    Experimental and numerical studies of titanium foil/steel explosively welded clad plate

    2023-07-31 13:30:56ZhixiongBiXuejioLiKeYngRongKiQunWngMengenXuTingzhoZhngXindeDiJingyeQinYongWu
    Defence Technology 2023年7期

    Zhi-xiong Bi ,Xue-jio Li ,Ke Yng ,Rong Ki ,Qun Wng ,Meng-en Xu ,Ting-zho Zhng ,Xin-de Di ,Jing-ye Qin ,Yong Wu

    a School of Civil Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    b School of Chemical Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    cSchool of Mining Engineering, Anhui University of Science and Technology, Huainan, Anhui, 232001, PR China

    Keywords:Explosive welding Pressure transfer layer Titanium foil Simulation Bonding property

    ABSTRACT Ti/Fe clad plate had attracted extensive attention because of its important application.In order to reduce the titanium layer thickness,the explosive welding of TA1 titanium foil to Q235 steel plate was carried out.The interfacial bonding performance was analyzed by micromorphology analysis and mechanical property test,and the formation process of interfacial wave and molten block in the vortex was simulated by smoothed particle hydrodynamics (SPH) method.The results showed that salt as pressure transfer layer used in explosive welding could play a good buffer effect on the collision between flyer and base layers.Regular waveforms were formed on the bonding interface,and the titanium foil/steel clad plate exhibited good welding quality and bonding property.The crest of the observed interfacial wave moved 200 μm from the beginning to the final formation,and it was important of jet on the formation of interfacial waveform.The interface was mainly bonded in the form of molten layer,and the grains near the interface were streamlined.Molten block containing intermetallic compounds and metal oxides appeared in the vortex of wave crest.

    1.Introduction

    Titanium could rapidly form a stable oxidizing protective film in air or solution[1-4].Ti/Fe clad plate has both corrosion resistances of titanium and toughness of steel,which has great utilization potentiality in chemical equipment,power generation assembly and ocean engineering [5-7].Explosive welding is an important processing method for Ti/Fe clad plate,which converts chemical energy released by explosive detonation into kinetic energy of flyer layer to achieve metallurgical bonding between the two metallic plates [8-11].Flyer layer for explosive welding needs to collide with base layer at high speed,thus the thickness of flyer layer is generally more than 2 mm to withstand explosion load [12-15].However,titanium layer with a thickness of 400 nm could play a corrosion resistance effect [1,2,16].

    Due to the excellent bonding ability and corrosion resistance,it has drawn increasing interest in the explosive welding of titanium to steel.In Ning et al.'s work,Zr/Ti/Fe clad plate was fabricated by explosive welding,and their microstructure and mechanical properties were studied.The corrosion resistance of zirconium and titanium in the trilaminar clad plate was complementary[14].Song et al.[7] explored the microstructure of explosive cladding joints formed among parallel titanium and steel plates and found the bonding interface formed pronounced hierarchical microstructures.Somasundaram et al.[15] investigated the interfacial structure and corrosion resistance of TA1/304L clad plate by changing mass ratio and preset angle.The microstructural study revealed the transformation from straight to wavy interface while increasing loading ratios,and the clad plate has superior performance in corrosion environment because of the formation of titanium oxide layer.In Chu et al.’s study[12],low carbon steel and pure titanium were welded by explosive welding,and intermetallic compounds of Fe2Ti and FeTi were found at the bonding interface.Zhou et al.[6]investigated the tensile shear failure mechanism and mechanical properties of TA2/Q235 clad plate.The tensile shear failure mainly occurred along the interfacial wave direction and was caused by the defects of cavities,cracks and brittle intermetallic compounds.

    The cladding thickness of clad plate might only need a few hundred microns to meet the performance requirements.Many attempts had been made to realize explosive welding of metallic foil,and the bonding properties and interfacial formation mechanism of clad plates were investigated by numerical simulation,mechanical property testing and microstructure analysis.In Yang et al.’s study[11],aluminum plate as a protective layer was placed between explosive and tantalum foil,and the tantalum foil was successfully welded to steel plate by improving traditional explosive welding technology.The microstructures of welded joints were analyzed by scanning electron microscope (SEM) and energy disperse spectroscopy (EDS),and the corrosion resistance of Ta/Fe clad plate was investigated by corrosion test.Inao et al.[17] reported that the explosive welding of aluminum foil to magnesium alloy plate was successfully realized by adding gel material as pressure transfer layer to the surface of aluminum foil,and the attenuation effect of gel material on collision energy was studied.Yang et al.[18] explored a double-layer structure consisted of a cardboard and a thin aluminum plate as a buffer layer to reduce the surface ablation and stress wave damage of copper foil/steel explosive welding.The interface evolutions,nanomechanical properties and relevant governing mechanisms of copper foil/steel welding system were investigated by SPH simulation method and advanced characterization.In Liu’s work[19],the metallic glass foil was attached on a driver plate,and an aluminum plate was coated by a Fe-based metallic glass foil.The explosive welding process was simulated by a self-developed code and the bonding mechanism was studied by numerical analysis.The buffer materials used above were inevitably damaged under the explosion load and could not be reused.

    In this work,the explosive welding of titanium foil to steel plate was studied by using low detonation velocity emulsion explosive as welding charge and salt as pressure transfer layer.Microstructure evolution of the welding interface was characterized by optical microscope(OM),scanning electron microscope(SEM)and energy disperse spectroscopy (EDS).The mechanical property was measured by tensile and bending tests.The explosive welding process was simulated by smoothed particle hydrodynamics(SPH)method.

    2.Materials and models

    2.1.Experimental procedure

    A TA1 titanium plate with a dimension of 200 μm × 100 mm × 200 mm was bonded to a Q235 steel with a dimension of 15 × 100 × 200 mm3.The chemical composition of participant metals is given in Table 1.

    Table 1 Chemical composition of TA1 titanium and Q235 steel.(mass fraction%).

    Based on emulsion matrix(Table 2),hollow glass microspheres were used as sensitizer and diluent to prepare low detonation velocity emulsion explosive with 20% microsphere content,whose density was 685 kg/m3and detonation velocity was 3148 m/s.Aluminum honeycomb plate was used as explosive frame,which had good compressive resistance and could ensure uniform charge thickness.Honeycomb structure explosive with a thickness of12 mm was prepared by filling honeycomb pores with the emulsion explosive,specific parameters of aluminum honeycomb panel could be found in previous work[20].A 5 mm thick salt layer was placed on the surface of flyer plate as pressure transfer layer.Salt crystal was liquefied under the high temperature of 1079 K,which could protect titanium foil from high temperature burn and reduce impact load damage [21,22].

    Table 2 Emulsion matrix component.(mass fraction%).

    A parallel structure was employed to the explosive welding assembly,as shown in Fig.1.The stand-off distance between base and flyer layers was 4 mm.The inner surfaces of the titanium foil and steel plate were polished,and the welding assembly was placed on the foundation of spherical tank.The initiating end was located on the left part of the charge.

    Fig.1.Assembly drawing of explosive welding of TA1 titanium to Q235 steel.

    After explosive welding,the specimens for microscopic morphology analysis were cut parallel to the direction of detonation by wire cutting machine.The position of the specimen was 100 mm away from the initiation end,which can avoid unstable detonation effect of the explosive in the initiation end.The general morphology was checked via OM(Carl Zeiss Axio Imager A1m)and SEM (Phenom ProX).The mechanical properties were tested by universal testing machine (MTS 810).

    2.2.Explosive welding simulation

    2.2.1.Collision velocity

    A 2D planar model was developed in ANSYS/AUTODYN code for the explosive welding of TA1 titanium foil to Q235 steel plate.The SPH processor exhibited advantages in accurately simulating the deformation behavior of materials [23,24].The parameters of emulsion explosive and salt in the simulation were consistent with those in the experiment.To obtain the collision velocity between flyer and base plates,2D simulation based on ANSYS/AUTODYN code was carried out.The flyer material was TA1 titanium with a thickness of 200 μm,and the base material was Q235 steel with a thickness of 15 mm.The stand-off distance between base and flyer layers was 4 mm.A gauges point was set on the inner surface of flyer layer every 3 mm,as shown in Fig.2.The particle size was 0.1 × 0.1 mm2,and there were 96,600 particles in the model.

    Fig.2.Assembly drawing of explosive welding.

    Jones-Wilkins-Lee (JWL) equation of state (EOS) was used for the explosive,and its calculation formula was as follows [25]:

    wherePis the detonation product pressure,AJ,BJ,R1,R2and ω are the material coefficients,E0is the initial specific internal energy,and V0is the relative specific volume of detonation gas products.The state parameters of the emulsion explosive are listed in Table 3.

    Table 3 Jones-Wilkins-Lee equation of state parameters of explosive.

    Pressure transfer layer was modelled using Compaction equation of state and Mo Granular material model,which had better simulation effect for granular material.Compaction equation of state is often used to describe granular materials,and its calculation formula was as follows [26]:

    wherePis the pressure,a,c,d,and λ are constant parameters that will be determined based on various curve fitting techniques.ρ0is the initial density of the material,ρHis the current density of the material.

    The pressure transfer layer was formed by salt particles,and the density of salt particles with various sizes was different.In order to reduce the differences to achieve better simulation effect.Different initial parameters were set for Compaction equation of state and Mo Granular material model.In the work,four kinds of particles were set to form the pressure transfer layer,the initial densities salt of salt particles with the same size were shown in Table 4.

    Table 4 Compaction equation of state parameters of pressure transfer layer.

    The Mo Granular material model can be described as [27].where σY,σP,σρand F denote the total yield stress,the pressure yield stress,the density yield stress and the pressure of granular respectively.Accordingly,pressure yield stress and the density yield stress of pressure transfer layers composed of the four kinds of particles were shown in Table 5.

    Table 5 Mo Granular material model parameters of pressure transfer layer.

    where ρ is the material density,Γ0is the Grüneisen coefficient,c0is the volumetric sound velocity,sis the material constant,eis the inner energy,c0is the bulk sound velocity.The specific parameters of the Mie-Gruneisen equation of state of TA1 titanium and Q235 steel are shown in Table 6.

    Table 6 Mie-Gruneisen equation of state parameters of TA1 titanium and Q235 steel.

    Johnson-Cook material model was used as the constitutive model for Q235 steel,which could be expressed as [30,31].

    where εPis the effective plastic strain;is the effective plastic strain rate;A,B,C,m and n are the correlation constants of materials,T2is the particle temperature,T* is the dimensionless temperature,Tris the reference temperature,Tmis the melting point.The specific parameters of Johnson-Cook material model of Q235 steel were shown in Table 7.

    Table 7 Johnson-Cook material model parameters for Q235 steel.

    Steinberg-Guinan material model was used as the constitutive model for TA1 titanium,which described the expressions of shear modulus and flow stress before material melting as [32-34].

    whereYis the flow stress,μ is the shear modulus,is the equivalent plastic strain,V1is the relative volume,Y0,β1,n,μ0,b,h and T1are the given medium constants.The specific parameters of the Steinberg-Guinan material model for TA1 titanium were shown in Table 8.

    Table 8 Steinberg-Guinan material model parameters for TA1 titanium.

    2.2.2.Collision simulation

    In order to obtain TA1/Q235 explosive welding parameters and study the formation mechanism of wavy interface,the collision velocities of 11 gauges points were obtained by explosive welding simulation,and the collision angles of the corresponding collision velocities were calculated.The formula for calculating the collision angle with parallel installation structure could be expressed as[35,36].

    wherevpis the collision velocity,vcis the collision point velocity,β is the collision angle,and vdis the detonation velocity of explosive.

    The critical collision velocity between dissimilar metal plates was given by the following formula [37]:

    When the girl had finished she went back to find the cows, but they had gone, and though she hunted everywhere she never found them; and she had to return home and confess to her master, who scolded her bitterly, and afterwards beat her

    wherevp,minis the critical velocity,vp1andvp2are the minimum collision velocity between flyer layers and between base layers,respectively,p1andp2are the collision pressure between flyer layers and between base layers,respectively,CV1andCV2are the volume sound velocities of flyer and base layers,respectively,ρ1and ρ2are the density of flyer and base layers,respectively,and σb1and σb2are the tensile strengths of flyer and base layers,respectively.

    According to the fluid mechanics theory,when the collision point velocity exceeded its lower limit,the interfacial metal transformed from laminar flow to turbulent flow,resulting in a wavy bonding.For the critical collision point velocity,the formula was as follows [38]:

    wherevc,minis the critical collision point velocity,Reis the Reynolds number,andH1andH2are the Vickers hardness of flyer and base plates,respectively.

    Walsh et al.[39] proposed that the ultimate collision velocity between dissimilar metal plates could be expressed as

    wherevp,maxis the ultimate collision velocity,CP1andCP2are the specific heat capacities of flyer and base layers,respectively,α1and α2are the thermal diffusivity of flyer and base layers,respectively,C1and C2are the sonic speed of flyer and base layers,respectively,δ1and δ2are the thickness of flyer and base layers,respectively,Tmpminis the lower melting point of flyer and base layers,tminis the shortest time for the sparse waves to reflect to the bonding interface,and N is the coefficient related to the sonic speed of material.

    In explosive welding,a large enough collision angle was required for the interfacial metal to produce jet.Therefore,the formula of ultimate collision point velocity was proposed by collision angle [40].

    wherevc,maxis the ultimate collision point velocity.

    An oblique collision assembly was used to focus on the collision process of Ti/Fe explosive welding in the simulation model,as shown in Fig.3.In order to save calculation time,the size of TA1 titanium as flyer layer was 200 μm×10 mm,and the size of Q235 steel as base layer was 0.5×10 mm2.The equation of state,material model and numerical simulation method remained unchanged.The particle size was reduced to 4 × 4 μm2,and there were 437,500 particles in the model,which could be enough to get accurate simulation results.The collision angles were calculated according to the collision velocities of the 11 gauges points,as shown in Table 9.

    Fig.3.Schematic diagram of oblique collision model.

    Table 9 Collision velocities and collision angles in the model.

    3.Results and discussion

    3.1.Simulation results of TA1/Q235 explosive welding

    The upper limit and lower limit parameters of TA1/Q235 weldability window were calculated according to Eq.(13) to Eq.(20),as shown in Table 10.

    Table 10 Weldability window parameters for TA1/Q235 explosive welding.

    The critical collision velocity and limit collision velocity of the welding mode were 423 m/s and 2027 m/s,respectively,which was marked by dotted lines in Fig.4.

    The collision velocities of the welding models were all higher than the critical collision velocities,which indicated that the parameters used for explosive welding of titanium foil to steel plate were reasonable [41].The starting and ending points of the explosive were affected by sparse wave,where the collision velocity was small [10].However,the detonation velocity increased and tended to be stable as the detonation transmission distance increased.

    According to the parameters in Table 10,the weldability window was obtained,as shown in Fig.5.The collision velocities and collision angles of the 11 gauges points were represented by dotted lines in different colors.

    Fig.5.Weldability window of TA1/Q235 explosive welding.

    It could be seen in Fig.4 that the first gauges point was located at the edge of the weldability window,and the following gauges points were in the middle of the window.The lower collision velocity at the initiating end would affect the interfacial bonding of clad plate.

    3.2.Collision simulation results

    TA1/Q235 explosive welding was simulated by the welding parameters of the 11 groups in Table 9,and the results were shown in Fig.6.

    The collision velocity of the first group was low,and the interface exhibited a linear bonding.From the second group to the next ten groups,as the detonation transmission distance increased,the collision velocity gradually stabilized,and the bonding interface transformed from straight to wavy.There were scattered particles in the collision zone,which were metal jets of titanium and steel.The number of titanium particles were significantly more than that of steel particles.Materials with low density were more likely to form jets,which was consistent with the results of Wang [42].Metal jet could remove oxide layer and impurities on the inner surface of base and flyer layers,which was beneficial to the bonding of the two materials.

    3.3.Microscopic morphology analysis

    In order to study the morphology of TA1/Q235 bonding interface,the metallographic sample was prepared by grinding and polishing the sample along the direction parallel to the detonation wave.The microstructure was observed by OM,as shown in Fig.7.

    Fig.7.Metallographic structure of TA1/Q235 interface.

    Fig.7 showed' the metallographic structure of TA1/Q235 clad plate.A black molten metal appeared at the interface,which was mainly bonded in the form of molten layer,and the grains near the interface were streamlined.During explosive welding,the high speed collision in a very short time caused the melting of the interfacial metal and strong plastic deformation of the grains on the steel side,resulting in rheological phenomenon and the grains on the steel side exhibited a streamline shape.The phenomenon was accordance with previous works [43-45].The interfacial air was not completely discharged in the high speed collision between base and flyer layers.Under the joint action of adiabatic compression heat and plastic deformation heat,the interfacial metals melted and diffused to form a black molten layer [44].

    It could be seen in Fig.7 that the metallographic structure in the vortex of the crest contained Ti metal particles.Part of the broken particles were involved in the vortex during the movement,and finally formed molten blocks coated by base material.It was consistent with the phenomenon observed in the explosive welding by predecessors [11,46,47].

    In order to further study,the components of the molten block in the vortex and molten layer at the crest,SEM observation and EDS analysis were performed,and the results were shown in Fig.8.

    Fig.8.SEM and EDS analysis of the TA1/Q235 clad plate:(a)waveform at the interface;(b)Point scanning at the crest;(c)Map scanning at the crest;(d)Partial magnification of the molten region at the crest.

    Fig.8(a) showed the back scattering diagram of the TA1/Q235 bonding interface.The average wavelength and amplitude were 100 μm and 35 μm,respectively.No holes and cracks appeared at the interface,indicating that the TA1/Q235 clad plate had good bonding quality.The average thickness of titanium layer was 170 μm,lower than its original thickness of 200 μm.Because the residual energy of the collision between base and flyer layers directly was acted on the metallic material,the residual deformation occurred in the thickness of the clad plate [19,40].Fig.8(b)displayed the local magnified scanning electron microscopy image of the wave crest.Molten layer exited on the TA1/Q235 bonding surface and the vortex of the crest contained molten block.Point scanning was conducted for points 1 to 6 in Fig.8(b)to analyze the components of molten layer and molten block,and the results were shown in Table 11.According to the point scanning element analysis of points 1 to 3,the molten layer was mainly composed of Ti element and contained a small amount of Fe and O elements.It could be seen in Table 11 that O element was detected in the molten layer,which might be because the inner surface of the metallic plate was not completely cleaned or the air between flyer and base plates was not completely expelled [5,48].According to the atom ratio of Ti to Fe,the molten block was mainly composed of intermetallic compounds of FeTi and Fe2Ti [7,10,12].

    Table 11 Point scanning analysis results.

    It could be observed in Fig.8(c) and (d) that the tissues on the steel side rotated,and the metallic particles in the middle form vortices,reflecting the characteristics of rotational motion during the formation of the wavy interface.It was consistent with the grain deformation of steel in the metallographic observation,indicating that the interfacial metal was in a state of high temperature and high pressure in the process of explosive welding,and the metal exhibited quasi-fluid behavior [18,19].The molten titanium and oxygen elements might form a small amount of titanium oxides,while a small amount of Fe elements diffused to the titanium layer near the interface.The molten metal cooled in a very short time,thus elemental diffusion was not obvious.

    3.4.Mechanical property testing

    The tensile and bending specimens were prepared following GB/T 6396-2008,which was used to characterize the bonding strength of the interface under tensile failure and the plastic deformation ability of the clad plate under bending load.The tensile and bending specimens were processed by three-point bending and tensile tests,respectively.The thickness of tensile and bending specimens was 2 mm,including 200 μm thick titanium layer and 1.8 mm thick steel layer.The specific sizes were shown in Fig.9 and Fig.10.

    Fig.9.The size of tensile specimen.

    Fig.10.The size of bending specimen.

    The specimens were put into the three-point bending mold for bending test,and the bending specimen was observed for separation or crack to characterize its cold working bending performance.Experimental conditions and results were shown in Table 12 and Fig.11,respectively.

    Fig.11.Physical drawing of specimen after bending.

    Table 12 Conditions and results of bending test.

    It could be seen from Table 12 and Fig.11 that no separation or local cracks were found at the interface of outcurve and incurve specimens,and the interface remained intact,indicating that the clad plates had good bending properties during cold working.

    There might be microscopic defects at the bonding interface of the clad plate,and these defects might develop along the welding direction as crack sources under the action of external loading.The fracture morphology was observed by SEM to study interfacial morphology and bonding quality of tensile fracture specimens.The tensile failure specimen and fracture morphology were shown in Fig.12 and Fig.13,respectively.

    Fig.12.Physical drawing of tensile failure specimen.

    Fig.13.Fractography of tensile fracture specimen close to the interface: (a) At the interface;(b) TA1 layer;(c) Q235 layer.

    Fig.13 showed the fractography of titanium foil/steel tensilefailure specimen.No separation and cracks were observed at the fracture interface,and the bonding quality of the interface was good.The tensile fracture exhibited obvious plastic deformation,and there were numerous dimples with different sizes on the fracture surface of titanium and steel layers.Compared with that of the titanium side,the dimple size on the steel side was smaller and shallower,as shown in Fig.13(b) and Fig.13(c).After high speed collision,high temperature melting and rapid cooling occurred at the interface [11].Although the process restored the toughness of the material to some extent,the possible microscopic holes in the material could be not eliminated.After nucleation,growth and aggregation of microspores under plastic deformation,these microspores were connected to each other,resulting in the ductile fracture of the material [5,48].

    3.5.Formation mechanism of waveform and molten block

    Explosive welding is transient and it is difficult to study the whole welding process through experiment.Bahrani-blackcrossland theory,helmholtz instability theory,vortex shedding mechanism and stress wave mechanism are the main theoretical achievements at present,among which Bahrani-black-crossland theory has a high degree of recognition.The theory takes into account the effects of collision point pressure,jet penetration and shear stress,which describes the formation of vortices and periodic waveforms vividly [18,49].

    The parameters of collision velocity of 1358 m/s and collision angle of 2°were used for the collision simulation.The particles that constituted the waveform were tracked,and their velocity vectors at each stage were shown in Fig.14.The observation position was fixed and the variation of interfacial waveform was recorded every 0.01 μs,as shown in Fig.14(a).The observed interfacial wave crest moved 200 μm from the beginning to the final formation.Therefore,when the collision velocity was appropriate,the interface still needed a certain distance to form wavy bonding,which might affect the bonding morphology at the initiation point.The simulation and velocity vector diagrams of key positions of explosive welding interface were studied,as shown in Fig.14(b)-Fig.14(f).In the Bahrani-black-crossland theory,it was considered that the interface presented wavy bonding under the action of salient and re-entrant jets [49].

    Fig.14.Collision simulation diagrams and velocity vector diagram: (a) The changing process of waveform formation,The steps of interfacial waveform formation (b1-d1)with corresponding velocity vector (b2-d2),The beginning of the vortex (e1) with corresponding velocity vector (e2),(f) The end of the vortex.

    Fig.14(b1) showed the initial position of the interfacial waveform.It could be seen that the salient jet generated by the previous waveform scoured base material.The jet resulted in indentation and bump on the surface of base material,which gradually developed into a complete waveform in the subsequent evolution.The velocity of the re-entrant jet reached about 2000 m/s.The waveform formed under the action of high speed scouring and extrusion indicated the important role of jet on the formation of interfacial wave.The salient jet collided with the wave crest and formed reentrant jet in front of wave crest,as shown in Fig.14(c1) and Fig.14(d1).The direction of re-entrant jet was gradually downward,creating conditions for the formation of the next waveform(Fig.14(d1)).As the collision point moved,the particle velocity of the interfacial wave slowed down gradually.At this time,the reentrant jet was easy to form defects such as vortices and holes(Fig.14(e1)),which could affect the bonding performance[11,21,44,50].The re-entrant jet was composed of molten steel and titanium at high temperature,and the air at the interface was not discharged in time,providing an environment for Fe and Ti elements to form metal oxides and intermetallic compounds at high temperature(Fig.14(f)).

    In the collision simulation study,vortex simulation diagram of TA1/Q235 explosive welding could be obtained,as shown in Fig.15(a).The molten block was composed of steel and titanium elements.This was because that steel and titanium melted in a high speed collision,resulting in mutual diffusion and the formation of intermetallic compounds.It could be seen in Fig.15(a)that the gap between particles was large,and there might be oxygen not completely expelled in time at the collision interface,resulting in the formation of metal oxides at the interface.It was similar to the component of molten block observed by SEM image in Fig.15(b).

    Fig.15.SEM and simulation images of vortex: (a) Simulation image of vortex;(b) SEM image of vortex.

    3.6.Interfacial characteristic of TA1/Q235 explosive welding

    The plastic strain,density,temperature and pressure variation rules of collision interface were obtained by numerical simulation to study the interfacial characteristic,as shown in Fig.16.

    Fig.16.Interfacial characteristic diagrams of explosive welding: (a) Temperature distribution;(b) Pressure distribution;(c) Density distribution;(d) Plastic strain distribution.

    Fig.16(a)-Fig.16(d)showed the temperature,pressure,density and effective plastic strain distributions of TA1/Q235 explosive welding interface,respectively.The temperature of the interface and vortex was close to 4000 K,and the interfacial pressure basically exceeded 18 GPa.As the distance from the interface increased,the temperature and pressure of base and flyer materials decreased rapidly.Both base and flyer materials melted,and intermetallic compounds were easily formed at the bonding interface [7,10,12].The molten layer at the interface was usually thin,and base and flyer materials still maintained good mechanical properties when the distance from the interface was 50 μm.The density of titanium and steel was 4.5 g/cm3and 8.0 g/cm3,respectively.However,the density of molten layer at the interface was 7.0 g/cm3,which was between that of titanium and steel.The interfacial metal melted under the action of high temperature and high pressure generated by high speed collision.The molten metal cooled in a very short time to form molten layer,and created conditions for the generation of intermetallic compounds[10,18].It was consistent with the SEM observation.The maximum effective plastic strain of the molten layer and the molten block in the vortex reaches 6.Generally,the higher the temperature was,the lower the strength of the metal was,and the pressure was sharply reduced as the distance from the interface increased [51].Therefore,the effective plastic strain value of the metal at the interface was much larger than that of materials far away from the interface.

    4.Conclusions

    The explosive welding of 200 μm thick titanium foil to steel plate was studied by numerical simulation and experiment.Optical microscope(OM),scanning electron microscope(SEM)and energy disperse spectroscopy (EDS) were used to observe the interfacial microscopic morphology of the TA1/Q235 clad plate.Smoothed particle hydrodynamics(SPH)simulation method code was used to study the forming mechanism of waveform and vortex,and the following conclusions could be obtained:

    (1) Salt was used as a pressure transfer layer,which could decrease the acceleration process of explosive welding and avoid the high temperature burn caused by explosive detonation,and titanium foil/steel explosive welding was successfully achieved.No separation or local cracks were found at the interface of bending and tensile fracture specimens,and the interface remained intact,indicating that the clad plate exhibited good cold workability.

    (2) Regular waveforms could be formed at the interface of the TA1/Q235 clad plate.The average thickness of the titanium layer was 170 μm,and the average wavelength and amplitude of the interfacial waveform were 100 μm and 35 μm,respectively.

    (3) The interface of titanium foil/steel clad plate was mainly bonded in the form of molten layer.The molten layer was mainly composed of Ti element,containing a small amount of Fe element.There were molten blocks in the vortex of wave crest.According to the atomic ratio,the intermetallic compounds were mainly composed of FeTi and Fe2Ti.

    (4) The re-entry jet resulted in indentation and bump on the surface of base material,which gradually developed into a complete waveform in the subsequent evolution,indicating the important role of jet on the formation of interfacial waveform.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    六月丁香七月| 丰满乱子伦码专区| 女人十人毛片免费观看3o分钟| av视频在线观看入口| 日本一二三区视频观看| 午夜激情欧美在线| 婷婷色av中文字幕| 午夜久久久久精精品| 国产成人a区在线观看| 看黄色毛片网站| 亚洲无线观看免费| 日本成人三级电影网站| 国产高潮美女av| 欧美日韩综合久久久久久| 亚洲国产精品合色在线| 久久久久久久久久久免费av| 身体一侧抽搐| 2021天堂中文幕一二区在线观| 国产不卡一卡二| 亚洲av男天堂| 麻豆国产97在线/欧美| 乱人视频在线观看| videossex国产| 国产成人影院久久av| 国产真实乱freesex| 麻豆av噜噜一区二区三区| 中文字幕免费在线视频6| 亚洲国产精品国产精品| 免费av观看视频| 九草在线视频观看| 日韩人妻高清精品专区| 国产精品av视频在线免费观看| 欧美精品国产亚洲| 色播亚洲综合网| 国产老妇伦熟女老妇高清| 国产淫片久久久久久久久| 免费看日本二区| av在线老鸭窝| 在线国产一区二区在线| 人体艺术视频欧美日本| 日本黄色视频三级网站网址| 亚洲真实伦在线观看| 成人国产麻豆网| 99热网站在线观看| 舔av片在线| 夜夜爽天天搞| 一进一出抽搐动态| 色尼玛亚洲综合影院| 亚洲av成人精品一区久久| 久久亚洲国产成人精品v| .国产精品久久| 日韩精品青青久久久久久| 看非洲黑人一级黄片| 免费电影在线观看免费观看| av视频在线观看入口| 国产精品一区www在线观看| 国产v大片淫在线免费观看| 天堂影院成人在线观看| 免费人成在线观看视频色| 日本熟妇午夜| 亚洲一区二区三区色噜噜| 在线观看av片永久免费下载| 成人三级黄色视频| 在线观看一区二区三区| 成人特级av手机在线观看| 国产高清有码在线观看视频| 久久久久九九精品影院| 麻豆精品久久久久久蜜桃| 99热全是精品| 亚洲欧美精品综合久久99| 亚洲国产精品国产精品| 97超碰精品成人国产| 97超碰精品成人国产| 熟妇人妻久久中文字幕3abv| 国产精品不卡视频一区二区| 十八禁国产超污无遮挡网站| 老女人水多毛片| 黄色欧美视频在线观看| 女的被弄到高潮叫床怎么办| 国产乱人偷精品视频| 国产日韩欧美在线精品| 国产精品乱码一区二三区的特点| 寂寞人妻少妇视频99o| 亚洲精品亚洲一区二区| 婷婷六月久久综合丁香| 精品久久国产蜜桃| 日韩高清综合在线| 国产一级毛片在线| 欧美最黄视频在线播放免费| 在线观看66精品国产| 日本五十路高清| av免费在线看不卡| 两个人视频免费观看高清| 好男人在线观看高清免费视频| 午夜精品国产一区二区电影 | 国产精品久久久久久久电影| 欧美日本亚洲视频在线播放| 一边亲一边摸免费视频| 又粗又爽又猛毛片免费看| 久久精品国产自在天天线| 亚洲国产欧美人成| 亚洲四区av| 成熟少妇高潮喷水视频| 在线国产一区二区在线| ponron亚洲| 男女啪啪激烈高潮av片| 99久久精品热视频| av在线天堂中文字幕| 国内精品宾馆在线| 亚洲天堂国产精品一区在线| 大香蕉久久网| 亚洲精品自拍成人| 神马国产精品三级电影在线观看| 丰满的人妻完整版| 一个人观看的视频www高清免费观看| 99在线视频只有这里精品首页| 欧美成人免费av一区二区三区| 啦啦啦韩国在线观看视频| 日韩,欧美,国产一区二区三区 | 99久久精品一区二区三区| 两性午夜刺激爽爽歪歪视频在线观看| 久久久午夜欧美精品| 免费不卡的大黄色大毛片视频在线观看 | 久久99蜜桃精品久久| 日韩中字成人| 天堂√8在线中文| 美女内射精品一级片tv| 欧美丝袜亚洲另类| 国产亚洲av片在线观看秒播厂 | 亚洲第一电影网av| 国产探花极品一区二区| 欧美+亚洲+日韩+国产| 日韩制服骚丝袜av| 九九热线精品视视频播放| 能在线免费看毛片的网站| 国产人妻一区二区三区在| 九九爱精品视频在线观看| 国产成人午夜福利电影在线观看| 久久久久国产网址| 少妇高潮的动态图| 一个人看的www免费观看视频| 国语自产精品视频在线第100页| 亚洲欧美日韩高清在线视频| 国产乱人偷精品视频| 老师上课跳d突然被开到最大视频| 给我免费播放毛片高清在线观看| 18禁裸乳无遮挡免费网站照片| 国产片特级美女逼逼视频| 国产精品嫩草影院av在线观看| 亚洲五月天丁香| 午夜福利视频1000在线观看| 国产伦精品一区二区三区视频9| 男女啪啪激烈高潮av片| 久久欧美精品欧美久久欧美| 成人毛片60女人毛片免费| 美女脱内裤让男人舔精品视频 | 国内精品一区二区在线观看| 成人三级黄色视频| 欧美激情在线99| 一本久久中文字幕| 99久久成人亚洲精品观看| 亚洲在久久综合| 在线观看av片永久免费下载| 国产一区亚洲一区在线观看| 青青草视频在线视频观看| 亚洲内射少妇av| 不卡视频在线观看欧美| 久久草成人影院| 国产一区二区在线观看日韩| 在线播放国产精品三级| 一卡2卡三卡四卡精品乱码亚洲| 能在线免费看毛片的网站| 日本黄色片子视频| 别揉我奶头 嗯啊视频| 精品国内亚洲2022精品成人| 成人综合一区亚洲| 国产黄片美女视频| 久久久久国产网址| 亚洲精品成人久久久久久| 亚洲一级一片aⅴ在线观看| 性插视频无遮挡在线免费观看| 免费看日本二区| 伊人久久精品亚洲午夜| 村上凉子中文字幕在线| 国产黄色小视频在线观看| 麻豆乱淫一区二区| 国产伦一二天堂av在线观看| 国产三级在线视频| 日韩成人av中文字幕在线观看| 国产精品一区www在线观看| 国产欧美日韩精品一区二区| 又粗又爽又猛毛片免费看| 久久久久久大精品| 免费看日本二区| 久久精品国产亚洲av涩爱 | 麻豆国产97在线/欧美| 久99久视频精品免费| 亚洲丝袜综合中文字幕| 此物有八面人人有两片| 久久久久久大精品| 中出人妻视频一区二区| 看免费成人av毛片| 色综合站精品国产| 人妻系列 视频| 精品久久久久久久人妻蜜臀av| 12—13女人毛片做爰片一| 精品午夜福利在线看| 春色校园在线视频观看| 天堂av国产一区二区熟女人妻| 亚洲精品自拍成人| 亚洲七黄色美女视频| 99热这里只有是精品在线观看| av专区在线播放| 国产女主播在线喷水免费视频网站 | 一边亲一边摸免费视频| 乱系列少妇在线播放| 国产探花在线观看一区二区| 2022亚洲国产成人精品| 99九九线精品视频在线观看视频| 日本撒尿小便嘘嘘汇集6| 亚洲av中文字字幕乱码综合| 九九在线视频观看精品| av天堂在线播放| 欧美一区二区亚洲| 校园春色视频在线观看| 内射极品少妇av片p| 日本爱情动作片www.在线观看| а√天堂www在线а√下载| 五月玫瑰六月丁香| 久久99蜜桃精品久久| 成人毛片a级毛片在线播放| 久久久久久久久久久丰满| 国产精品久久久久久精品电影小说 | 此物有八面人人有两片| 在线观看免费视频日本深夜| 国产成人a区在线观看| 嘟嘟电影网在线观看| 国产老妇伦熟女老妇高清| 免费人成视频x8x8入口观看| 嫩草影院新地址| 国产精品久久久久久亚洲av鲁大| 男人舔奶头视频| 最好的美女福利视频网| 亚洲精品成人久久久久久| 2022亚洲国产成人精品| 伦理电影大哥的女人| 国产69精品久久久久777片| 免费黄网站久久成人精品| 久久久国产成人免费| 哪个播放器可以免费观看大片| 国产精品人妻久久久久久| 久久精品国产鲁丝片午夜精品| 日韩 亚洲 欧美在线| 一边摸一边抽搐一进一小说| 两个人视频免费观看高清| 国产一区二区在线av高清观看| 熟妇人妻久久中文字幕3abv| 观看免费一级毛片| 国产精品麻豆人妻色哟哟久久 | 成人一区二区视频在线观看| 成人性生交大片免费视频hd| 卡戴珊不雅视频在线播放| 成人二区视频| 在线天堂最新版资源| АⅤ资源中文在线天堂| 免费在线观看成人毛片| 国产精品1区2区在线观看.| 爱豆传媒免费全集在线观看| 国产美女午夜福利| 亚洲,欧美,日韩| 在线观看一区二区三区| 久久午夜亚洲精品久久| 一级毛片aaaaaa免费看小| 国产三级中文精品| 69av精品久久久久久| 麻豆精品久久久久久蜜桃| 日韩在线高清观看一区二区三区| 亚洲成人中文字幕在线播放| 一本久久中文字幕| 久久亚洲国产成人精品v| 精品久久久久久久久亚洲| 六月丁香七月| 国内精品久久久久精免费| 久久久午夜欧美精品| 欧美zozozo另类| 国产亚洲av片在线观看秒播厂 | 在线a可以看的网站| 亚洲精品成人久久久久久| 天天躁日日操中文字幕| 中文字幕久久专区| 日本五十路高清| 少妇裸体淫交视频免费看高清| 国产精品久久电影中文字幕| 亚洲中文字幕一区二区三区有码在线看| 国内揄拍国产精品人妻在线| 一边摸一边抽搐一进一小说| 欧美变态另类bdsm刘玥| 欧美日韩精品成人综合77777| 毛片一级片免费看久久久久| 国产在线精品亚洲第一网站| av.在线天堂| 黄片wwwwww| 日韩高清综合在线| 少妇的逼水好多| 黄片wwwwww| 欧美zozozo另类| 亚洲三级黄色毛片| 国产极品天堂在线| а√天堂www在线а√下载| 亚洲av成人精品一区久久| 在线观看66精品国产| 天堂√8在线中文| 成人二区视频| 一进一出抽搐gif免费好疼| 免费大片18禁| 亚洲av成人精品一区久久| 日韩欧美精品v在线| 国产成人影院久久av| 久久亚洲国产成人精品v| 九九久久精品国产亚洲av麻豆| 99在线视频只有这里精品首页| 亚洲,欧美,日韩| 97超视频在线观看视频| 午夜爱爱视频在线播放| 国产精品电影一区二区三区| 成人国产麻豆网| 精品一区二区三区视频在线| av在线亚洲专区| 亚洲综合色惰| 日本黄色片子视频| 不卡视频在线观看欧美| 一本—道久久a久久精品蜜桃钙片 精品乱码久久久久久99久播 | 亚洲精品乱码久久久久久按摩| 免费观看人在逋| 国产av一区在线观看免费| 色哟哟哟哟哟哟| a级毛色黄片| 在线观看美女被高潮喷水网站| 亚洲无线在线观看| 桃色一区二区三区在线观看| 亚洲成人av在线免费| 天堂√8在线中文| 国产精品蜜桃在线观看 | 久久久国产成人精品二区| 男的添女的下面高潮视频| 国产成人影院久久av| 免费av观看视频| 国产老妇女一区| 精品免费久久久久久久清纯| 亚洲欧美日韩高清在线视频| av黄色大香蕉| 午夜亚洲福利在线播放| 成人性生交大片免费视频hd| 亚洲天堂国产精品一区在线| 国产探花极品一区二区| 国产免费一级a男人的天堂| eeuss影院久久| 最近视频中文字幕2019在线8| 日本欧美国产在线视频| 久久久久九九精品影院| 老司机福利观看| 尾随美女入室| 日本黄色视频三级网站网址| 久久亚洲精品不卡| 一本—道久久a久久精品蜜桃钙片 精品乱码久久久久久99久播 | 国产在视频线在精品| 国产伦在线观看视频一区| 亚洲国产高清在线一区二区三| 国产蜜桃级精品一区二区三区| 少妇的逼好多水| 免费电影在线观看免费观看| 69av精品久久久久久| 国产一区二区激情短视频| 婷婷六月久久综合丁香| 国产男人的电影天堂91| 哪里可以看免费的av片| 长腿黑丝高跟| 国产视频首页在线观看| 欧美成人一区二区免费高清观看| 亚洲va在线va天堂va国产| 国产真实乱freesex| 人妻少妇偷人精品九色| 成人午夜精彩视频在线观看| 久久久久久久久大av| 免费黄网站久久成人精品| 亚洲成人中文字幕在线播放| 可以在线观看的亚洲视频| 成人毛片60女人毛片免费| 一区二区三区四区激情视频 | 免费电影在线观看免费观看| 国产亚洲av片在线观看秒播厂 | 99久久成人亚洲精品观看| 国产午夜精品久久久久久一区二区三区| 非洲黑人性xxxx精品又粗又长| 国产高清不卡午夜福利| 18禁裸乳无遮挡免费网站照片| 亚洲性久久影院| 美女xxoo啪啪120秒动态图| 国产人妻一区二区三区在| 日本黄大片高清| 性色avwww在线观看| 国产伦一二天堂av在线观看| 日韩成人av中文字幕在线观看| 天堂av国产一区二区熟女人妻| 色综合站精品国产| 如何舔出高潮| 亚洲欧洲国产日韩| 欧洲精品卡2卡3卡4卡5卡区| 精品欧美国产一区二区三| 国产精品人妻久久久久久| 欧美一区二区国产精品久久精品| 国产 一区 欧美 日韩| 国产私拍福利视频在线观看| 又爽又黄无遮挡网站| 91aial.com中文字幕在线观看| 韩国av在线不卡| 色哟哟哟哟哟哟| 亚洲av一区综合| 亚洲丝袜综合中文字幕| 日产精品乱码卡一卡2卡三| 免费观看的影片在线观看| 婷婷亚洲欧美| 亚洲七黄色美女视频| 波多野结衣巨乳人妻| 国产视频首页在线观看| 久久久久免费精品人妻一区二区| 色吧在线观看| 成人综合一区亚洲| 亚洲内射少妇av| 国产在视频线在精品| 国产精品人妻久久久影院| 国内久久婷婷六月综合欲色啪| 丰满的人妻完整版| 91精品国产九色| 国内揄拍国产精品人妻在线| 内地一区二区视频在线| 亚洲国产精品sss在线观看| 午夜精品国产一区二区电影 | 深爱激情五月婷婷| 乱码一卡2卡4卡精品| 国产亚洲91精品色在线| 国产大屁股一区二区在线视频| 91麻豆精品激情在线观看国产| 级片在线观看| 人人妻人人澡欧美一区二区| 国产真实乱freesex| 99视频精品全部免费 在线| 国产三级中文精品| 超碰av人人做人人爽久久| 天堂影院成人在线观看| 国产成人精品婷婷| 日韩一区二区视频免费看| 久久中文看片网| 丝袜喷水一区| 国产成人福利小说| 99热精品在线国产| 狂野欧美激情性xxxx在线观看| 日韩视频在线欧美| 色哟哟·www| 日韩在线高清观看一区二区三区| 国产成人福利小说| 熟妇人妻久久中文字幕3abv| 久久久久久久午夜电影| 欧美人与善性xxx| 亚洲av熟女| 人人妻人人看人人澡| 欧美一区二区亚洲| 国产精品.久久久| 久久综合国产亚洲精品| 国产精品.久久久| 99riav亚洲国产免费| 黄色日韩在线| 日韩亚洲欧美综合| 亚洲电影在线观看av| 精品一区二区三区视频在线| av天堂在线播放| 亚洲成人久久爱视频| 日本五十路高清| 国产美女午夜福利| 欧美日韩精品成人综合77777| 日本在线视频免费播放| 国产不卡一卡二| 日韩视频在线欧美| 欧美激情国产日韩精品一区| 亚洲第一区二区三区不卡| 99久久中文字幕三级久久日本| 麻豆成人午夜福利视频| 日本在线视频免费播放| 少妇熟女aⅴ在线视频| 高清日韩中文字幕在线| 日韩视频在线欧美| 久久欧美精品欧美久久欧美| 搡老妇女老女人老熟妇| 国产视频首页在线观看| 六月丁香七月| 久久精品国产99精品国产亚洲性色| 国产色爽女视频免费观看| 免费无遮挡裸体视频| 日韩中字成人| 久久精品影院6| 美女高潮的动态| 国产蜜桃级精品一区二区三区| 免费观看精品视频网站| 久久人人爽人人爽人人片va| 国产伦理片在线播放av一区 | 老司机影院成人| 日本-黄色视频高清免费观看| 国产美女午夜福利| 国产精品精品国产色婷婷| 国产精品野战在线观看| 国产黄片视频在线免费观看| 两性午夜刺激爽爽歪歪视频在线观看| 一边摸一边抽搐一进一小说| 22中文网久久字幕| 国产中年淑女户外野战色| 国产一区二区在线观看日韩| 欧美极品一区二区三区四区| 国产高清视频在线观看网站| 中文资源天堂在线| 一级二级三级毛片免费看| 三级男女做爰猛烈吃奶摸视频| 亚洲国产精品成人久久小说 | 麻豆乱淫一区二区| 久久人人精品亚洲av| 中文字幕人妻熟人妻熟丝袜美| 99久久中文字幕三级久久日本| 又黄又爽又刺激的免费视频.| 九九热线精品视视频播放| 日韩一区二区视频免费看| 女人十人毛片免费观看3o分钟| av.在线天堂| 毛片女人毛片| 国产三级在线视频| 亚洲第一电影网av| 日韩欧美一区二区三区在线观看| 午夜免费男女啪啪视频观看| 亚洲av熟女| 日韩在线高清观看一区二区三区| 欧美性猛交╳xxx乱大交人| 91精品一卡2卡3卡4卡| 六月丁香七月| 亚洲最大成人中文| 亚洲五月天丁香| 成人高潮视频无遮挡免费网站| 免费观看的影片在线观看| 亚洲乱码一区二区免费版| 免费看av在线观看网站| 色吧在线观看| 色5月婷婷丁香| 亚洲七黄色美女视频| 国产午夜福利久久久久久| 热99re8久久精品国产| 中文欧美无线码| 观看免费一级毛片| 国产成人精品婷婷| 伦理电影大哥的女人| 国产淫片久久久久久久久| 精品人妻偷拍中文字幕| 欧洲精品卡2卡3卡4卡5卡区| a级毛片a级免费在线| 亚洲性久久影院| 国产精品嫩草影院av在线观看| 美女大奶头视频| 欧美成人精品欧美一级黄| 亚洲国产欧洲综合997久久,| 国产成人freesex在线| 久久久久久大精品| 夫妻性生交免费视频一级片| 秋霞在线观看毛片| 国产精品无大码| 大又大粗又爽又黄少妇毛片口| 一区二区三区四区激情视频 | 人妻少妇偷人精品九色| 亚洲欧洲国产日韩| 真实男女啪啪啪动态图| 欧美日韩乱码在线| 欧美不卡视频在线免费观看| 国产精品美女特级片免费视频播放器| 亚洲欧洲国产日韩| 真实男女啪啪啪动态图| 噜噜噜噜噜久久久久久91| 99视频精品全部免费 在线| 成人二区视频| 国产高清激情床上av| 久久亚洲国产成人精品v| 春色校园在线视频观看| 91久久精品电影网| 亚洲精品乱码久久久v下载方式| 亚洲无线在线观看| 久久久久国产网址| 乱系列少妇在线播放| 成人国产麻豆网| 丝袜喷水一区| 99国产精品一区二区蜜桃av| 中文字幕av成人在线电影| 亚洲国产精品久久男人天堂| 国产黄a三级三级三级人| 亚洲经典国产精华液单| 美女高潮的动态| 久久久成人免费电影| 亚洲无线观看免费| 国产精品久久久久久精品电影小说 | 久久久色成人| 久久精品国产自在天天线| 久久久久久久亚洲中文字幕| 精品免费久久久久久久清纯| 日韩av不卡免费在线播放| 亚洲av免费高清在线观看| 26uuu在线亚洲综合色| 国产精品电影一区二区三区| 日韩成人av中文字幕在线观看| 天天躁夜夜躁狠狠久久av| av黄色大香蕉| 97在线视频观看| 亚洲第一区二区三区不卡|