoet al.[18]reported a new method for L10-FeNi preparation through annealing the FeNi-based amorphous ribbons(Fe42Ni41.3Si8B4P4Cu0.7)and the coercivity reached 700 Oe, which appeared to be promising for the mass production of L10-FeNi hard magnetic material. However,the process still needs to be improved since the obtained parameters of materials are still much lower than the commonly used rare-earth containing counterparts. The understanding of this process such as the crystallization mechanism,optimum process condition, and other influence factors are still unknown.In this work,the annealing process of Fe42Ni41.3Si8B4P4Cu0.7amorphous alloy was studied to clarify the phase transition sequence and the L10-FeNi formation mechanism during the process. Such understanding could contribute to the improvement of the process and lead to the practical fabrication of L10-FeNi rare-earth free hard magnet in the future.

    2. Experiment and simulation details

    Fe42Ni41.3Si8B4P4Cu0.7amorphous ribbons with 20 μm thick were prepared by melt-spinning technique with the ingot pre-alloyed from pure elements (99.9 mass% Fe, Ni and B,99.99 mass%Cu and Si)and 99.7 mass%Fe3P compound.The annealing process was performed by sealing the amorphous ribbons into argon filled quartz tubes and heating with a program-controlled furnace.

    The thermal properties of as-spun ribbons were investigated by a differential scanning calorimeter (DSC) at different heating rates of 5°C/min, 10°C/min, 20°C/min and 40°C/min,under argon atmosphere.The structures of as-spun and annealed ribbons were characterized via x-ray diffractometer (XRD). A transmission electron microscopy (TEM,FEI Talos F200X) was used for the microstructure measurements of annealed samples. The magnetic properties of asspun and annealed ribbons were examined by a vibrating sample magnetometer (VSM). Hysteresis loops were measured through applying magnetic fields in different directions with respect to the ribbon planes for the maximum coercivity value of each sample and the maximum magnetic field was 15000 Oe.

    Viennaab-initiosimulation pack(VASP)was used to perform simulation works based on the density functional theory.Interactions between particles (ions and electrons) were described with projector augmented-wave pseudopotentials on the Perdew-Burke-Ernzerhof (PBE) type generalized gradient approximation basis. Canonical ensemble was applied as the number of atoms, the sampling volume and the temperature were configured. TheK-mesh was set to be 9×9×9 for the simulation of crystalline structure. The temperature was controlled by Nos′e thermostat.[19]

    The following is the configuration of the simulation processes. The crystalline structures were initially configured as perfect L10-FeNi lattice with 32 atoms. Structural relaxations were performed with or without the cases of Si or Co inclusion. The original and stabilized structures were then subjected to the calculation of system energy and uniaxial magneto-crystalline anisotropy. The temperature in all simulation processes was set to be 300 K if needed.

    3. Results and discussion

    3.1. Thermal properties of the amorphous alloy

    The fully amorphous structure of the as-spun ribbons could be confirmed from the XRD pattern as shown in Fig.1.

    Fig. 1. XRD patterns of Fe42Ni41.3Si8B4P4Cu0.7 ribbons of as-spun state and annealed states at temperatures of 460-540 °C for 1 h with the insert showing(001)superlattice peak of L10-FeNi for the annealed sample at 540 °C for 1 h.

    Fig.2. (a)DSC curves with the heating rates of 5 °C/min,10 °C/min,20 °C/min and 40 °C/min. (b) Kissinger plots corresponding to two crystallization stages of Fe42Ni41.3Si8B4P4Cu0.7 amorphous alloy.

    After obtaining amorphous ribbons, annealing temperatures have to be determined referring to the DSC measurements. Figure 2(a) shows the DSC curves with the heating rates of 5°C/min,10°C/min,20°C/min and 40°C/min. Two steps of crystallization could be distinguished as two exothermic peaks were observed in each curve. The onset crystallization temperature at each stage(Tx1,Tx2)can be found increasing under higher heating rates asTx1varies from 379°C to 401°C andTx2varies from 465°C to 498°C,respectively.

    Activation energies of crystallization can be calculated by linear fitting[Fig.2(b)]based on the Kissinger function[20]

    whereβis the heating rate,Txis the onset crystallization temperature at each stage,Exis the activation energy of crystallization andRis the gas constant. As a result, the activation energies (Ex1,Ex2) of the two stages were 322 kJ/mol and 286 kJ/mol,respectively.

    3.2. High temperature annealing

    Annealing of the amorphous ribbons at 460-540°C for 1 h was performed to investigate the crystallization products with the completion of both crystallization stages. XRD patterns shown in Fig.1 indicate the information of the main crystallized phases during the annealing,includingα-Fe,A1/L10-FeNi and other compounds such as borides and phosphides.However, the fundamental diffraction peaks in L10-FeNi,which are overlapping with those in A1-FeNi,cannot be used to distinguish the A1 and L10phases through XRD patterns,and the L10-FeNi superlattice peaks such as the (001) and(110)ones,theoretically being extremely smaller than the fundamental ones,could only be distinguished in traces of the enlarged pattern as shown in the insert of Fig. 1. Nevertheless,being one of the most concerned property for hard magnetic materials, the coercivity versus temperature with 1 h annealing is plotted in Fig. 3. It is well-expected to find out from Fig.3 that beyond 480°C,higher temperatures lead to smaller coercivity, since it is reported that high temperatures could turn L10-FeNi into soft magnetic and chemically disordered A1-FeNi phase. It is also revealed that although being exposed above the order-disorder transition temperature[12]for 1 h, L10-FeNi phase is not fully removed as the coercivity is still higher than 500 Oe, indicating the phase transition in the FeNi-based alloy system is still very low so that L10-FeNi phase is not fully removed. In comparison, the amorphous ribbons were annealed at 600°C for 1 h, and the coercivity decreased to be less than 160 Oe. On the other hand, the temperature of 460°C seems too low for the amorphous alloy to be fully crystallized within 1 h, since the trace of residual amorphous halo peak can still be observable in XRD pattern(Fig.1).

    Therefore,the temperature range of 480-540°C appears to be too high for effective synthesis of L10-FeNi from the amorphous alloy.Since the crystallization of amorphous phase could be completed within a few minutes under such temperatures,prolonged annealing time may only lead to the loss of L10phase,and higher temperatures will make the loss faster.

    Fig.3. Annealing temperature dependence of coercivity of Fe42Ni41.3Si8B4P4Cu0.7 ribbons annealed at temperatures of 460-540 °C for 1 h.

    3.3. Low temperature annealing

    A temperature between the two crystallization stages,400°C,was chosen as the annealing temperature to further investigate the formation mechanism of L10-FeNi and improve the coercivity of materials. The structures of annealed ribbons for 10 min,1 h,24 h,138 h and 282 h,were characterized by XRD(Fig.4).Within 1 h annealing,only the diffraction peaks corresponding toα-Fe appear. L10,A1 and some other compound phases emerge and increase rapidly with prolonged annealing time. Despite of the difficulty in detecting superlattice peaks, the (001) superlattice peak was observed in annealed sample for 138 h,as shown in the insert of Fig.4,providing a convincing evidence of L10-FeNi formation.

    Fig. 4. XRD patterns of Fe42Ni41.3Si8B4P4Cu0.7 ribbons annealed at 400 °C for 10 min, 1 h, 24 h, 138 h and 282 h. The insert shows the(001)superlattice peak of L10-FeNi for the annealed sample at 400 °C for 138 h.

    Figure 5(a)presents the hysteresis loops of as-spun state and annealed states(400°C for 10 min,1 h,24 h,138 h,282 h)with the insert of a magnified section at low field.The coercivity evolution of samples is extracted from the hysteresis loops and shown in Fig.5(b). Dramatic rise of coercivity can be observed from the figure as the annealing time reaches 24 h,and the largest coercivity of 861 Oe is obtained in the annealed sample for 138 h. In order to further confirm the existence of L10phase, TEM observation has been adopted. Bright-field TEM image,high-resolution image in TEM image marked by red circle, and diffraction pattern with fast Fourier transformation(FFT)corresponding to the square area(white line)of high-resolution image were shown Fig.6. Mean grain size of crystallized phases is distinguished to be around 27 nm. Diagram of theoretical (111) fundamental and (110) superlattice diffraction of L10-FeNi phase with an intersection angle of 35.3°was depicted in Fig.6(d)as a counterpart for comparison with experimental results. As shown in Fig.6(c),diffraction pattern was very similar to the theoretical diffraction pattern of L10-FeNi[Fig.6(d)]. The results provide a strong evidence for the formation of L10-FeNi in the annealed samples.

    Fig.5. (a)Hysteresis loops of Fe42Ni41.3Si8B4P4Cu0.7 as-spun ribbons and those at 400 °C for 10 min, 24 h, 138 h and 282 h with the insert of a magnified section at low field. (b) Annealing time dependence of coercivity of annealed ribbons at 400 °C.

    Both XRD patterns and magnetic measurements indicate that the formation of Fe-Ni phases and other compounds,corresponding to the second stage of crystallization, takes place when the samples are annealed at 400°C for 24 h. Such annealing temperature is lower than the respective onset temperature by more than 60°C,whereTx2is determined by DSC to be around 465°C with a heating rate of 5°C/min. Low stability of the residual amorphous phase is responsible for such behaviors. In fact, after the crystallization of the first stage,the residual amorphous may become more unstable since the activation energy of the second crystallization stage appears to be significantly lower than that of the first one[Fig.2(b)].

    Nevertheless,the structure of ribbons continued to evolve for days under 400°C as the coercivity reaches its peak value of 861 Oe when samples have been annealed for 138 h.Such a slow process indicates that the diffusion activity of Fe and Ni in the amorphous alloy under this temperature is still sluggish.

    Fig. 6. (a) Bright-field TEM image of annealed sample at 400 °C for 138 h. (b) High-resolution image corresponding to the region marked with red circle in(a). (c)Diffraction pattern after FFT of area marked with white line in(b).(d)Diagram of theoretical(110)fundamental and(111)superlattice diffraction of L10-FeNi phase.

    3.4. Stability of L10-FeNi in the annealed ribbons

    It was reported that L10-FeNi with highly ordered chemical arrangement could transform into chemically disordered A1-FeNi phase when the temperature goes beyond~320°C.[12]However, L10-FeNi refused to disappear when the alloy ribbons were annealed at 400°C for days in this study,indicating the stability of L10-FeNi formed in the alloy ribbons was somehow enhanced,as shown in Fig.5(b).

    Since the transformation from L10-FeNi to A1-FeNi does not involve the participation of other phases or long-range redistribution of the elements,the stability of L10-FeNi against A1-FeNi should not be affected by the other phases. The variation of transformation temperature could only be attributed by the inclusion of other elements in L10-FeNi, and Si is the most possible element in the Fe-Ni-Si-B-P-Cu alloy that can be dissolved in L10phase.

    In principle, the thermal stability of phases could be described by the free energy

    whereG,H,TandSrepresent Gibbs free energy, enthalpy,temperature and entropy of the phases,respectively. LargerScould help bring downGwhenTrises, thus the chemically disordered A1 phase with larger entropy could become more stable than L10phase at high temperatures. However, the inclusion of other elements may help increase the entropy of L10phase so that it could withstand higher temperature against the A1 phase. With enhanced thermal stability, L10phase could be synthesized more efficiently at higher temperature,and the corresponding atoms should tend to form L10phase instead of A1 phase.

    In order to confirm the solubility of Si and some other elements in L10-FeNi and investigate the consequent effects,ab initiomolecular dynamics simulation was carried out. The sampling region includes 2×2×2 unicells of L10-FeNi and one of the atoms (either Fe or Ni) was replaced by Si or Co to find out whether the addition of these elements could be introduced into L10-FeNi phase without seriously deteriorating the magneto-crystalline anisotropy. The systems with or without replacing atoms were firstly relaxed to remove artificial effects and bring lattice deformation that caused by the doping atoms. The system energy change after Si or Co atoms substitution for Fe/Ni was calculated to determine whether the doping atoms could be embedded in the L10-FeNi lattice. The magneto-crystalline anisotropies of systems were calculated to examine if the addition of these elements,which was aimed to enhance the thermal stability of the hard magnetic L10-FeNi phase, will inevitably seriously deteriorate the hard magnetic appearance of L10-phase.

    Fig.7.Simulated structures of Fe16Ni16,Fe15Ni16Si1,and Fe16Ni15Si1.

    The simulated structures of Fe16Ni16, Fe15Ni16Si1and Fe16Ni15Si1are shown in Fig. 7, and the changes of free energy and magneto-crystalline anisotropy energy(Ku)at 300 K in Fe16Ni16X1, and Fe16Ni16X1(X=Si, Co) compared with those in Fe16Ni16are listed in Table 2. TheKuin L10-FeNi was calculated to be 8.02 J/mol(1.16 J/cm3),reasonably agreeing with the previously reported value of~1.30 J/cm3.Both Si and Co were found soluble in Ni substitutional sites of L10-FeNi as the free energy reduces. Moreover, the addition of Si could reduceKuto 3.98 J/mol,but the addition of Co is found much less harmful to it (7.06 J/mol). Therefore, with certain degree of Si addition,L10-FeNi could have its thermal stability increased due to the increased entropy but magnetic hardness significantly decreased, whereas the addition of Co might theoretically be an even better option since it is much less harmful to the hard magnetic properties.

    Table 1. The free energy difference and magneto-crystalline anisotropy energy(Ku)of L10-FeNi with Si or Co addition at 300 K.

    To further investigate the dynamical stability of Fe16Ni15X1(X= Si, Co) with L10lattice, phonon properties were simulated as shown in Fig. 8 with a counterpart of L10-FeNi phase for comparison. Positive frequency modes of all these phases indicate the dynamical stability of optimized structures of Fe16Ni15X1(X=Si,Co)and atoms have been in their local most stable positions,agreeing well with the results of system energies.

    Fig.8. Phonon dispersion curves of(a)Fe16Ni16,(b)Fe16Ni15Si1 and Fe16Ni15Co1 with L10 lattice.

    3.5. Origin of the L10-FeNi in the alloy ribbons

    Further improvement of the process requires the clarification of the timing and origin of L10-FeNi formation in annealed ribbons. It is clear that L10-FeNi is not a direct product from the first stage of crystallization as samples annealed at 400°C within 1 h failed to exhibit a high coercivity and FeNi phase could hardly be observed in Fig.4,thus it could only be originated from the residual amorphous phase during second stage of crystallization and/or from pre-formed phases.

    In order to clarify these possibilities, experiments were designed as the as-spun ribbons were firstly annealed at 520°C for 3 h or 24 h to be fully crystallized,then kept at 400°C for a period of time to find out whether the crystalline phases could contribute to the formation of L10-FeNi under such annealing temperature. Coercivity values of annealed samples were shown in Table 2. When it is annealed under 400°C,the rise of coercivity takes place mainly during the period from 1 h to 24 h, accomplished with the disappearance of residual amorphous signal in the XRD patterns,indicating that the L10phase is mainly precipitated from the residual amorphous during the second crystallization stage. However,slight increment of coercivity could also be observed during annealing under 400°C after full crystallization as have already been annealed under 520°C for 3 h or 24 h. Such increment is probably due to the limited transformation from other high temperature crystalline phases towards L10phase, or the removal of B from L10lattice and improvement of the ordering quality of the L10phase due to the reduced temperature from 520°C to 400°C.

    Table 2.Coercivity evolution of annealed ribbons under various conditions.

    3.6. Direction dependent hysteresis behavior of the sheet samples

    It is reasonable to believe that the microstructures of annealed samples are isotropic since they were made from amorphous structure without external stress or other anisotropic effects. However, hysteresis loops of annealed samples as well as the coercivity appear to be different at various directions,as shown in Fig. 9, thus the anisotropic shape of sample should be the main reason.

    The annealed samples consist of hard magnetic L10-FeNi phase, soft magneticα-Fe and A1-FeNi phases, and some other compound phases. During a magnetic reversal process,some of soft magnetic regions will yield to the external magnetic field easily,and the increasing magnetic field will expand the reversed regions as the domain wall propagates. The hard magnetic L10-FeNi grains,which have their magnetic moment hard to change,will act as pinning sites that prevent the propagation of the domain walls,leading to the rise of coercivity.

    In samples with a shape of sheet,the domain wall should always be perpendicular to the sheet plane to minimize the area as well as the energy of it, thus only the in-plane part of the magnetic field is effective to the propagation of domain wall. Overcoming the pinning sites requires the effective magnetic field to reach a certain threshold. When the angle between the field and sample plane (θ) increases,larger coercivity is measured following a simplified Kondorsky model, and such a phenomenon is well-discussed in previous reports.[21,22]

    Fig. 9. (a) Hysteresis loops of Fe42Ni41.3Si8B4P4Cu0.7 annealed ribbons at 400 °C for 138 h with applied magnetic field in the angle of 0 °,82 ° and 90 ° with respect to the sample plane. (b) Direction dependence of coercivity of ribbons annealed at 400 °C for 24 h,138 h 210 h and 282 h.

    The monotonic increase of coercivity withθbecomes reversed whenθgoes close to 90°. At high angles, instead of easy reversal, the moments of soft magnetic regions are confined to reduce the net out-of-plane moment due to the strong demagnetization effect. In order to cancel the magnetic moment of hard magnetic phases,the soft magnetic phase will exhibit opposite magnetic moment to form magnetic dipoles,and the changing of external magnetic field could only take effect on forming or breaking these dipoles. Thus,no sharp change of magnetic moment could be observed from the hysteresis loops at 90°,and the coercivity becomes greatly reduced since the demagnetization field already takes strong effect on reducing the magnetic moment towards zero in the measured direction.

    Therefore, the difference of magnetic behaviors in various directions of the sample is determined by both domain wall pinning effect and demagnetization effect, the former of which is dominant at low angles with respect to the sample plane and the latter become dominant at high angles.

    3.7. Discussion on the improvement of the process

    Up to now, achieving 861 Oe by annealing FeNi-based amorphous ribbons is still far from the purpose of fabricating application-worthy L10-FeNi hard magnets.To further improve L10-FeNi magnets by annealing amorphous alloys, we should mainly focus on the following factors.

    Firstly,the addition of some elements,such as Si or Co,is considered promising to improve the thermal stability of L10-FeNi. With enhanced thermal stability, amorphous structure will tend to crystallize into more L10-FeNi instead of A1-FeNi,and the process could be operated at higher temperature for faster synthesis.

    Secondly, amorphous alloy composition with lowTxof the critical stage should be found. Since L10-FeNi always has higher chemical ordering and smaller entropy than A1-FeNi,lower temperature will make the free energy difference between L10-FeNi and A1-FeNi become larger,thus the amorphous alloy will prefer to crystallize into L10-FeNi more rather than A1-FeNi.

    Besides, it is found that the first stage of crystallization has hardly any direct contribution to the formation of L10-FeNi. Therefore, the alloy composition could be redesigned to remove part of Fe and to remove Cu that is practical in promotingα-Fe formation but not effective for the formation of L10-FeNi. The volume fraction of L10phase probably is increased and the coercivity would be improved when the precipitation ofα-Fe is suppressed.

    4. Conclusion

    The formation mechanism of L10-FeNi through annealing Fe42Ni41.3Si8B4P4Cu0.7amorphous alloy has been studied. The maximum coercivity of 861 Oe was obtained in the sample prepared by annealing amorphous ribbons at 400°C for 138 h. Annealing at higher temperature will result in smaller coercivity since L10-FeNi could transform into A1-FeNi, but too low temperature could greatly slow down the preparation progress. L10-FeNi in the annealed ribbons was mainly precipitated from the residual amorphous alloy during the second crystallization stage.A slight increase of coercivity was found for fully crystallized samples annealed at 400°C,probably due to limited transformation from other high temperature crystalline phases towards L10phase,or the removal of B from L10lattice and improvement of the ordering quality of the L10phase due to the reduced temperature from 520°C to 400°C.

    It is found that the L10-FeNi formed during annealing at 400°C is stable. According the computational simulation,the substitution of Si or Co for Ni sites in L10-FeNi lattice could enhance the stability of L10phase.

    It is revealed that the difference of magnetic behaviors in various directions of the sheet samples is caused by the domain wall pinning effect and demagnetization effect, leading to the phenomenon of non-monotonic direction dependent coercivity with peak values lies in the angle of 82°to sample plane.

    Acknowledgements

    This work was supported by the National Natural Science Foundation of China (Grant Nos. 51971179 and 51971180),the Natural Science Foundation of Chongqing, China (Grant No. cstc2019jcyj-msxmX0328), Shaanxi Provincial Natural Science Foundation, China (Grant No. 2020JM-112),Guangdong Provincial Science and Technology Program,China (Grant No. 2019B090905009), the Fundamental Research Funds for the Central Universities of China (Grant No. D5000210731), and Shaanxi Provincial Key R&D Program, China (Grant No. 2021KWZ-13). The computational work was performed on supercomputing system in Institute for Materials Research,Tohoku University.

    猜你喜歡
    張巖崇德
    昆明崇德水泥有限公司
    撿玉米
    把實事真正辦到群眾心坎里
    雷鋒(2022年2期)2022-04-12 00:08:12
    岜沙苗寨繡花女
    金秋(2020年12期)2020-12-03 23:04:07
    政策發(fā)力,為經(jīng)濟(jì)復(fù)蘇保駕護(hù)航
    中國報道(2020年4期)2020-04-19 10:07:34
    崇德鎮(zhèn)“蒲公英農(nóng)民詩社”詩教工作紀(jì)實
    中華詩詞(2020年8期)2020-02-06 09:27:20
    Morphological characters and DNA barcoding of Syngnathus schlegeli in the coastal waters of China*
    春天里的發(fā)現(xiàn) 等
    《工程力學(xué)》課程中PBL教學(xué)模式的應(yīng)用探討
    崇德向善著力踐行社會主義核心價值觀
    嫁个100分男人电影在线观看| 一进一出抽搐动态| 最近在线观看免费完整版| 色精品久久人妻99蜜桃| 亚洲av不卡在线观看| 国产精品久久视频播放| 国产久久久一区二区三区| 国产 一区 欧美 日韩| 日韩精品中文字幕看吧| eeuss影院久久| 最好的美女福利视频网| 综合色av麻豆| 中文字幕精品亚洲无线码一区| 久久久精品大字幕| 国产一级毛片七仙女欲春2| 好男人电影高清在线观看| 亚州av有码| av视频在线观看入口| 很黄的视频免费| 亚洲人与动物交配视频| 成人精品一区二区免费| 亚洲成人久久性| 欧美三级亚洲精品| 亚洲av美国av| 午夜精品在线福利| 最近最新中文字幕大全电影3| 激情在线观看视频在线高清| av欧美777| 超碰av人人做人人爽久久| 国产高清有码在线观看视频| 欧美极品一区二区三区四区| 国产成人啪精品午夜网站| 搞女人的毛片| av国产免费在线观看| 舔av片在线| 一级作爱视频免费观看| 国产伦精品一区二区三区四那| 成年女人看的毛片在线观看| 国产高清视频在线观看网站| 日韩欧美精品v在线| 天堂动漫精品| 99久久无色码亚洲精品果冻| 真人一进一出gif抽搐免费| 国产精品一及| 啦啦啦观看免费观看视频高清| 天堂网av新在线| 亚洲一区二区三区不卡视频| 成年女人看的毛片在线观看| 婷婷色综合大香蕉| 欧美在线黄色| 色吧在线观看| a级毛片免费高清观看在线播放| 深爱激情五月婷婷| 精品欧美国产一区二区三| 国产精品久久久久久久久免 | 97超级碰碰碰精品色视频在线观看| 极品教师在线视频| 国产av一区在线观看免费| 国产av一区在线观看免费| 国产精品乱码一区二三区的特点| 午夜福利在线在线| 国产精品精品国产色婷婷| 无人区码免费观看不卡| 搡老熟女国产l中国老女人| 欧美又色又爽又黄视频| 男女之事视频高清在线观看| 久久精品国产亚洲av天美| 亚洲最大成人中文| 五月伊人婷婷丁香| 亚洲av熟女| 蜜桃亚洲精品一区二区三区| 人妻制服诱惑在线中文字幕| 一区福利在线观看| 午夜福利在线观看吧| 国产成人啪精品午夜网站| 国产白丝娇喘喷水9色精品| 一区福利在线观看| 日韩欧美精品免费久久 | 国产欧美日韩精品亚洲av| 午夜福利视频1000在线观看| 国产精品电影一区二区三区| 欧美又色又爽又黄视频| 亚洲av熟女| 欧美极品一区二区三区四区| 一个人看的www免费观看视频| 男人舔女人下体高潮全视频| 免费搜索国产男女视频| 最近最新中文字幕大全电影3| 亚洲中文字幕日韩| 久久人人爽人人爽人人片va | 国产精品1区2区在线观看.| 少妇被粗大猛烈的视频| 18禁裸乳无遮挡免费网站照片| 在线播放国产精品三级| 精品一区二区三区视频在线观看免费| 麻豆国产97在线/欧美| 一级作爱视频免费观看| 欧美日韩国产亚洲二区| 一区福利在线观看| 1024手机看黄色片| 亚洲成av人片在线播放无| 99国产极品粉嫩在线观看| 欧美性猛交╳xxx乱大交人| xxxwww97欧美| 激情在线观看视频在线高清| 日本精品一区二区三区蜜桃| 热99re8久久精品国产| 色综合婷婷激情| 波多野结衣高清无吗| 黄色视频,在线免费观看| 欧美中文日本在线观看视频| 婷婷亚洲欧美| 在线免费观看的www视频| 亚洲成av人片免费观看| 在线国产一区二区在线| 欧美在线黄色| 18禁裸乳无遮挡免费网站照片| 亚洲在线自拍视频| 亚洲成人久久性| 欧美日韩中文字幕国产精品一区二区三区| 又爽又黄无遮挡网站| 欧美精品啪啪一区二区三区| avwww免费| 中亚洲国语对白在线视频| 黄色丝袜av网址大全| 免费无遮挡裸体视频| 免费av毛片视频| 免费观看的影片在线观看| 久久久精品大字幕| 国产精品影院久久| 男女视频在线观看网站免费| 中文在线观看免费www的网站| 永久网站在线| 美女xxoo啪啪120秒动态图 | 国产一区二区亚洲精品在线观看| 欧美成人免费av一区二区三区| 国产白丝娇喘喷水9色精品| 国产精品免费一区二区三区在线| 国产中年淑女户外野战色| 一本综合久久免费| www.色视频.com| 嫁个100分男人电影在线观看| 精品国内亚洲2022精品成人| 人人妻人人澡欧美一区二区| 中亚洲国语对白在线视频| 亚洲在线自拍视频| 国产真实伦视频高清在线观看 | 久久久久精品国产欧美久久久| 成人特级黄色片久久久久久久| 男女床上黄色一级片免费看| 熟女人妻精品中文字幕| 国产精品国产高清国产av| 男女做爰动态图高潮gif福利片| 性色avwww在线观看| 啦啦啦观看免费观看视频高清| 欧美又色又爽又黄视频| 18美女黄网站色大片免费观看| 国产 一区 欧美 日韩| ponron亚洲| 极品教师在线免费播放| 级片在线观看| 成人av一区二区三区在线看| 亚洲欧美日韩卡通动漫| 高潮久久久久久久久久久不卡| 久久精品人妻少妇| av视频在线观看入口| 观看免费一级毛片| 欧美又色又爽又黄视频| 给我免费播放毛片高清在线观看| 欧美日本视频| 99久久99久久久精品蜜桃| 97碰自拍视频| 99久久无色码亚洲精品果冻| 成人精品一区二区免费| 色综合亚洲欧美另类图片| 日韩高清综合在线| 搡老熟女国产l中国老女人| 国产精品av视频在线免费观看| 午夜福利视频1000在线观看| 色综合婷婷激情| 男人舔女人下体高潮全视频| 久久久国产成人免费| netflix在线观看网站| eeuss影院久久| 禁无遮挡网站| 国产精品99久久久久久久久| 99热只有精品国产| 老司机午夜福利在线观看视频| 免费观看精品视频网站| 男人舔奶头视频| 国内毛片毛片毛片毛片毛片| 久久精品国产99精品国产亚洲性色| 亚洲最大成人中文| 国产一区二区亚洲精品在线观看| 色尼玛亚洲综合影院| 悠悠久久av| 我要搜黄色片| 在线播放国产精品三级| 村上凉子中文字幕在线| 亚洲aⅴ乱码一区二区在线播放| 国产综合懂色| 美女免费视频网站| 亚洲最大成人手机在线| 757午夜福利合集在线观看| 欧美黑人欧美精品刺激| 如何舔出高潮| 日韩精品青青久久久久久| 一区二区三区四区激情视频 | 国产精品女同一区二区软件 | 一区二区三区激情视频| 国产黄色小视频在线观看| 久久国产精品人妻蜜桃| 免费看a级黄色片| 中亚洲国语对白在线视频| a级一级毛片免费在线观看| 午夜福利欧美成人| 99热6这里只有精品| 国产黄片美女视频| av在线天堂中文字幕| 久久伊人香网站| 久久久久久九九精品二区国产| 一区二区三区四区激情视频 | 欧美成人性av电影在线观看| 又黄又爽又刺激的免费视频.| 老熟妇仑乱视频hdxx| 亚洲av熟女| 丁香六月欧美| avwww免费| 中文字幕精品亚洲无线码一区| 三级男女做爰猛烈吃奶摸视频| 露出奶头的视频| 色尼玛亚洲综合影院| 午夜免费成人在线视频| 国产人妻一区二区三区在| 国产乱人伦免费视频| 九九热线精品视视频播放| 精品人妻一区二区三区麻豆 | 国产伦在线观看视频一区| 丰满人妻一区二区三区视频av| 欧美丝袜亚洲另类 | 精品午夜福利在线看| 成人鲁丝片一二三区免费| 国产精品一区二区性色av| 欧美成人性av电影在线观看| 小蜜桃在线观看免费完整版高清| 亚洲自偷自拍三级| 亚洲av不卡在线观看| 久久精品人妻少妇| 亚洲国产色片| 国产精品久久久久久久电影| 一个人观看的视频www高清免费观看| 天堂av国产一区二区熟女人妻| 精品一区二区免费观看| 色综合欧美亚洲国产小说| 久久热精品热| 午夜老司机福利剧场| 特级一级黄色大片| 99国产综合亚洲精品| 国产在线精品亚洲第一网站| 亚洲激情在线av| 国产精品亚洲av一区麻豆| 1000部很黄的大片| 男人的好看免费观看在线视频| 国产免费男女视频| 美女xxoo啪啪120秒动态图 | 欧美成人a在线观看| 日韩欧美在线乱码| 变态另类丝袜制服| 直男gayav资源| 亚洲欧美日韩无卡精品| 很黄的视频免费| 身体一侧抽搐| 亚洲欧美清纯卡通| 欧美最新免费一区二区三区 | 国产欧美日韩精品一区二区| 天堂动漫精品| 国产成人a区在线观看| 色噜噜av男人的天堂激情| 精品无人区乱码1区二区| 夜夜看夜夜爽夜夜摸| 国产高清有码在线观看视频| 国产免费男女视频| 噜噜噜噜噜久久久久久91| 又黄又爽又刺激的免费视频.| 最新中文字幕久久久久| 男人狂女人下面高潮的视频| 国产午夜精品久久久久久一区二区三区 | 精品久久久久久久人妻蜜臀av| 免费电影在线观看免费观看| 精品无人区乱码1区二区| 夜夜爽天天搞| 国产成人av教育| 亚洲七黄色美女视频| a级毛片免费高清观看在线播放| 18+在线观看网站| 欧美潮喷喷水| 国产成+人综合+亚洲专区| 91在线观看av| 成人美女网站在线观看视频| 最近最新中文字幕大全电影3| 中文在线观看免费www的网站| 亚洲中文字幕一区二区三区有码在线看| 亚洲中文字幕一区二区三区有码在线看| 自拍偷自拍亚洲精品老妇| 90打野战视频偷拍视频| 免费观看人在逋| 18美女黄网站色大片免费观看| 亚洲人成电影免费在线| 久久人妻av系列| 午夜免费男女啪啪视频观看 | 一级a爱片免费观看的视频| 最新中文字幕久久久久| 深爱激情五月婷婷| 精品一区二区免费观看| www.999成人在线观看| 国产不卡一卡二| www.999成人在线观看| 免费搜索国产男女视频| 国产精品美女特级片免费视频播放器| 男人舔女人下体高潮全视频| 久久久久久久午夜电影| 超碰av人人做人人爽久久| a在线观看视频网站| 国产成人aa在线观看| 亚洲人成伊人成综合网2020| 精品欧美国产一区二区三| 午夜福利视频1000在线观看| 最后的刺客免费高清国语| av在线天堂中文字幕| av女优亚洲男人天堂| 久久精品国产99精品国产亚洲性色| 国产 一区 欧美 日韩| 国内精品久久久久精免费| h日本视频在线播放| 午夜福利在线观看免费完整高清在 | 一本精品99久久精品77| 十八禁国产超污无遮挡网站| 国产精品人妻久久久久久| 亚洲精品在线美女| 12—13女人毛片做爰片一| av天堂在线播放| 亚洲内射少妇av| 久久精品影院6| 欧美成人性av电影在线观看| 1024手机看黄色片| 啦啦啦观看免费观看视频高清| 身体一侧抽搐| 国产精品一区二区三区四区久久| 色精品久久人妻99蜜桃| 内地一区二区视频在线| 国产精品国产高清国产av| 一级a爱片免费观看的视频| 中亚洲国语对白在线视频| 久久久久性生活片| 国产精品不卡视频一区二区 | 久久久精品欧美日韩精品| 美女 人体艺术 gogo| 9191精品国产免费久久| 午夜福利18| 免费观看人在逋| 性欧美人与动物交配| 在线十欧美十亚洲十日本专区| 日韩成人在线观看一区二区三区| 亚洲精品粉嫩美女一区| 免费在线观看成人毛片| 国产在线男女| 嫩草影视91久久| 嫩草影院精品99| 欧美黄色淫秽网站| 99久久99久久久精品蜜桃| 成年女人看的毛片在线观看| 欧美激情国产日韩精品一区| 少妇高潮的动态图| 性欧美人与动物交配| 午夜精品一区二区三区免费看| 国产精品人妻久久久久久| 午夜两性在线视频| 亚洲天堂国产精品一区在线| netflix在线观看网站| 亚洲,欧美精品.| 免费观看人在逋| a在线观看视频网站| 欧美丝袜亚洲另类 | 国产一区二区在线观看日韩| 欧美激情在线99| 欧美成人一区二区免费高清观看| 欧美xxxx性猛交bbbb| 又黄又爽又刺激的免费视频.| 免费看光身美女| .国产精品久久| 午夜福利在线观看免费完整高清在 | 午夜福利18| 嫩草影院精品99| 午夜福利视频1000在线观看| 日本黄色片子视频| 亚洲欧美日韩高清在线视频| 亚洲中文字幕日韩| 亚洲成人精品中文字幕电影| avwww免费| 淫秽高清视频在线观看| 能在线免费观看的黄片| 国产精品久久久久久久久免 | 免费av观看视频| 婷婷精品国产亚洲av在线| 亚洲自拍偷在线| 一个人观看的视频www高清免费观看| 欧美黄色淫秽网站| 国产精品乱码一区二三区的特点| 久久99热这里只有精品18| 天美传媒精品一区二区| 97超级碰碰碰精品色视频在线观看| 网址你懂的国产日韩在线| 久久婷婷人人爽人人干人人爱| 亚洲五月天丁香| 精品国内亚洲2022精品成人| 亚洲专区中文字幕在线| 综合色av麻豆| 国产在视频线在精品| 成人特级黄色片久久久久久久| 亚州av有码| 欧洲精品卡2卡3卡4卡5卡区| 日本黄大片高清| 俄罗斯特黄特色一大片| 国产成人av教育| 国产精品电影一区二区三区| 9191精品国产免费久久| 欧美日韩黄片免| 午夜a级毛片| 我要搜黄色片| 亚洲av免费高清在线观看| 青草久久国产| 十八禁国产超污无遮挡网站| 午夜两性在线视频| 一区福利在线观看| 亚洲av第一区精品v没综合| 国产精品久久电影中文字幕| 欧美激情久久久久久爽电影| 人人妻人人澡欧美一区二区| 深夜精品福利| 三级毛片av免费| 99精品在免费线老司机午夜| 日本成人三级电影网站| 亚洲av二区三区四区| 久久国产乱子免费精品| 国模一区二区三区四区视频| 亚洲avbb在线观看| 欧美激情久久久久久爽电影| 变态另类成人亚洲欧美熟女| 在线观看一区二区三区| 欧美日韩乱码在线| 精品久久久久久成人av| 国产精品99久久久久久久久| 国产精品久久久久久精品电影| 色av中文字幕| 国内精品美女久久久久久| 欧美黑人巨大hd| 十八禁国产超污无遮挡网站| 国产精品久久久久久亚洲av鲁大| 欧美精品国产亚洲| 给我免费播放毛片高清在线观看| 久久久精品大字幕| 又紧又爽又黄一区二区| 美女xxoo啪啪120秒动态图 | 18禁黄网站禁片午夜丰满| 啦啦啦观看免费观看视频高清| 婷婷精品国产亚洲av| 久久久久久久午夜电影| 亚洲国产色片| 看免费av毛片| 国产高潮美女av| 国产黄a三级三级三级人| 国产亚洲精品久久久com| 欧洲精品卡2卡3卡4卡5卡区| 人妻制服诱惑在线中文字幕| 日韩欧美精品v在线| 中文字幕熟女人妻在线| 亚洲精华国产精华精| 高潮久久久久久久久久久不卡| 女同久久另类99精品国产91| 久久亚洲精品不卡| 欧美在线一区亚洲| 日韩大尺度精品在线看网址| 国内精品美女久久久久久| 久久久成人免费电影| 成人性生交大片免费视频hd| 成人一区二区视频在线观看| 神马国产精品三级电影在线观看| 天堂√8在线中文| 一级av片app| 欧美精品啪啪一区二区三区| 婷婷色综合大香蕉| 欧美黑人欧美精品刺激| 亚洲一区高清亚洲精品| 国内精品一区二区在线观看| 黄色女人牲交| 欧美3d第一页| 国内精品一区二区在线观看| 欧美bdsm另类| 三级毛片av免费| 搡老熟女国产l中国老女人| 国产高潮美女av| 亚洲黑人精品在线| 如何舔出高潮| 成人国产综合亚洲| 露出奶头的视频| 国产日本99.免费观看| 少妇熟女aⅴ在线视频| 亚洲国产欧洲综合997久久,| 麻豆国产av国片精品| 中文字幕av在线有码专区| 每晚都被弄得嗷嗷叫到高潮| 国产黄a三级三级三级人| 非洲黑人性xxxx精品又粗又长| 亚洲午夜理论影院| 免费电影在线观看免费观看| 亚洲最大成人手机在线| 日韩大尺度精品在线看网址| 国产主播在线观看一区二区| 国产亚洲精品久久久com| 久久久久久久久久成人| 久久精品夜夜夜夜夜久久蜜豆| 午夜福利在线观看吧| 国产伦在线观看视频一区| 久久精品国产自在天天线| 欧美成人a在线观看| 亚洲无线观看免费| 一级a爱片免费观看的视频| 亚洲国产欧美人成| 老女人水多毛片| 国产乱人视频| 亚洲最大成人手机在线| 免费一级毛片在线播放高清视频| 亚洲真实伦在线观看| 国产亚洲av嫩草精品影院| 99热精品在线国产| 国产一区二区三区视频了| 毛片一级片免费看久久久久 | 日本精品一区二区三区蜜桃| 久9热在线精品视频| 欧美日本视频| 国产欧美日韩精品亚洲av| 蜜桃亚洲精品一区二区三区| 大型黄色视频在线免费观看| av视频在线观看入口| 直男gayav资源| 97碰自拍视频| 国产精品久久视频播放| 免费看光身美女| 美女高潮喷水抽搐中文字幕| 最近在线观看免费完整版| 黄色日韩在线| 久久精品影院6| 日韩欧美在线二视频| 欧美日韩黄片免| 性色av乱码一区二区三区2| 日韩大尺度精品在线看网址| 2021天堂中文幕一二区在线观| 精品免费久久久久久久清纯| 天堂影院成人在线观看| 在线观看66精品国产| 两个人视频免费观看高清| 九色国产91popny在线| 精品久久久久久久久亚洲 | 久久精品国产清高在天天线| 给我免费播放毛片高清在线观看| 9191精品国产免费久久| 国产精品久久久久久亚洲av鲁大| 久久精品影院6| 国产精品久久久久久久久免 | 3wmmmm亚洲av在线观看| 日韩高清综合在线| 国产精品人妻久久久久久| a级毛片免费高清观看在线播放| 亚洲精品456在线播放app | 我的女老师完整版在线观看| 亚洲美女搞黄在线观看 | 波多野结衣高清作品| 十八禁国产超污无遮挡网站| 天堂动漫精品| 国产色爽女视频免费观看| 日韩欧美三级三区| 欧美中文日本在线观看视频| 日本五十路高清| 一本久久中文字幕| 欧美日韩黄片免| 亚洲精华国产精华精| 国产精品1区2区在线观看.| 亚洲无线在线观看| 久久伊人香网站| 99久久精品热视频| 性欧美人与动物交配| 久久精品久久久久久噜噜老黄 | 麻豆成人av在线观看| 精品久久久久久久末码| 在线播放无遮挡| 国产精品精品国产色婷婷| 两性午夜刺激爽爽歪歪视频在线观看| 欧美+日韩+精品| 听说在线观看完整版免费高清| 久久国产精品人妻蜜桃| 亚洲av.av天堂| 午夜福利成人在线免费观看| 国内揄拍国产精品人妻在线| 无人区码免费观看不卡| 国内精品一区二区在线观看| 亚洲aⅴ乱码一区二区在线播放| 国产激情偷乱视频一区二区| 一二三四社区在线视频社区8| 一级av片app| 永久网站在线| 88av欧美| 99精品在免费线老司机午夜| 久久亚洲精品不卡| 国产精品永久免费网站| 久久人人精品亚洲av|