    A comparative corrosion behavior of Mg,AZ31 and AZ91 alloys in 3.5% NaCl solution

    2015-02-16 00:38:12*
    Journal of Magnesium and Alloys 2015年2期

    *

    CSIR-Advanced Materials and Processes Research Institute,Bhopal 462026,M.P.,India

    A comparative corrosion behavior of Mg,AZ31 and AZ91 alloys in 3.5% NaCl solution

    I.B.Singh*,M.Singh,S.Das

    CSIR-Advanced Materials and Processes Research Institute,Bhopal 462026,M.P.,India

    The corrosion behavior of Mg,AZ31 and AZ91 has been evaluated in 3.5%NaCl solution using weight loss,electrochemical polarization and impedance measurements.Corrosion rate derived from the weight losses demonstrated the occurrence of steeply fast corrosion reaction on AZ91 alloy after three hours of immersion,indicating the start of galvanic corrosion.An increase of corrosion rate with immersion time was also observed for AZ31 but with lesser extent than AZ91 alloy.Whereas Mg metals showed a decrease of corrosion rate with immersion time, suggesting the formation of a protective layer on their surfaces.In contrast,the corrosion current density(Icorr)derived from the Tafel plots, exhibited their corrosion resistances in order of Mg>AZ91>AZ31.Electrochemical charge transfer resistance(Rct)and double layer capacitance measured by electrochemical impedance spectroscopy(EIS),are well in accordance with the measured Icorr.EIS measurements with time and microstructural examination of the corroded and uncorroded samples are helpful in elucidation of results measured by electrochemical polarization.

    Mg and alloys;Weight loss;Electrochemical measurements;SEM

    1.Introduction

    Magnesium based alloys possess an attractive combination of low density and high strength/weight/ratio which are quite useful for their applications in automotive and aerospace industries.However,they are very reactive in the humid or wet atmosphere as their loosen oxide layer make them highly corrosive.Their corrosion reaction becomes much more pronounced when they are exposed in aqueous marine environment.Occurrence of the galvanic corrosion is another problem with Mg alloys as magnesium has the lowest electrode potential and acts as anode in the alloy[1-4].Though alloying of Al and Zn with Mg increases their strength but make them venerable to galvanic corrosion.Mg-Al alloys are the most common category of magnesium alloy.There are different opinions about the role of Al on the corrosion resistance of magnesium alloy.Lunder et al.[5]observed that when aluminum content reaches 8%(mass fraction),the corrosion resistance of magnesium alloy improve in a noticeable level. Warner et al.[6]reported that even 5%addition of Al in magnesium alloys is benefcial in improving their corrosion resistance.Whereas Hemann et al.[7]indicated that 9%and above Al is helpful in improving of corrosion resistance of magnesium alloy.However,no one among them studied the approximate exposure period at which this alloy becomes suxcitible for galvanic corrosion at neutral pH.

    Alloying effect of Al and Zn on corrosion of Mg is latively less studies.Cao et al.[8]investigated the corrosion behavior of Mg and AZ91 alloy in 0.1 M NaCl solution using electrochemical studies.They observed a highly corrosive nature of AZ91 alloy as compared to Mg metal.Cheng et al.[9]studied the infuence of alloying elements like Zr,Al on the corrosion resistance of Mg in 1 M NaCl solution using electrochemical measurements.They observed AZ91 alloy shows the worst corrosion resistance among AZ31,AZ91,AM60 and ZK60 alloys. Though, electrochemical measurements including electrochemical impedance spectroscopy are quite useful in the determination corrosion kinetics and diffusion phenomena at the metal/electrolytes interfaces,weight loss measurement is still considered most authentic method for corrosion rate determination in free corrosion condition.As per our knowledge no one has made corrosion rate determination using weight loss measurement especially for Mg and their alloys in chloride bearing corrosive system.

    With this view,the present work was aimed to make a detail corrosion studies of the Mg metal and their alloys,AZ31 and AZ91 in 3.5%NaCl solution using weight loss,electrochemical and microstructural studies.

    2.Experimental

    The materials used in the present study,were commercial grade Mg(~99%pure)metal and as cast AZ31(Al 3 wt%,Zn 1 wt%,balanced Mg)and AZ91(Al 9 wt%,Zn 1 wt%, balanced Mg)alloys.The casting of the alloys was made in the oxygen protective atmosphere.In weight loss measurement rectangular samples of dimension 2.5 cm×2.5 cm×0.25 cm were used.Samples were polished well with different grades of emery paper.Before immersing,samples were degreased using trichoroethylene solution.In weight loss measurement, pre-weighted samples were immersed vertically in 3.5%NaCl with the help of polypropylene make thread tightened at one end of the sample through drilled hole.Immersed samples were removed from the solution after different intervals of time.After removing,samples were washed carefully,dried in air and again re-weighted.The corrosion rate was derived using following Eq.(1)

    where corrosion rate is in millimeter per year,W,weight loss in mg,D,density and T,time in hour.

    Electrochemical measurements like open circuit potential (OCP)variation with time,potentiodynamic polarizations and electrochemical impedance spectroscopy were performed in 3.5 wt%NaCl solution at room temperature(25°C)using a Solartron make 1280 Z corrosion measurement system.Three electrodes system,namely,a working electrode(area:1 cm2), a platinum counter electrode(area:2 cm2)and a saturated calomel electrode(SCE),as a reference electrode were employed in the present investigation.Open circuit potential (OCP)variations with time were recorded up to 30 min of exposure.Afterward,Tafel plot was obtained by carrying out partial potentiodynamic polarization in the potential range±150 mV from OCP at the potential scan rate of 1 mV/ s.In a separate experiment potentiodynamic polarization was made by scanning potential from-150 mV(SCE)from OCP to 1.5 V(SCE)in the anodic potential.EIS analysis was done in the frequency range of 20 mHz to 20 kHz using a sinusoidal ac signal of 10 mV at the open circuit potential.The reproducibility of the electrochemical test was verifed by carrying out two to three measurements on a fresh polished specimen. All the measurements have been performed in aerated solution under static condition.Different parameters of polarization curves and impedance diagrams were derived from software Corrware 2 and Z plot,respectively using curve ftting method. After completion of EIS measurement,were cleaned properly and used for their microstructural examination.

    3.Results and discussion

    Different corrosion reactions involved in magnesium and their alloys are similar neutral and alkaline media.The overall reaction[10]can be expressed as

    However,the above reaction presents a general description and does not explain the involvement of different stages of corrosion.For e.g.naturally formed oxide or passive flm present on Mg alloy can exhibit a high corrosion resistance up to certain exposure period.But the same alloy may show suddenly a very fast corrosion after passing of critical exposure period at which galvanic corrosion start.Therefore,the corrosion property of magnesium alloys is associated with the nature of naturally formed oxide flm present on their surfaces and also related to content of their cathodic alloying elements present in their matrix.Mg-Al-Zn alloy is the most common category of magnesium alloy where Al and Zn are the main cathodic elements which determine the corrosion of alloys.In both alloys,Zn content is same.Therefore,their entire corrosion property depends on the presence of Al content.On the other side it is well known that pure Mg metal posses better corrosion resistances than their alloys.Thus a comprehensive corrosion study comprises of weight loss and electrochemical measurements is carried out to understand the role of Al content on the critical exposure period at which galvanic corrosion starts and their comparative corrosion behavior in chloride bearing neutral solution.

    3.1.Weight loss measurement

    Weight loss measurement indicated that Mg metal demonstrates a very less weight loss as compared to AZ91 and AZ31 alloy up to 72 h of exposure.In comparison to AZ31, AZ91 alloy showed less weight loss up to initially 3 h of exposure.Thereafter,their steep increase of weight loss was measured.The corrosion rate(mm/y)derived as per Eq.(1),is plotted against time(Fig.1).From the trend one can see that the corrosion rate of AZ91 occurs comparatively much less than AZ31 alloy till initial 3 h of immersion.After this,there was a steep rise in their corrosion rate(6 mm/y)was measured. Whereas AZ31 alloy showed even less than one mm/y corrosion rate after 3 h of immersion.The increase in corrosion rate of AZ91 alloy was continued with fast rate till 32 h of immersion.After this period,a decline in their corrosion ratewas measured.After removing,specimens were observed visually porous structure.Due to decrease of dimension of the specimen,weight loss measurement was stopped after 48 h of immersion.

    Fig.1.Corrosion rate variations with time for Mg,AZ1 and AZ91 alloys in 3.5%NaCl solution.

    In case of AZ31 alloy,it showed a linear increase of weight loss till 72 h of immersion.Interestingly,Mg metal showed better corrosion resistances as compared to AZ91 alloy even after 72 h of immersion.But it showed very high corrosion rate as compared to Mg metal.Interestingly,a decrease in corrosion rate with exposure time was measured for Mg metal. The surface of the immersed Mg metal was intact even after 72 h of exposure.These this suggest that a protective nature of oxide flm forms at the Mg surfaces which reduces their corrosion signifcantly.A steep increase of corrosion rate after 3 h of immersion of AZ91 alloy evidences the occurrence of fast corrosion reaction that increases with exposure period possibly due to start of galvanic corrosion.Moreover,intensity of the galvanic corrosion appears to be quite high for AZ91 alloy.Presence of a higher Al content in the AZ91 alloy presumably increases the potential difference that results the start of galvanic corrosion with fast rate.

    3.2.Electrochemical measurements

    3.2.1.OCP behavior

    Fig.2.OCP measurement with time for Mg,AZ31 and AZ91 alloys in 3.5% NaCl solution.

    The open-circuit potential(OCP)variations with time curves obtained for all the three studied substrates,are presented in Fig.2.From the trend,it can be noted that their initial OCP moves in negative direction till 5 min of measurement.Afterward,it increases toward positive direction and their increase rate slows down after 20 min of duration. However,their OCP could not attain steady state even after 30 min of measurement.Increase of OCP towards positive side is more for AZ31 alloy as compared to AZ91 and Mg metal. Observed OCP values indicate that OCP of Mg occurs more negative(-1.66 V)as compared to AZ31(-1.56 V)and AZ91(-1.6 V).Occurrence of a more negative OCP for Mg metal indicates their active behavior possibly their oxidation in to Mg2+ion that changes equilibrium potential more negative. Though the standard potential of the magnesium electrode is -2.37 V but measurement of their OCP as-1.66 V indicates the formation Mg(OH)2layer over it which is more cathodic in nature.In comparison,more positive OCP of AZ31 and AZ91 alloys may be due to the presence of beta phases which increases the free potential in the positive direction[11]. Observed OCP behavior is in accordance with the weight loss measurement as initially a higher corrosion rate was measured for Mg metal(Fig.1).Formation of mixed hydroxides of Al, Zn along with Mg can be explained similarly.Presence of pure hydroxide containing layer at the Mg surface seems to be more protective compared to mixed hydroxides layer forms on AZ31 and AZ91 alloy surfaces.

    3.2.2.Tafel plots

    Fig.3.Tafel plots for Mg,AZ31 and AZ91 alloys in 3.5%NaCl solution.

    Fig.3 shows the partial cathodic and anodic polarization curves obtained after carrying partial cathodic and anodicpolarization from OCP±150 mV.Different corrosion parameters like corrosion potential(Ecorr),corrosion current density(Icorr),anodic(βa)and cathodic(βc)Tafel constants derived by the Tafel extrapolation,are given in Table 1. Measured Icorrvalues attributes an order of magnitude lower Icorrfor Mg metal as compared to AZ31 and AZ91 alloys.Icorrof AZ91 alloy shows nearly fve times higher than Mg metal. On the other side Icorrof AZ31 alloy occurs nearly twenty times higher than Mg metal.Whereas AZ91 alloy posses three times higher Icorrthan AZ31 alloy.However,derived Icorrvalues make contradiction from the corrosion rates measured from weight losses as AZ91 alloy exhibited unexpectedly a higher corrosion rate as compared to Mg and AZ31 alloy after 3 h of immersion.Occurrence of a lower Icorrof AZ91 alloy than AZ31 alloy suggests their better corrosion resistance in the initial period of exposure.Measurement of a higher values of cathodic Tafel constant(βc)for Mg metal indicates the occurrence of a pronounced cathodic controlled reaction i.e. oxygen reduction reaction as per following reaction(3)

    Since oxygen reduction is a main cathodic reaction,its control is one of the main factor in reducing of corresponding oxidation reaction(formation of Mg2+ion after discharge of two e-).Once hydrolysis reaction starts corrosion reaction proceeds bytheoxidationofMgasMg2+andtheir involvement with OH-ions that produced by the reduction of water molecule[12,13].ThisresultstheformationofMg(OH)2precipitates at the metal surfaces.The reaction involve in the formation of Mg(OH)2can be expressed as per following(reaction 4).

    The overall reactions could be given as per following reaction.

    Similar reactions may also involve in the corrosion of Al and Zn of the alloys.Measurement of a lower βcvalues for AZ31 and AZ91 alloys than Mg metal indicates their lesser tendency in controlling of cathodic reaction.Due to increased cathodic reaction(reaction 3),OH-generation becomes more that increases the anodic oxidation reaction i.e metal dissolution.This is the main reason that anodic Tafel constant(βc) values increases for AZ31 and AZ91 alloys.

    3.2.3.Current density vs time behavior

    The corrosion current fows at OCP were measured under potentiostatically controlled condition.Fig.4 shows thevariations of current densities with time at OCP.From the trends,it can be seen that AZ31 alloy shows an increased anodic current with time,indicating the occurrence of anodic reaction(metal oxidation)under free corrosion condition.The current fows for Mg and AZ91 alloys,are appeared to less anodic,indicating the occurrence of a slow anodic reaction. Present current vs time implies the occurrence of a slow rate of corrosion reaction in Mg and AZ91 alloy as compared to AZ31 alloy.OCP measurements have also demonstrated similar trend of variation with time.

    Table 1Different corrosion parameters derived from Tafel plots.

    Fig.4.Potentiostatic current density behavior with time Mg,AZ31 and AZ91 alloys in 3.5%NaCl solution.

    3.2.4.Potentiodynamic polarization

    Fig.5.Potentiodynamic polarization Mg,AZ31 and AZ91 alloys in 3.5% NaCl solution.

    Potentiodynamic polarization curves recorded in a wide anodic potential range(up to 1.5 V)are demonstrated in Fig.5.From the potentiodynamic polarization behavior,it can be seen that the nature of increase of current densities with potential,is similar for all the three types of electrodes. However,a limitation of current increase start at 1 V for Mgand AZ91 alloy while limitation in current increase occurs at 1.1 V for AZ31 alloy.Occurrence of limitations in current during anodic polarization is mainly due to the accumulation of corrosion product at the electrode surfaces that reduces the current increase further.It is therefore,polarization of metal in this potential region becomes potential independent.

    3.2.5.Electrochemical impedance spectroscopy(EIS) studies

    EIS measurement in the form of Nyquist plot,was carried out after 30 and 90 min of exposure.As shown in Figs.6 and 7,Nyquist plots demonstrate the occurrence of one capacitive semi circle from higher to the middle frequency region and an inductive loop in the lower frequency region for all the three electrodes.In contrast,Cao et al.[8]and Cheng et al.[9]reported the existence of two semicircles;one in the higher frequency and another one in the lower frequency regions. Though,their observed frst semicircle in higher frequency regions was almost indistinguishable.In the present case,the radius of the semicircle occurs considerably more for Mg than AZ91 alloy.In case of AZ31 alloy,it becomes comparatively very less(Fig.6).After the increase of immersion time to 90 min,the radius of semicircle increases further for Mg metal while it decreases for AZ31 and AZ91 alloys(Fig.7).It is reported that the high frequency part in the Nyquist plot represents the properties of the coatings,whereas the low frequency part associated with the Faradaic processes occurring on the bare metal[14,15].In case of Mg and their alloys, presence of thick oxide flm itself behaves as coating that protects metal up to certain level.Therefore,observation of capacitive behavior from higher to middle frequency region is associated with the resistance of the oxide flm.Since the oxide flm present at the Mg metal possess more corrosion resistance,shows a better capacitive behavior.Presence of a poor capacitive behavior for AZ31 and AZ91 alloys suggest their more corrosive behavior.Occurrence of capacitive loops at the low frequency region for AZ91 and AZ31 alloys indicate the continuation of Faradaic process i.e.diffusion process at the metal/solution interfaces.The appearance of a low frequency inductive loop is also related to relaxation of the adsorbed anions on the surface of the metal[15,16].Based on this,it may further be described that presence of Cl-in the corrosive media increases their adsorption at the AZ31 and AZ91 alloy.This results the increase of oxidation of metal by consuming electrons from the oxidized metal at the adsorb sites.This ultimately starts corrosion reaction at particular adsorbed site.Exhibition of comparatively less pronounced inductive loop for Mg metal suggests their lower susceptibility for adsorption Cl-ions.

    Fig.6.EIS measurements(Nyquist diagram)in Mg,AZ31 and AZ91 alloys in 3.5%NaCl solution after 30 min of exposure.

    Fig.7.EIS measurements(Nyquist diagram)in Mg,AZ31 and AZ91 alloys in 3.5%NaCl solution after 90 min of exposure.

    Different EIS parameters like Rct,solution resistance(Rs), and double layer capacitance(Cdl)as given in Table 1,are derived by curve ftting method.Due to presence of one semi circle,an equivalent circuit consisting of resistor connected in series to a parallely connected resistor and capacitor has been used for data analysis.From Table 2,it can be noted that Rctof Mg increases from 310 to 495 Ω cm2after 30 min-90 min exposure.An increase of charge resistance with time attributes the sequential growth of protective Mg(OH)2layer at the Mg surface.In case of AZ91 and AZ31 alloys Rctreduces from 76 to 42 Ω cm2and from 25 to 9.5 respectively after 30-90 min,suggesting decrease of their corrosion resistances with time.In opposite to Rct,an increase of Cdlvalues was measured for both alloy with time.As seen in Table 2,Cdlof AZ31 and AZ91 alloy increases nearly an order of magnitude higher after 30-90 min of exposure.Since Cdlis associated with the water/electrolytes uptake through the pores/defects of the surface flm[17,18],an increase Cdlwith time for AZ91 and AZ31 alloy implies the increase of porosities/defects in their oxide flm.Increase of porosities in the flm increases the diffusion reaction.A decrease of Cdlwith exposure time as observed for the Mg metal(Table 2),suggesting the decrease of porosities/defects in the oxide flm that increases their corrosion resistance.Measurement of Rctand Cdlvalues are well in accordance with the corrosion rate measured byweight loss and Tafel extrapolation as Mg metal showed much better corrosion resistance compared to than AZ31 and AZ91 alloys.

    Table 2Different corrosion parameters derived from EIS diagrams.

    3.2.6.Microstructural examinations

    Surface morphologies of the corroded and uncorroded specimens(after 90 min of exposure)were examined by SEM. Photomicrographs as shown in Fig.8,demonstrates uncorroded(a)and corroded Mg surface(b).As compared to uncorroded surface,corroded surface shows the accumulation of corrosion product over the grain boundaries.Since grain boundaries are thermodynamically more active,precipitation of corrosion product(Mg(OH)2)in this region reduces the corrosion attack.This is perhaps reason for owing better corrosion resistances by Mg metal.

    The surface morphology of uncorroded surface of AZ31 alloy as depicted in Fig.9a,exhibit the presence of a larger area consisting of α phase(matrix)which is surrounded by β phase(Mg17Al12).In case AZ91 alloys,it is diffcult to distinguish between α and β phase as surface is covered by oxide layer(Fig.10a).On the other side,corroded surface of the both alloys shows a presence of thick corrosion product layer(Figs.9b and 10b)which is not protective in nature.

    There is general opinion that presence of β phase in magnesium/alloys plays a major role in their corrosion resistances/ passivation.It acts as a cathode and shows a good passive behavior in broad pH ranges.After the dissolution of the anodic phase(α phase of the matrix),the surrounding phase(β phase)may play the role of a barrier layer in the inhibition of the corrosion reaction.According to the previous studies [19,20],the role of β phase in corrosion process related to its content,size and distribution.When the mass fraction of β phase is high,the grain size of magnesium alloy is small,and the β phase distributes continuously in the matrix containing α phase,so it may play the role of a barrier layer to deter corrosion.On the contrary,if the grain size is larger and the distance between β phases is enlarged,galvanic corrosion may occur that results the decline of the corrosion resistance. Presence of β phase enhances their potential differences which responsible for the generation of local galvanic cells.This ultimately starts corrosion reaction which increases with the time.Based on the above,it may therefore be concluded that presence of a substantial level of Al(~9 wt%)in AZ91 that posses more β phases,exhibits much pronounced galvanic corrosion as compared to AZ31 alloy.

    4.Conclusions

    ·Weight loss measurement shows initially an increase of corrosion rate in order of Mg<AZ91<AZ31 in 3.5% NaCl solution.After 3 h of immersion,the corrosion rate of AZ91 becomes much more than AZ31 alloy due to start of galvanic corrosion.

    ·Measurement of a decrease of corrosion rate with immersion time for Mg metal indicates the formation of a continuous layer of Mg(OH)2at their surface that increases corrosion resistances.Mixed hydroxides of Mg,Al and Zn form at the alloys surface are not benefcial in improving of their corrosion resistance.

    ·Corrosion current density derived from the Tafel extrapolation indicates similar trend as corrosion rate measured by weight loss data during initial immersion period.

    ·Charge transfer resistancemeasurement indicates an increase of corrosion resistance in order as AZ31<AZ91<Mg which is well in accordance with the corrosion rate measurement by Tafel plots and weight loss measurement.Measurement of an increase of Rctwith time for Mg evidences the formation of protective layer over their surfaces while decrease of Rctwith time for both alloys indicates their corrosion with time.

    Fig.8.SEM photomicrographs of Mg uncorroded(a)and corroded after 90 min exposure(b).

    Fig.9.SEM photomicrographs of AZ31 alloy uncorroded(a)and corroded after 90 min exposure(b).

    Fig.10.SEM photomicrographs of Mg uncorroded(a)and corroded after 90 min exposure(b).

    Acknowledgment

    Authors are thankful to director,CSIR-AMPRI for proving laboratory facilities.The present work has not been supported by any funding agency.

    [1]J.I.Skar,Mat.Corros.50(1999)2-10.

    [2]E.Boese,J.Gollener,A.Heyn,J.Strunz Mat.Corros.52(2001) 247-256.

    [3]H.O.Teeple,ASTM,STP 175(1956)89-115.

    [4]G.Song,B.Johnnsson,S.Hapugoda,D.Jhon,Corros.Sci.49(2007) 1245-1265.

    [5]O.Lunder,J.S.Lein,T.Avenue,K.Nisanisanclolu,Corrosion 45(1989) 741-748.

    [6]T.J.Warner,N.Thorne,G.Anussbaum,W.M.Stobbs,J.Surf.Int.Ana. 19(1992)386-392.

    [7]F.Hehman,F.H.fross,W.Young,J.Met.39(1987)14-21.

    [8]F.H.Cao,V.H.Len,Z.Zhang,V.H.Zhang,X.Zhang,Russ.J.Electrochem.43(2007)837-843.

    [9]Y.L.Chang,T.W.Qin,H.M.Wang,Z.Zhang,Trans.Nonferr.Met.Soc. China 19(2005)517-524.

    [10]H.W.Huo,Y.Li,H.N.Wang,F.H.Wang,Mater.Rev.15(2001)25-27.

    [11]M.C.Zhao,P.J.Uggowitzer,M.Liu,P.Schmutz,G.Song,A.Altre, Trans.Tech.Public(2009)473-478.

    [12]P.M.Brandford,B.Case,G.Dearnaley,J.F.Rurner,I.S.Woolseyz, Corros.Sci.169(1976)747-766.

    [13]K.G.Cowan,J.A.Harrison,Electrochim.Acta 25(1980)899-912.

    [14]N.Pebre,T.Picaud,M.Durprat,F.Dabosi,Corros.Sci.29(1989) 1073-1086.

    [15]G.Ruhi,O.P.Modi,I.B.Singh,Surf.Coat.Technol.204(2009) 359-365.

    [16]L.Tomcsanyi,K.Tomcsanyi,I.Varga,H.Batrik,E.Horanyi, E.Maleczki,Electrochim.Acta 34(1989)855-859.

    [17]I.B.Singh,D.P.Mondal,M.Singh,S.Das,Corros.Sci.51(2009) 234-241.

    [18]F.Bellucci,L.Nicodem,Corrosion 49(1993)235-240.

    [19]G.L.Song,A.Andrej,D.Mathew,Corros.Sci.41(1999)249-273.

    [20]G.L.Song,A.Andrej,X.L.Wu,B.Zhang,Corros.Sci.40(1998) 1769-1791.

    Received 17 September 2014;revised 15 January 2015;accepted 2 February 2015 Available online 18 April 2015

    *Corresponding author.Tel.:+91 755 2488260.

    E-mail address:ibsingh58@yahoo.com(I.B.Singh).

    Peer review under responsibility of National Engineering Research Center for Magnesium Alloys of China,Chongqing University.

    http://dx.doi.org/10.1016/j.jma.2015.02.004.

    2213-9567/Copyright 2015,National Engineering Research Center for Magnesium Alloys of China,Chongqing University.Production and hosting by Elsevier B.V.All rights reserved.

    Copyright 2015,National Engineering Research Center for Magnesium Alloys of China,Chongqing University.Production and hosting by Elsevier B.V.All rights reserved.

    久久久久亚洲av毛片大全| 91麻豆av在线| 99在线视频只有这里精品首页| 国产亚洲精品久久久久5区| 啦啦啦 在线观看视频| 久久天堂一区二区三区四区| 久久精品aⅴ一区二区三区四区| 久久人人精品亚洲av| 国产爱豆传媒在线观看 | xxxwww97欧美| 亚洲成人久久爱视频| 十八禁人妻一区二区| 高清毛片免费观看视频网站| 亚洲国产欧美一区二区综合| 久久久国产精品麻豆| 老汉色av国产亚洲站长工具| 午夜视频精品福利| 成人18禁高潮啪啪吃奶动态图| 亚洲九九香蕉| 精品电影一区二区在线| 怎么达到女性高潮| 成人午夜高清在线视频 | 亚洲熟妇中文字幕五十中出| 国产精品1区2区在线观看.| 婷婷丁香在线五月| 亚洲精品粉嫩美女一区| 在线观看www视频免费| 99久久综合精品五月天人人| 日韩视频一区二区在线观看| 亚洲av成人不卡在线观看播放网| 国产又黄又爽又无遮挡在线| 99国产精品一区二区蜜桃av| 欧美av亚洲av综合av国产av| 国产伦一二天堂av在线观看| 真人一进一出gif抽搐免费| 精品国产美女av久久久久小说| 在线视频色国产色| 2021天堂中文幕一二区在线观 | 禁无遮挡网站| 久久精品91无色码中文字幕| 亚洲aⅴ乱码一区二区在线播放 | 久久久久久免费高清国产稀缺| 国产精品电影一区二区三区| 日韩大尺度精品在线看网址| 亚洲国产中文字幕在线视频| 精品久久久久久久久久久久久 | 国语自产精品视频在线第100页| 老司机深夜福利视频在线观看| 日韩精品中文字幕看吧| www日本在线高清视频| 女性被躁到高潮视频| 色老头精品视频在线观看| 午夜日韩欧美国产| 中文字幕高清在线视频| 精品卡一卡二卡四卡免费| 男男h啪啪无遮挡| 国产亚洲精品综合一区在线观看 | 制服人妻中文乱码| 法律面前人人平等表现在哪些方面| 久久草成人影院| 狂野欧美激情性xxxx| 久久草成人影院| 欧美另类亚洲清纯唯美| 国产精品久久电影中文字幕| 亚洲男人的天堂狠狠| 欧美国产日韩亚洲一区| 精品久久久久久久久久久久久 | 精品少妇一区二区三区视频日本电影| 亚洲av五月六月丁香网| 精品少妇一区二区三区视频日本电影| 侵犯人妻中文字幕一二三四区| 一级黄色大片毛片| 亚洲 欧美 日韩 在线 免费| 在线观看www视频免费| 国内少妇人妻偷人精品xxx网站 | a在线观看视频网站| 黄片大片在线免费观看| 成年人黄色毛片网站| 后天国语完整版免费观看| 午夜精品久久久久久毛片777| 午夜精品久久久久久毛片777| 在线观看免费午夜福利视频| 日韩有码中文字幕| 热99re8久久精品国产| 亚洲人成电影免费在线| bbb黄色大片| 黄色片一级片一级黄色片| 亚洲一区高清亚洲精品| 亚洲精品国产一区二区精华液| 国产精品永久免费网站| 中文字幕最新亚洲高清| www.精华液| 特大巨黑吊av在线直播 | 久久久久亚洲av毛片大全| 无遮挡黄片免费观看| 免费在线观看影片大全网站| 国产激情偷乱视频一区二区| 欧美丝袜亚洲另类 | 久久人妻福利社区极品人妻图片| 欧美性长视频在线观看| 高清在线国产一区| 免费在线观看黄色视频的| 欧美性猛交╳xxx乱大交人| 免费高清视频大片| 亚洲av电影在线进入| 亚洲国产精品成人综合色| 国产精品 国内视频| 日本免费a在线| 国产黄色小视频在线观看| 久久亚洲真实| 老鸭窝网址在线观看| 给我免费播放毛片高清在线观看| 后天国语完整版免费观看| 老司机午夜十八禁免费视频| 老司机午夜福利在线观看视频| 熟女少妇亚洲综合色aaa.| 国产99久久九九免费精品| 亚洲一区二区三区不卡视频| netflix在线观看网站| 国产成+人综合+亚洲专区| 亚洲av五月六月丁香网| 日本成人三级电影网站| 悠悠久久av| 国产亚洲av嫩草精品影院| 黄片小视频在线播放| 亚洲精品粉嫩美女一区| 欧美日韩乱码在线| 久久精品91无色码中文字幕| av福利片在线| 成人三级做爰电影| 亚洲精品中文字幕一二三四区| 中文字幕另类日韩欧美亚洲嫩草| 欧美激情高清一区二区三区| 亚洲欧美一区二区三区黑人| 国产亚洲av嫩草精品影院| 中文字幕精品亚洲无线码一区 | 成人国语在线视频| 99热这里只有精品一区 | 日本熟妇午夜| 中文字幕精品免费在线观看视频| 亚洲午夜精品一区,二区,三区| 亚洲专区国产一区二区| 亚洲五月色婷婷综合| 999精品在线视频| 亚洲自拍偷在线| 久久天堂一区二区三区四区| 变态另类丝袜制服| 天天添夜夜摸| 午夜福利在线观看吧| 久9热在线精品视频| 亚洲精品国产一区二区精华液| 观看免费一级毛片| 亚洲国产日韩欧美精品在线观看 | 少妇 在线观看| 一级a爱视频在线免费观看| 一区二区三区高清视频在线| 波多野结衣av一区二区av| 久久婷婷人人爽人人干人人爱| 哪里可以看免费的av片| 一夜夜www| 久久精品成人免费网站| 精品一区二区三区四区五区乱码| 性欧美人与动物交配| 久久人妻av系列| 一级毛片精品| 超碰成人久久| 欧美一区二区精品小视频在线| 日韩成人在线观看一区二区三区| 久久99热这里只有精品18| 欧美性猛交黑人性爽| 国产高清有码在线观看视频 | 亚洲激情在线av| 欧美激情高清一区二区三区| 十八禁人妻一区二区| aaaaa片日本免费| 国产高清videossex| 男女那种视频在线观看| 欧美乱色亚洲激情| 久久精品91蜜桃| 丁香欧美五月| 99热只有精品国产| 久久中文字幕人妻熟女| 久久久久国内视频| 久久久国产成人免费| 美女扒开内裤让男人捅视频| 看免费av毛片| 免费在线观看视频国产中文字幕亚洲| 亚洲中文字幕日韩| 国产三级在线视频| 日本精品一区二区三区蜜桃| 久久人妻福利社区极品人妻图片| 高清毛片免费观看视频网站| 亚洲成国产人片在线观看| 久久午夜综合久久蜜桃| 欧美绝顶高潮抽搐喷水| 国产精品国产高清国产av| 中文字幕精品免费在线观看视频| 国产精品亚洲一级av第二区| 国产野战对白在线观看| 久久亚洲精品不卡| 在线永久观看黄色视频| 亚洲人成77777在线视频| 日韩大码丰满熟妇| 很黄的视频免费| 日韩欧美国产在线观看| 亚洲自偷自拍图片 自拍| 黄色 视频免费看| 草草在线视频免费看| 极品教师在线免费播放| 国产精华一区二区三区| 欧美成人免费av一区二区三区| 亚洲av片天天在线观看| 亚洲精品中文字幕在线视频| 国产精品久久久人人做人人爽| 午夜亚洲福利在线播放| 99在线视频只有这里精品首页| 午夜久久久久精精品| 人妻丰满熟妇av一区二区三区| 美女国产高潮福利片在线看| 91字幕亚洲| 88av欧美| 禁无遮挡网站| 亚洲国产中文字幕在线视频| 黄色毛片三级朝国网站| 亚洲专区国产一区二区| 99re在线观看精品视频| 色综合站精品国产| 长腿黑丝高跟| 51午夜福利影视在线观看| 久久久国产成人免费| 99热这里只有精品一区 | 中文字幕最新亚洲高清| 91九色精品人成在线观看| 在线十欧美十亚洲十日本专区| 好看av亚洲va欧美ⅴa在| 国产亚洲精品久久久久久毛片| 亚洲精品一区av在线观看| 十八禁网站免费在线| 欧美黑人巨大hd| 两人在一起打扑克的视频| 在线国产一区二区在线| 日本免费一区二区三区高清不卡| 亚洲国产精品sss在线观看| 波多野结衣高清作品| 色精品久久人妻99蜜桃| 国产精品久久电影中文字幕| 成人永久免费在线观看视频| 精品电影一区二区在线| 亚洲成av片中文字幕在线观看| 亚洲一码二码三码区别大吗| 亚洲一卡2卡3卡4卡5卡精品中文| 一卡2卡三卡四卡精品乱码亚洲| 好看av亚洲va欧美ⅴa在| 国产爱豆传媒在线观看 | www.自偷自拍.com| 天堂√8在线中文| 69av精品久久久久久| 欧美日韩一级在线毛片| 50天的宝宝边吃奶边哭怎么回事| 精品不卡国产一区二区三区| 久久婷婷成人综合色麻豆| 91九色精品人成在线观看| 欧美日韩中文字幕国产精品一区二区三区| 丝袜人妻中文字幕| 欧美zozozo另类| 日本五十路高清| 草草在线视频免费看| 啪啪无遮挡十八禁网站| 精品日产1卡2卡| 欧美激情久久久久久爽电影| 91成人精品电影| 国产精品av久久久久免费| 国产成人av教育| 日日夜夜操网爽| 国产精品综合久久久久久久免费| 哪里可以看免费的av片| 女警被强在线播放| 99久久99久久久精品蜜桃| 国产精品久久久久久亚洲av鲁大| АⅤ资源中文在线天堂| 国产熟女午夜一区二区三区| 亚洲精品av麻豆狂野| 少妇粗大呻吟视频| 女生性感内裤真人,穿戴方法视频| 成人手机av| 黄色a级毛片大全视频| 99久久久亚洲精品蜜臀av| 国产午夜精品久久久久久| 操出白浆在线播放| 中文字幕高清在线视频| 亚洲自拍偷在线| 亚洲一码二码三码区别大吗| 久久久久久亚洲精品国产蜜桃av| 亚洲最大成人中文| 亚洲成人精品中文字幕电影| 18禁美女被吸乳视频| 日韩欧美在线二视频| 国产精品98久久久久久宅男小说| 久久99热这里只有精品18| 18美女黄网站色大片免费观看| www.熟女人妻精品国产| 国产精品1区2区在线观看.| 一进一出好大好爽视频| 视频在线观看一区二区三区| 法律面前人人平等表现在哪些方面| 美女国产高潮福利片在线看| av在线播放免费不卡| 色播亚洲综合网| 久久久久精品国产欧美久久久| 一二三四在线观看免费中文在| 久久精品国产清高在天天线| 国产精华一区二区三区| 欧美国产日韩亚洲一区| 一级黄色大片毛片| 两个人免费观看高清视频| 精品久久久久久久末码| 日本三级黄在线观看| 亚洲av五月六月丁香网| 香蕉av资源在线| 一区二区三区精品91| 脱女人内裤的视频| 国产爱豆传媒在线观看 | 美女高潮到喷水免费观看| 国内精品久久久久久久电影| 亚洲av片天天在线观看| 婷婷精品国产亚洲av在线| 国产高清有码在线观看视频 | 91av网站免费观看| 色综合欧美亚洲国产小说| 国产精品99久久99久久久不卡| 午夜福利欧美成人| 99riav亚洲国产免费| 一级毛片精品| 人人妻,人人澡人人爽秒播| 国产伦人伦偷精品视频| 亚洲国产中文字幕在线视频| 一级黄色大片毛片| 国产午夜精品久久久久久| 十分钟在线观看高清视频www| 亚洲一区中文字幕在线| 久久婷婷人人爽人人干人人爱| 18禁裸乳无遮挡免费网站照片 | 精品福利观看| 免费电影在线观看免费观看| 麻豆国产av国片精品| 亚洲中文日韩欧美视频| 丁香欧美五月| 视频在线观看一区二区三区| 免费观看精品视频网站| 欧美又色又爽又黄视频| 99国产综合亚洲精品| 精品久久久久久成人av| 亚洲国产高清在线一区二区三 | 麻豆国产av国片精品| 淫妇啪啪啪对白视频| 一边摸一边做爽爽视频免费| 亚洲久久久国产精品| 99热6这里只有精品| 色播在线永久视频| 日韩成人在线观看一区二区三区| 国产精品久久久久久人妻精品电影| 午夜久久久久精精品| 日韩免费av在线播放| 久久久久久大精品| www国产在线视频色| 麻豆成人av在线观看| 国产精品日韩av在线免费观看| 欧美色欧美亚洲另类二区| 国产精品乱码一区二三区的特点| 欧美黄色片欧美黄色片| 亚洲色图 男人天堂 中文字幕| 亚洲av片天天在线观看| 国产一区在线观看成人免费| 十八禁人妻一区二区| 可以在线观看毛片的网站| 久久人人精品亚洲av| 国产精品 国内视频| 夜夜躁狠狠躁天天躁| 此物有八面人人有两片| 国产一区二区三区在线臀色熟女| 精品久久蜜臀av无| 国产精品亚洲一级av第二区| 日本精品一区二区三区蜜桃| 真人一进一出gif抽搐免费| 亚洲av中文字字幕乱码综合 | 午夜福利视频1000在线观看| 一级毛片女人18水好多| 午夜视频精品福利| 狠狠狠狠99中文字幕| 国产高清videossex| 日韩欧美 国产精品| 丝袜美腿诱惑在线| 亚洲国产中文字幕在线视频| 国产亚洲av高清不卡| videosex国产| 欧美中文日本在线观看视频| 亚洲色图av天堂| 黄色视频不卡| www国产在线视频色| 在线观看www视频免费| 久久久久久大精品| 亚洲国产中文字幕在线视频| 每晚都被弄得嗷嗷叫到高潮| 欧美激情高清一区二区三区| 黑人欧美特级aaaaaa片| 精品久久久久久,| 母亲3免费完整高清在线观看| 我的亚洲天堂| 国产男靠女视频免费网站| 一级片免费观看大全| 久久久久久久久中文| av在线播放免费不卡| 美女 人体艺术 gogo| 亚洲一区中文字幕在线| 亚洲精品粉嫩美女一区| 在线看三级毛片| 日本成人三级电影网站| 成人免费观看视频高清| √禁漫天堂资源中文www| 午夜视频精品福利| 亚洲一码二码三码区别大吗| 脱女人内裤的视频| 美女午夜性视频免费| 后天国语完整版免费观看| 不卡av一区二区三区| 深夜精品福利| 精品久久蜜臀av无| 日韩欧美 国产精品| 亚洲aⅴ乱码一区二区在线播放 | 99热这里只有精品一区 | 精品国产一区二区三区四区第35| 国产精品久久久人人做人人爽| 亚洲av电影在线进入| 亚洲欧美精品综合久久99| 每晚都被弄得嗷嗷叫到高潮| 夜夜爽天天搞| 日本在线视频免费播放| 老司机在亚洲福利影院| 久久久水蜜桃国产精品网| 国产精华一区二区三区| 国产成人精品久久二区二区免费| 国产欧美日韩一区二区三| 国产单亲对白刺激| 欧美一区二区精品小视频在线| 亚洲五月天丁香| 精品卡一卡二卡四卡免费| 亚洲精品色激情综合| 精品久久久久久成人av| 国内少妇人妻偷人精品xxx网站 | 午夜视频精品福利| 在线观看午夜福利视频| 欧美性长视频在线观看| 久久久国产精品麻豆| 最近最新中文字幕大全电影3 | 国产亚洲精品久久久久5区| 可以在线观看毛片的网站| 国产免费av片在线观看野外av| 国产亚洲欧美98| 欧美一区二区精品小视频在线| 又大又爽又粗| 中文字幕精品免费在线观看视频| 啦啦啦 在线观看视频| www.熟女人妻精品国产| 18禁黄网站禁片免费观看直播| 非洲黑人性xxxx精品又粗又长| 久久婷婷成人综合色麻豆| a级毛片在线看网站| 中文字幕精品免费在线观看视频| 国产三级黄色录像| 天堂影院成人在线观看| 午夜福利欧美成人| 十分钟在线观看高清视频www| 嫩草影视91久久| 给我免费播放毛片高清在线观看| 色婷婷久久久亚洲欧美| 亚洲人成77777在线视频| 国产99久久九九免费精品| 亚洲激情在线av| 99久久综合精品五月天人人| 精品人妻1区二区| 午夜精品久久久久久毛片777| 亚洲人成网站在线播放欧美日韩| 69av精品久久久久久| 又黄又粗又硬又大视频| videosex国产| 中文字幕久久专区| 国产伦一二天堂av在线观看| 国产一区二区激情短视频| 久久国产精品人妻蜜桃| 久久99热这里只有精品18| 亚洲欧美精品综合久久99| 欧美日本亚洲视频在线播放| 久99久视频精品免费| 亚洲中文字幕一区二区三区有码在线看 | 久久久久久久久中文| 亚洲第一青青草原| 成人三级做爰电影| 久久久国产欧美日韩av| 在线av久久热| 午夜影院日韩av| 国产视频内射| 韩国精品一区二区三区| 制服诱惑二区| 成人特级黄色片久久久久久久| 精品久久久久久久末码| 久久久久国产精品人妻aⅴ院| 99国产综合亚洲精品| 在线国产一区二区在线| 国产一区二区在线av高清观看| 50天的宝宝边吃奶边哭怎么回事| 欧美午夜高清在线| 国产精品 欧美亚洲| 啦啦啦免费观看视频1| 久久久久久亚洲精品国产蜜桃av| 亚洲av成人不卡在线观看播放网| 国产真实乱freesex| 国产成人欧美| 成人手机av| 在线观看66精品国产| 精品久久久久久久末码| 亚洲av五月六月丁香网| а√天堂www在线а√下载| 超碰成人久久| 午夜亚洲福利在线播放| 国产熟女xx| 成在线人永久免费视频| 精品卡一卡二卡四卡免费| 亚洲中文av在线| 99精品在免费线老司机午夜| 国产成年人精品一区二区| 国产又黄又爽又无遮挡在线| 久久99热这里只有精品18| 日本在线视频免费播放| 男女做爰动态图高潮gif福利片| 亚洲精品国产一区二区精华液| 久久国产精品男人的天堂亚洲| 久久精品国产99精品国产亚洲性色| 久久人人精品亚洲av| 十分钟在线观看高清视频www| 午夜福利在线在线| 非洲黑人性xxxx精品又粗又长| 日韩免费av在线播放| 中文字幕人妻熟女乱码| 国产一级毛片七仙女欲春2 | 久久国产精品影院| 国产精品 国内视频| 手机成人av网站| 最近最新免费中文字幕在线| 在线观看66精品国产| 视频在线观看一区二区三区| 精品少妇一区二区三区视频日本电影| 亚洲精华国产精华精| 亚洲五月色婷婷综合| 男人的好看免费观看在线视频 | 欧美日韩黄片免| 成年人黄色毛片网站| 999久久久精品免费观看国产| tocl精华| 悠悠久久av| 人人妻人人澡人人看| 国产精品久久久久久亚洲av鲁大| 国产极品粉嫩免费观看在线| 日韩免费av在线播放| 免费在线观看成人毛片| 国产三级在线视频| 婷婷丁香在线五月| 久久婷婷人人爽人人干人人爱| 正在播放国产对白刺激| 黄片小视频在线播放| 人妻丰满熟妇av一区二区三区| av有码第一页| 亚洲国产欧美网| 欧美激情高清一区二区三区| 99国产精品一区二区三区| 大型av网站在线播放| 国产精品一区二区精品视频观看| 欧美在线一区亚洲| 欧美日韩精品网址| 久久天躁狠狠躁夜夜2o2o| 国产视频一区二区在线看| 亚洲五月婷婷丁香| 久久香蕉精品热| 亚洲成av人片免费观看| 免费在线观看影片大全网站| 可以在线观看的亚洲视频| 免费看a级黄色片| 欧美日韩亚洲国产一区二区在线观看| 国产主播在线观看一区二区| 日本三级黄在线观看| 99热只有精品国产| 亚洲精品av麻豆狂野| 国产精品爽爽va在线观看网站 | 亚洲精品在线观看二区| 国产成人欧美在线观看| 亚洲精品久久成人aⅴ小说| 欧美中文综合在线视频| 国产精品,欧美在线| xxx96com| 色综合站精品国产| 在线观看舔阴道视频| 51午夜福利影视在线观看| 亚洲欧美精品综合一区二区三区| 两性夫妻黄色片| 日韩精品青青久久久久久| 精品久久蜜臀av无| 丰满的人妻完整版| 精品国产乱子伦一区二区三区| 久久久国产精品麻豆| 不卡av一区二区三区| 叶爱在线成人免费视频播放| 熟妇人妻久久中文字幕3abv| 老鸭窝网址在线观看| 国产一级毛片七仙女欲春2 | 不卡一级毛片| 亚洲人成伊人成综合网2020|