    Development of open-porosity magnesium foam produced by investment casting

    2022-09-26 03:08:26HonortKponCrstenBlwertJekChemnowskiKrzysztofNploh
    Journal of Magnesium and Alloys 2022年7期

    Honort Kp?on,Crsten Blwert,Jek Ch?emnowski,Krzysztof Nploh

    a Faculty of Mechanical Engineering,Wroc?aw University of Science and Technology,Ul.Smoluchowskiego 25,Wroc?aw 50-370,Poland

    b Institute of Surface Science,Helmholtz-Zentrum Geesthacht,Max-Planck-Straβe 1,Geesthacht,21502,Germany

    c Faculty of Chemistry,Wroc?aw University of Science and Technology,Wybrze˙ze Stanis?awa Wyspia′nskiego 27,Wroc?aw,50-370,Poland

    Abstract High-porosity,open-cell AZ91 magnesium alloy foams of two pore sizes were fabricated by means of investment casting technology,using PUR foam patterns.Foam casting variables such as pressure,mould temperature and metal pouring temperature were thoroughly investigated to define the most optimal casting conditions.The mechanical properties of the fabricated foams were measured in compression tests.A potential application for the foams considered is temporary bioresorbable bone implants,therefore the mechanical properties of the foams were compared with those of cancellous bone tissue.Foams with smaller pore size and lower porosity(20 PPI and 80%–87%)exhibited mechanical properties in the lower regions of the cancellous bone property range(Young’s modulus 36.5–77.5 MPa),while foams with higher pore size and porosity(10 PPI and~90%)were found to have insufficient compression strength(Young’s modulus 11.65–23.8),but thickening their walls and lowering their porosity below 90% yielded foams with Young’s modulus between 36.5 and 77.5 MPa.Foam fractures were also investigated to determine their collapse mechanism.A series of corrosion tests in stimulated body fluid was carried out to determine their applicability as a biomaterial.The Plasma Electrolytic Oxidation(PEO)process was used in a feasibility study to examine the microstructure and chemical composition of foams with protective coating.

    Keywords:Magnesium foams;AZ91 investment casting;Bone implants;Plasma electrolytic oxidation.

    1.Introduction

    Metal foams exhibit properties that are unique amongst metal materials.Due to their high surface-to-volume ratio and lower weight,they have found applications mostly in the automotive and aircraft industries,but also as lightweight construction materials,silencers,heat exchangers,filters and catalysts in the chemical industry,or as shock absorbing material in military vehicles[1].On top of that,their porous structure offers the possibility of developing biomaterials applicable as biomedical implants.

    Magnesium,as a material with good biocompatibility,seems like the perfect candidate for this application.It also has similar density and mechanical properties to bone tissue:magnesium density ranges from 1.74 to 2.0 g/cm3,while bone tissue density ranges from 1.8 to 2.1 g/cm3;elastic modulus for Mg ranges from 41 to 45 GPa,while for bone tissue,it ranges from 3 to 20 GPa[2].This means that their mechanical properties are not the same,but much closer than those of steel,titanium or Co-Cr alloys.These properties are an important factor because they decrease the stress in the boneimplant interface,resulting in a more stable environment for bone tissue growth[3].

    Another advantage of magnesium over other materials is biodegradability,which is very important for application as short-term implants.The use of biodegradable material spares the patient the additional steps of removing the implant at the end of treatment.One of the biggest drawbacks of magnesium–low corrosion resistance–poses no threat to the human body since its corrosion products are soluble,non-toxic and can be easily excreted in the urine.Magnesium implants can be gradually dissolved with no harm to the patient’s health,as opposed to steel,titanium or Co-Cr implants that can release toxic products during the corrosion process.Its ions are naturally present in the human body and essential to its metabolism.It is estimated that about 1 mol of Mg is stored in the body of a healthy 70 kg person,half of which is stored in bone tissue[4].One problem with this process is that magnesium corrosion locally increases hydrogen concentration and creates hydrogen bubbles near the implant,which can cause segregation of tissue layers and tissue necrosis,leading to delayed healing[5].

    In order to extend the life of Mg foam implants before they dissolve,special coatings can be developed.Plasma Electrolytic Oxidation(PEO)has proved to be a very efficient method of creating protective coatings on metals such as aluminium[6]or magnesium[7].Their porous structure was found to have both advantages and disadvantages in biomedical applications.It gives less protection against corrosion,but on the other hand,pores have a significant role in hydroxyapatite growth and in better adhesion to bone structure through mechanical interlocking[8].That is why further research in this area is a promising field of study.

    The best known and widely used method for the fabrication of magnesium foams is the space-holder method,which uses a negative pattern(e.g.,salt particles)pre-form that is infiltrated with liquid metal and cleaned.This method,employing salt particle patterns,was used for example in research on Mg-Zn-Ca scaffolds with cubic NaCl particles as a space holder,obtained by Dong et al[9]..Other salt patterns,shaped on 3D-printed polymer scaffolds and after model firing,were infiltrated with pure Mg by Kirkland et al[10]..Jiang and He on the other hand,used a 3D titanium wire structure that was infiltrated with Mg and then removed in a HF solution[11].A significant problem with the space holder method is the residues that cannot be removed from the deep regions of magnesium structures and in the case of salt patterns,they increase corrosion process.Another popular technique for magnesium foam processing is powder metallurgy.Seyedraoufi and Mirdamadi[12]fabricated Mg-Zn alloy foams using powder metallurgy,with carbamide as a space holder,while Yang et al.fabricated closed-cell foams using powder metallurgy with CaCO3as the blowing agent from Mg-Al alloy in[13,14],and Mg-Al-Zn alloy in[15].

    Investment casting can be another method for fabricating magnesium foams.3D structures made with wax or polymer are prepared(for example through fused deposition modelling),put in investment moulds and burnt away.Maier et al.[16]made such models from wax using FDM technology and fabricated magnesium 3D scaffold structures.A different kind of pattern,with much bigger porosity and less preparation effort,can be obtained by using polyurethane foam.Yamada et al.[17]investigated such foams for AZ91 alloy,with a pore size of around 4.5 mm and a density of 0.05 g/cm3.However,they revealed lower mechanical properties(plateau stress of 0.11 MPa),which means that the foams need to be reinforced for this method to be applicable in biomedical implants.The method presented in this research uses a polyurethane foam pattern coated with a wax slurry in order to increase its density and mechanical properties.This technique produces foams with controlled morphology(as opposed to the salt particle space holder method),by using easily available uniform materials and less specialised equipment than the methods mentioned above.

    2.Materials and methods

    2.1.Foam casting process

    The magnesium-based foams were cast with AZ91 alloy(9 wt% of Al,0.13 wt% of Mn,and 0.7 wt% of Zn)widely used in die casting[18].Foam fabrication was based on the investment casting technology combined with evaporation of polyurethane(PUR)foam-pattern.The entire process is illustrated in Fig.1.

    A specific mesh size defined by the PPI parameter(pores per inch)was maintained in two sizes:10 PPI with approximately 6 mm pore size and 20 PPI with approximately 3 mm pore size.The porosity parameter was changed by coating the cell walls with a wax-based slurry.Two 10 PPI foams were coated with a thicker wax layer to study the difference in wall thickness which can be obtained with the same PPI number.The foam structure is presented in Fig.2.The moulds for the research were made in?100 mm casting flasks,using Ransom&Randolph Argentum gypsum-based investment.The moulds were subjected to heat treatment during which the foams were burnt away to create a cavity:an exact copy of the pattern.The heat treatment was carried out at the following temperatures:

    ·dehydrating and dewaxing at temperatures rising from 150 to 370 °C,

    ·burning and firing at 730 °C for 2 h,

    ·cooling down to a pouring temperature of 550 °C.

    The AZ91 magnesium alloy was cast in 660–680 °C,in SF6protective gas atmosphere.The mould and metal temperatures during pouring were selected based on calculations followed by experimental trials.However,the process conditions and outcomes may vary depending on multiple factors,such as the shape and size of the gating system,the vacuum system,and the casting flask size,etc.

    Fig.1.Diagram illustrating the process of AZ91 foam investment casting.

    Fig.2.Macro-scale photograph of AZ91 magnesium alloy foam with 20 PPI.

    The temperature of the mould and of the liquid metal,as well as the vacuum value are the most important pouring parameters to ensure effective penetration of intricate mould cavity and simultaneously minimise the adverse reaction between the metal and the ceramic material.The process variables can be classified into three groups related to(1)the characteristics of the casting mould,(2)the pouring conditions and(3)the properties of the alloy.As the molten metal front penetrates through very narrow channels,it may cool quickly and crystallise prematurely.The key issue is the thermal diffusivity of the mass.With low thermal conductivity and average specific heat that characterize investment casting moulding materials,it can be assumed that with fast pouring the flowing metal heats only a thin layer of the mould cavity.Therefore,a sufficiently high-pressure gradient(high vacuum in the autoclave)must be provided so that the flowing metal loses only a small amount of heat and reaches the longest possible distance.The pressure,calculated from Eq.(1),should be exerted on the metal front in order to overcome the resistance of the mould-Pmould,resulting from the existing gas inside the cavity and the formation of a new metal–mould interface.Moreover,the meniscus-shaped metal front of radiusRwill be inhibited by the surface tension acting on it.

    Fig.3.AZ91 10 PPI foams:(a)non-coated,porosity 92%;(b)wax slurry-coated,porosity 85%.

    The generated vacuum can reduce the amount of gas in the cavity as long as the mould is permeable.To improve this parameter,fine graphite flakes were added to the commercial ceramic mass and later gasified during the heat treatment of the mould,making the mass more porous.After spiral casting tests with varying path width,it was possible to define appropriate temperature parameters.With a narrow path,the length of the flow was similar,and the influence of metal temperature was small.For the real mould,it was necessary to select the lowest possible temperature values so that,on the one hand,the metal completely filled the cavity,to avoid misruns,and on the other hand,to limit the reaction of the liquid metal with the mass.Fig.3 shows the structure of the AZ91 alloy foam with an open porosity of 92% or 85% both based on the original 10 PPI PUR foam size.

    During pouring,a small amount of air and gas penetrates through the walls of the mould placed in the autoclave.Accelerated oxidation causes an increase in the temperature,which may locally exceed 1200°C.Then one of the components of the moulding mass–calcium sulphate-can decompose according to formula(1)[19]:

    and oxygen is released,which intensifies the reaction and finally the mould is violently ruptured by large amounts of sulphur dioxide.Hence,it was necessary to develop a protective cover by feeding a gas mixture(SF6/CO2)and by controlling the temperature parameters very precisely both during the pouring and cooling of the casting.The interaction of the liquid and cooling magnesium with the mould mass should be limited to inhibit the reaction of magnesium with silicon oxide and the formation of Mg2Si as in formula(2)[20]:

    Such Mg2Si crystals were observed right next to the casting surface(see Fig.4).These inclusions triggered intergranular corrosion and accelerated the biodegradation process.Additionally,MgAl2O4and Mg2SiO4can form on the casting surface,as observed by Vyas and Sutaria[21]when AZ91 interacts with alumina or silica binder present in some shell moulds.In order to produce a good quality magnesium foam,the process conditions should allow for the formation of a continuous MgS layer by reaction with protective gas or compounds,and possibly a short contact of the liquid alloy with the ceramic mould.

    Measurements of temperature and pressure near the mould cavity show that the temperature decreases very slowly during solidification(dT/dt≈4.5 °C/min for the first minutes)and the applied low pressure forces metal to fill the entire volume in a fraction of a second.Therefore,the crucial factor affecting the chemical interaction between metal and ceramic is their contact time while the metal is still in the liquid state since this is when harmful reactions and deterioration of the casting surface can occur.The total energyQreleased from the solidifying metal is the sum of the latent heat of solidification and the superheat,as Eq.(2)shows:

    The thermo-physical properties of AZ91 alloy and mould materials with assigned symbols are shown in Table 1.The flux of this heat transferred through the interface metal/mould at timetcan be calculated from the Eq.(3)according to Rundman[22]:

    Table 1The thermo-physical properties of AZ91 alloys and the investment casting mould.

    Table 2Parameters for PEO foam treatment.

    using the integral of determined function in Eq.(4):

    and comparing the total heat dissipated through the casting area interface A(calculated according to the method proposed by Chen et al.[23]),the solidification timetscan be calculated for different temperatures of the poured metal and the preheated mould according to Eq.(5)[22]:

    Fig.4.Microstructure and EDS spectrum of the foam with Mg2Si formed during interaction with moulding material at high process temperature(620°C mould/740°C metal).

    Since two opposing requirements must be met in the casting process(solidification time long enough to allow the metal to fill the entire mould and short enough to prevent a metalmould material reaction),it is crucial to find the range of mould and metal temperatures sufficient to reach solidification time between 1 and 15 s(ideally 5 s).The calculated solidification times are presented in Fig.5,with mould temperatures ranging from 250 to 550 °C and metal pouring temperatures ranging from 600 °C to 720 °C.As can be seen,solidification time rises exponentially with increasing mould temperature,which suggests the most optimal temperature range of 500 °C–525 °C for the 10 PPI foam(square points on the plot)and 525–550°C for the 20 PPI foam(circle points on the plot).The effect of the pouring temperature on solidification time is relevant when the mould is preheated above 500 °C and is most visible in mould temperatures over 550°C.Below 500 °C,metal solidifies almost immediately irrespectively of temperature.At a mould temperature of 450 °C for 10 PPI foams,the solidification time allows(in ideal conditions)filling the mould;however,in 20 PPI foams,tsis shorter than 1 s.For mould temperatures over 525°C,the pouring temperature in 10 PPI foams has a significant impact on the solidification time and should be kept below 660 °C.The 20 PPI foams,due to their larger interface area,solidify faster and in mould temperatures up to 550 °C have shorttsregardless of the pouring temperature.Consequently,temperatures up to 720 °C can be used since it is the upper limit for AZ91 casting,above which oxidation and combustion danger increases[25].The separately calculated length of metal flow in the cylindrical mould channel using Fleming’s formula[26]indicates that a mould temperature in the range of 440–500 °C is required to fill a 6-cm foam-shaped cavity.Finally,the calculated process parameters allow the production of AZ91 foam blocks with maximum dimensions of 80×80×40 mm,with a homogeneousα-Mg-Mg17Al12structure as seen in Fig.6.

    2.2.Testing procedures

    Compression tests on uncoated foams were carried out on a universal testing machine(Tinius Olsen H25KT).The specimens had a cross-section of 35×23 mm(±2 mm)and a height of 40 mm(±2 mm).They were extracted from larger blocks and then weighed and measured.Their porosity,which was measured using Archimedes’principle,ranged from 83% to 92%.The compression tests were performed with a displacement range set to 10 mm/min,using a 10 kN load cell.

    The microstructures of coatings,casts and fractures were examined with a scanning electron microscope(SEM,Hitachi TM-3000)and analysed with an EDS detector to determine their shapes,sizes,thickness,composition and compression characteristics.

    Fig.5.Calculated solidification time of AZ91 foam casts poured into preheated ceramic moulds at the temperature of 600–720 °C.

    Fig.6.SEM micrographs of the α-Mg-Mg17Al12 structure of AZ91 foam.

    Fig.7.Stress-strain curves of AZ91 foams under compression tests:(a)10 PPI foams with thin wax coat(A1-A5,90–91% porosity)and thick wax coat(A6-A7,82–85% porosity),(b)20 PPI foams with thin wax coats.(For interpretation of the references to color in this figure,the reader is referred to the web version of this article.)

    The foam surface was treated by Plasma Electrolytic Oxidation(PEO)processing,using different treatment parameters(Table 2).A pulsed DC power source was used to treat the foams for 20 min under constant current.Different electrolytes with and without particles,and different current densities were tested to identify problems with foam processing and to improve the performance conditions.A set of foam specimen was cleaned prior to PEO treatment for 30 s in an aqueous solution of 150 g/L acetic acid.The foam was the anode in the process and a stainless steel tube cathode was integrated in the cooling system in an effort to maintain the temperature of the electrolyte at 20±2 °C.

    ICP-OES studies–analysis of the elemental composition of SBF elemental analysis in body solutions was performed using the technique of ICP-OES(Inductively Coupled Plasma Optical Emission Spectrometry).Under experimental conditions,the samples(in five replications)were immersed in 100 ml of SBF.

    The content of the elements entering the matrix of the magnesium alloy and the elements forming the corrosive solution during the exposure of the samples to SBF was analysed.Knowing the concentration of the alloying elements after exposure to SBF makes it possible to determine the biocompatibility of the magnesium alloy as an implant,while the rate of loss of calcium and phosphorus from the SBF solution leads to the assumption that a thin layer of apatite ceramics was formed on the surface of the magnesium alloy,which slowed down the corrosion process of the metallic material.

    The measurements were conducted in an SBF solution,which imitates the corrosiveness of the biological aqueous environment of the human body.The SBF was prepared according to the methodology established by Kokubo and Takadama[27](8.035 g NaCl,0.355 g NaHCO3,0.225 g KCl,0.231 g K2HPO4·3H2O,0.311 g MgCl2·6H2O,39 mL 1.0 mol/L HCl,0.292 g CaCl2,0.072 g Na2SO4,6.118 g(HOCH2)3CNH2and 0–5 ml of 1.0 mol/L HCl).

    3.Results and discussion

    3.1.Mechanical properties

    The analysis of the magnesium foam compression tests shows a correlation between the porosity of the foam and its mechanical properties.The foams from B series(with 20 PPI)had lower porosities and higher compression strength than the thin wax-coated foams from A series(10 PPI)that had higher porosities and bigger pores and struts.The thick-coated 10 PPI foams,described in Section 2,had similar porosities and mechanical properties as the 20 PPI foams.Fig.7 shows the stress-strain curves from both series,with a linear part,plateau and densification area.This kind of compression test curve is typical for metal foams–initially the stress increases linearly until the struts start to break.As the foam slowly collapses,the stress remains stable,creating plateau of the stress-strain curve.Eventually the crushed foam density increases and the material starts to behave like a monolyth.Due to magnesium’s microstructural and crystallographic properties it has brittle collapse mechanism,therefore the stress-strain curve lines are rigid.The properties of all the tested samples are summarized in Table 3.

    Table 3Properties of selected AZ91 foams test samples presented on Fig.7.

    The compression test results showed that all fabricated foams achieved compressive strengths no higher than 2.2 MPa and Young’s moduli below 80 MPa.These results vary greatly from those obtained by other methods.Posada et al.fabricated foams with Young’s moduli in the range of 0.8–1.8 GPa,while Rúa obtained foams with Young’s moduli of about 1.45 GPa[28,29].However,the porosity and morphology of their foams significantly differed from those produced in this research.They used the salt space holder method,withwhich Posada obtained foams with porosities ranging from 60 to 79%,while Rúa fabricated foams with porosities ranging from 36 to 53%.The lower mechanical properties of the foams in this study may be due to the very high porosity and very low foam strut thickness.The compression process was recorded on video and analysed frame-by frame to determine how the foam deformation processed.Fig.8 shows photographs of the foam compression process in different displacement phases.The red lines highlight the areas where deformations occurred.A frame-by-frame analysis shows that the first breakage occurs on the surface touching the compression plates and then new deformation lines appear on the thin struts adjacent to the areas strengthened by pattern modification.The collapse mechanism of these foams is slightly different from that of foams with lower porosities and with more closed cells,such as those developed by Bayani and Mirbahgerri[30].Due to thinner and more fragile struts,first fractures occur sooner and at the interfaces of both compression plates.Then,instead of a propagating crack near the compression plates,deformations appear in random weak spots within the foam material.A similar mechanism was also reported for Duocel foams by Zhou and Soboyejo[31].

    Fig.8.Magnesium foam at different cracking stages during a compression test and the stages’locations on a stress-strain curve.(For interpretation of the references to color in this figure,the reader is referred to the web version of this article.)

    As Fig.9 shows,both compressive strength and Young’s modulus drop significantly when porosity levels go over 90%because the metal weight is no longer capable of supporting the structure.Two samples of 10 PPI foam with lower porosities(82.6% and 85.7%)were fabricated in order to compare foams with similar densities and different pore sizes.Their Young’s modulus and compressive strengths were found to better than in 20 PPI foams of similar density.However,their compressive behaviour proved to be more unpredictable than that of 10 PPI foams with lower densities.Moreover,their stress-strain curves are more fluctuating and the structure crack points are clearly visible.Precise methods of controlling the density and uniformity of foam in the wax slurry coating process still need to be developed.At the current stage of technological development,as the wax content increases there is a smaller chance of obtaining foams with regular density and open pores.Thus,it is more beneficial to increase foam density by selecting ductile foams of smaller pore sizes than by thickening the wax layer in the pattern.Overall,the mechanical properties of the obtained foams are within the limits of properties of cancellous bone structures:Young’s modulus within 0.01–2 GPa and compressive strength within 0.2–80 MPa[32].

    Fig.9.Compression test results:Young’s modulus(a)and compressive strength(b)vs.porosity.

    The energy absorption properties of the foams were also calculated in order to determine which type of foam performs better in this regard.Specific energy absorption(SEA)was calculated using the following Eq.(6)[33]:

    Wheresfis crush length andmfis mass of the crushed material.The results of the calculation are shown in Fig.10.The SEA-porosity plot shows that foams with 20 PPI perform better at absorbing energy than 10 PPI foams.One possible explaination for this tendency is that the compression force in 20 PPI foams is spread over a higher amount of pores and strouts than in 10 PPI foams.The graph also indicates that,at least in the porosity range between 80 and 95%,increasing foam densitiy results in better energy absorption.The thickcoated 10 PPI foams of lower porosities(82.6 and 85.7%)performed worse than the 20 PPI foams with similar densities.This further supports the conclusion that minimizing pore size is a better way of increasing the density and mechanical properties of foam than increasing the mass of foam with a larger pore size.

    3.2.Fractography analysis

    In order to study the fracture behaviour of AZ91 foams,post-compression samples were analysed with an SEM microscope.Foams of such complex morphology undergo all kinds of deformations during compression tests.They not only become compressed,but also stretched,bent and sheared when the neighbouring struts get deformed.That is why analysing their fractographs is much more complicated than in the case of solid materials.The images presented in Fig.11 show that foam struts exhibit not only behaviours leading to simple compression fracture and fracture in the brittle mechanism caused by theα-Mg hexagonal structure[34]and/or relatively large grain size,but also leading to failure under bending and flexing in multiple directions(red arrows)in the ductile state,which is usually induced by the homogenous microstructure and the fine grain size.Another explanation for the two different types of collapse can be structural defects such as air bubbles or pre-existing cracks coming from shrinkage stresses in some of the struts which induce their brittle cracking.

    Analysis of the fractures on the struts shows that the foam has two kinds of fracture mechanisms:brittle and ductile.Fig.12 shows a strut with visible necking,but brittle cracks can be seen on the broken surface at a smaller scale.Similar fracture modes have been observed by other authors.Onck et al.studied Duocel aluminium foams[35];however,they obtained results with more ductile and less brittle collapse mechanisms,which can be explained by the better plasticity of aluminium compared to magnesium.The cracked surface of the magnesium alloy foam strut also has pre-existing voids and oxide impurities that initiated the failure.Such defects can be explained by the fact that during the casting process,molten AZ91 fills multiple channels at once,resulting in two liquid metal fronts meeting in one channel,with oxides and gas bubbles remaining at the connection point.Additionally,the casting parameters were adjusted to minimize the solidification time for finer grain size and reduce the formation of Mg2Si on the surface through the reaction between the metal and the mould material.Fast solidification creates a solid coating on metal and stops the vacuum from removing gas bubbles.Unfortunately,such problems are difficult to overcome in the casting process and can only be mitigated by improving casting conditions such as the vacuum environment and mould temperatures.

    Fig.10.Specific energy absorption(SEA)vs.foam porosity.

    Fig.11.SEM fractographs of compressed AZ91 foams with 20 PPI,showing both brittle strut breaking(green arrows)and ductile strut bending and/or flexing(red arrows).(For interpretation of the references to color in this figure legend,the reader is referred to the web version of this article.)

    Figs.12 and 13a show multiple small cracks at the surfaces of strut fractures,while Fig.13b shows a ruptured foam wall.Such cracks which appear on most of the deformed surfaces of the foam,as well as the ruptures in the struts and walls suggest that the collapse mechanism of the foam is brittle rather than ductile,which is a fairly common problem in magnesium and magnesium-based alloys that underlies the hexagonal crystallographic structure and the dislocation mechanisms of magnesium,which has been properly described by Wu and Curtin[34].Wall ruptures similar to those in Fig.13b were also observed in closed-cell aluminium foams by Onck et al[36].shortly before the final failure.Their foam,however,exhibited more brittle fracture behaviour,with metal debris visible on the SEM images,while AZ91 foam appears to fail in a“cleaner”manner,revealing the two remaining matching wall pieces.

    Fig.12.Broken strut tip of a 20 PPI AZ91 foam with visible necking and surface cracks.

    Fig.13.Brittle cracks at the tip of a broken strut(a)and a ruptured foam wall(b).

    Fig.14.Initial crack in the centre of a strut base(a)and a propagating crack at the connection of struts.

    Most of the observed cracks and fractures appear in areas with gas bubbles inclusions as defects,such as those shown in Figs.12b and 14.These cracks seem to be appearing far away from the weakest foam structure areas in the centre of the struts.Bigger gas bubbles initiate cracks obviously not only in struts,but also in stronger areas of the foam:at strut bases and strut connections.Therefore,compressive failure of the foam,while overwhelmingly occurring in the centre of individual struts,can be also initiated at strut connections,foam walls and strut bases,depending on the defects in the material structure.

    Fig.15.A bent strut of AZ91 10 PPI foam with cracks on the outer surface and wrinkling on the inner surface.

    It can be observed from Fig.15 that some of the struts show a more ductile deformation mechanism,with some of them bending almost 180° without fracture.However,many small cracks can be seen on both the outer and the inner bending surfaces.On the outer bending surface,major cracks propagate from defects,thus creating points for potential future strut fractures.Cracks of such shape on the outer bending surface were also observed by Zhou et al.[31]when they investigated aluminium foams.However,they observed more ductile failure modes as those cracks had less rigid edges than those on AZ91 foams because the hexagonal microstructure of magnesium causes more brittle collapse mechanisms.The inner bending surface of the strut,on the other hand,shows folds due to material build-up,initiating cracks and material layer detachment.

    3.3.Corrosive behaviour analysis

    Tests for the degradation of magnesium alloys are performed in various aquatic environments,for example,in solutions reflecting the chemical composition of body fluids.Most often,the corrosive medium is Hank’s or Ringer’s solution or simulated body fluid(SBF)[37–39].For magnesium alloys in the form of porous scaffolds,corrosion tests encounter a number of difficulties,such as those related to determining the size of the surface being tested[38].Therefore,the rate of degradation of the magnesium alloy(in the form of a scaffold)was determined by measuring changes in the concentration of the individual alloying elements entering the SBF.

    The aim of the research was to measure both the migration of the alloying elements to the SBF(Fig.16)and the components of SBF deposited on the surface of the metallic material(Fig.17)as a function of the exposure time.

    In aquatic environments,magnesium and its alloys react with water,resulting in the formation of Mg(OH)2and the release of hydrogen(H2).The reaction can be described by formula(3)[37]:

    The reaction in formula(3)causes changes in the concentration of individual elements in SBF(Figs.16 and 17).The changes in the concentration of Mg and Al(the main alloy components)in the SBF are shown in Fig.16a;the remaining alloy additions,the proportions of which in the alloy do not exceed 0.9% by weight are shown in Fig.16b.In SBF,the magnesium alloy(in the form of a scaffold)decomposes,which results in an increase in the concentration primarily of the main components of the Mg-Al alloy(Fig.16a).The release rate of magnesium ions was much faster than that of Al ions.After 216 h of exposure to SBF,the concentration of aluminium ions in the solution was almost 9 times lower than that of magnesium ions.

    The daily requirement of a healthy adult woman for magnesium is about 300–320 mg,and for men this dosage goes up to 400–420 mg.Thus,the average amount of magnesium released from the alloy into solution by the end of the experiment did not exceed these values.

    As a result of the dissolution of the melt and the evolution of H2,the pH value of the solution increased:after 216 h,the pH value was about 9.5–9.6,which is consistent with studies carried out by other researchers[40].At such a pH value,local alkalisation of the solution occurs,which promotes passivation of the surface of the magnesium alloy and,consequently,slows down the oxidation process of the metallic material.The observed slowdown in the migration of magnesium and aluminium to the SBF may have been the result of local passivation of the alloy surface(Fig.16a).

    The migration of Be,Ni,Cu,and Fe from the matrix to the SBF was negligible:after 216 h of exposure to SBF,their content in the solution was about 0.02–0.04 mg/dm3(Fig.17).Such a small concentration of these elements in the SBF does not exceed the acceptable daily requirement in an adult human;for example,for iron it is 1–3 mg,for copper 700 mg,and for nickel 0.3–0.5 mg.Both Zn and Si are necessary microelements for the proper functioning of the body.The daily requirement for zinc in an adult is a minimum of 5 mg,but the body should take it in higher doses,from 15 to 20 mg.In the case of silicon,it is assumed that the daily dosage for an adult should be 20–30 mg.The average daily consumption of silicon in the European and North American population is 20–50 mg,though it is higher in China and India(140–200 mg/day),where grains,fruits and vegetables make up the majority of the diet.Thus,the content of the elements Zn and Si released from the matrix of the magnesium alloy to the SBF(about 20 mg/dm3and about 5 mg/dm3,respectively,after 216 h of the alloy’s exposure to the solution)did not exceed the accepted doses for an adult human(Fig.17).The case was similar with Mn.

    Fig.16.Changes in the concentration of elements contained in the magnesium alloy after 216 h of exposure to SBF(a)for the main alloying elements,Mg and Al,and(b)for the elements whose proportion within the matrix does not exceed 1% by weight.

    Fig.17.Changes in the concentration of SBF elements during the exposure of the magnesium alloy to the solution.

    The changes in the concentration of ions comprising SBF were small and occurred mainly during the first 48 h of exposure(Fig.17).The lowered concentration of calcium and phosphorus indicates the adsorption of ions of these elements onto the surface of the scaffold.Data from the literature show that the presence of apatite ceramics is a desirable phase for corrosion protection of Mg alloys[41–43].In the following hours of exposure to the Mg alloy,the concentrations of Ca,P,K,and Na did not change significantly,which indicates the stability of SBF despite the increase in the pH of the solution.

    Fig.18.Phosphate-based PEO coating(a)and aluminate-based PEO coating with agglomerated CuO nanoparticles(b)deposited on AZ91 foams.

    Fig.19.Fracture of a single foam strut(bar)after PEO treatment in phosphate-based electrolyte(a)and a cross-section of the produced oxide layer with a typical outer porous and dense inner protective layer(b)20 min,2 A,foam as cast,electrolyte up to 44 °C.

    Fig.20.EDS analysis of PEO-coated AZ91 foam surface composition.

    3.4.Outlook PEO processing of foams

    Adding ceramic surface layers can affect the mechanic properties of the coatings on the one hand and,on the other hand,it can improve the degradation behaviour as well as provide opportunities for surface functionalisation e.g.adding antibacterial properties.However,the current work is just a first feasibility study to explore the conditions for applying such coatings by plasma electrolytic oxidation.

    The main intention was to screen a variety of different PEO parameters in order to identify a suitable range of parameters to uniformly cover the surface of the foams.The main challenge was to find a current density(actually a current value),since the real surface area is unknown as is the surface condition inside the foams.It turned out that the foam in its raw state needs a high current density to build up a dielectric layer in order to reach breakdown potential and start the discharges.In spite of the cooling of the electrolyte,the heat input was much higher and thus temperatures well beyond 40 °C were reached at the end of the 20 min treatments.At a final temperature of 60 °C,no stable PEO processing was possible anymore,with coating dissolution faster than its growth.Even at a final temperature of 40 °C,a typical PEO coating was produced(Fig.19b).Without cleaning the foam,it was not possible to further lower the current density.Therefore,a cleaning procedure was developed to remove possible surface contaminations from the surface based on an acidic cleaning step(a 30 s dip in aqueous 150 g/L acetic acid)and a rinse in deionised water.After cleaning,stable discharge conditions were obtained at much lower current densities and at low enough input energy levels that the cooling system was able to control the temperature at 20 °C,achieving conditions under which reproducible surface treatments were possible.Finally,the test was extended to different base electrolytes:besides phosphate also silicate and aluminate-based electrolytes were successfully used to apply uniform coatings on the foams.Fig.18a shows a typical surface of a phosphate coating and Fig.18b illustrates a typical aluminate coating with co-deposition of CuO nanoparticles(agglomerated).Latter was considered as a first attempt to see if the foams can be functionalised by particle additions.

    Fig.19 shows a foam element fracture with a protective oxide coating formed in the phosphate-based electrolyte,which includes an outer porous layer and a dense layer adjacent to the metal core.Typically,the coating contains elements from the electrolyte and the substrate,which are converted by the discharges into the ceramic-like coating Fig.20.shows the EDS analysis of the PEO coating composition,showing the expected coating forming elements(Mg,P and O).

    4.Conclusions

    ·Open-cell AZ91 Mg alloy foams were manufactured with an elaborated method based on investment casting,using wax-thickened PUR foam with two pore sizes(20 PPI and 10 PPI).20 PPI foams achieved porosity between 80.91 and 87%,while 10 PPI foams achieved porosity between

    90.55 and 91.82% in normal coated foams and between 82.55 and 85.74% in thick-coated foams.

    ·The thin-coated 10 PPI foams did not achieve mechanical properties sufficient for desired applications(Young’s modulus 11.65–23.8 MPa),while thick-coated foams performed well with a Young’s modulus of 36.5–77.5 MPa and a compressive strength of 1.15–2.20,although they turned out to be quite unpredictable and their fracture mechanism was more brittle.

    ·20 PPI foams performed satisfactorily in mechanical tests,with Young’s modulus ranging from 21 to 60 MPa and compressive strength ranging from 0.53 to 1.12 MPa,which fits the range of mechanical properties of cancellous bone structure,although further research on lower pore sizes and porosities should be conducted for a better understanding of the connection between foam structure and properties.

    ·Fractured foams SEM analysis showed that the foam collapsing mechanism consists mostly of brittle fracture and cracks.The fractures occur mostly in the middle of the struts,in areas with microstructural defects.Ductile deformations such as bending and necking were also observed.

    ·After the magnesium alloy was exposed to SBF,the concentration of elements entering the metal matrix did not exceed the acceptable daily requirement in an adult human.The slowdown in the release of the alloy elements may have been the result of both local passivation of the scaffold surface and the deposition of a thin layer of apatite ceramics on the implant.

    ·PEO coatings were applied successfully to add various ceramic type of surface layers to the foams.The dense inner layer in such coatings may provide good corrosion resistance,while the porous outer layer may be beneficial for bone implants application,both by providing a larger scaffold surface for hydroxyapatite growth and by improving adhesion.Particles can be used to add additional functionalities to the coatings e.g.antibacterial or photocatalytic properties.However,how the additional PEO coatings affect biocompatibility,mechanical integrity and degradation behaviour is a question of further studies.

    Conflic of interest

    The authors declare that they have no conflicts of interests.

    001.
    [6]C.Yang,J.Zhu,S.Cui,P.Chen,Z.Wu,Z.Ma,Z.Wu,Surface Coat.Technol.409(2021)126885,doi:10.1016/j.surfcoat.2021.126885.

    [7]A.G.Rakoch,E.P.Monakhova,Z.V.Khabibullina,M.Serdechnova,C.Blawert,M.L.Zheludkevich,A.A.Gladkova,J.Mag.Alloy.8(3)(2020)587–600,doi:10.1016/j.jma.2020.06.002.

    [8]G.Barati Darband,M.Aliofkhazraei,P.Hamghalam,N.Valizade,J.Mag.Alloy.5(1)(2017)74–132,doi:10.1016/j.jma.2017.02.004.

    [9]Q.Dong,Y.Li,H.Jiang,X.Zhou,H.Liu,M.Lu,J.Bai,J.Mag.Alloy.9(4)(2021)1329–1338,doi:10.1016/J.JMA.2020.05.022.

    [10]N.T.Kirkland,I.Kolbeinsson,T.Woodfield,G.J.Dias,M.P.Staiger,Mater.Sci.Eng.B Solid State Mater.Adv.Technol.176(2011)1666–1672 Elsevier,doi:10.1016/j.mseb.2011.04.006.

    [11]G.Jiang,G.He,Mater.Sci.Eng.C 43(2014)317–320,doi:10.1016/j.msec.2014.07.033.

    [12]Z.S.Seyedraoufi,S.Mirdamadi,J.Mech.Behav.Biomed.Mater.21(2013)1–8,doi:10.1016/j.jmbbm.2013.01.023.

    [13]D.Yang,Z.Hu,W.Chen,J.Lu,J.Chen,H.Wang,A.Ma,J.Manuf.Process.22(2016)290–296,doi:10.1016/J.JMAPRO.2016.04.003.

    [14]D.Yang,W.Chen,J.Lu,Z.Hu,Y.Feng,J.Chen,H.Wang,Metal Powder Rep.72(2)(2017)124–127,doi:10.1016/J.MPRP.2016.02.053.

    [15]D.Yang,S.Guo,J.Chen,C.Qiu,S.O.Agbedor,A.Ma,L.Wang,J.Alloy.Compd.857(2021)158112,doi:10.1016/J.JALLCOM.2020.158112.

    [16]H.J.Maier,S.Julmi,S.Behrens,C.Klose,A.K.Gartzke,P.Wriggers,A.Meyer-Lindenberg,JOM 72(5)(2020)1859–1869,doi:10.1007/s11837-020-04078-8.

    [17]Y.Yamada,K.Shimojima,Y.Sakaguchi,M.Mabuchi,M.Nakamura,T.Asahina,K.Higashi,Adv.Eng.Mater.2(4)(2000)184–187,doi:10.1002/(SICI)1527-2648(200004)2:4〈184::AID-ADEM184〉3.0.CO;2-W.

    [18]J.R.Davis,Metals Handbook,Desk Edition,2nd Ed.,ASM International,1998 Retrieved from https://app.knovel.com/web/toc.v/cid:kpMHDEE004/viewerType:toc/?toc-within=AZ91.

    [19]Z.Q.Yan,Z.A.Wang,X.F.Wang,H.Liu,J.R.Qiu,Trans.Nonferrous Met.Soc.China 25(2015)3490–3497,doi:10.1016/S1003-6326(15)63986-3.

    [20]X.Hu,D.Mayson,M.R.Barnett,J.Alloy.Compd.589(2014)485–490,doi:10.1016/J.JALLCOM.2013.11.092.

    [21]A.V.Vyas,M.P.Sutaria,Int.J.Met.20(4)(2020)139–144,doi:10.1007/s40962-020-00530-2.

    [22]K.B.Rundman,Metal Casting(Reference Book for MY4130),Dept.of Materials Science and Engineering,Michigan Tech.University,2000,pp.49–52.

    [23]J.Chen,X.Zhang,C.Li,X.Zhang,Y.Ren,J.He,J.Chen,Int.J.Photoenergy(2020)2020,doi:10.1155/2020/2478579.

    [24]Matweb.Plaster;Molded,Dry.Retrieved April 30,2021,from http://www.matweb.com/search/DataSheet.aspx?MatGUID=0e684bc25a1642d0a90aabe41f59b917

    [25]Q.Le,Z.Zhang,J.Cui,S.Chang,in:Materials Science Forum,610–613,Trans Tech Publications Ltd,2009,pp.754–757,doi:10.4028/www.scientific.net/MSF.610-613.754.

    [26]K.R.Ravi,R.M.Pillai,K.R.Amaranathan,B.C.Pai,M.Chakraborty,J.Alloy.Compd.(2008)Elsevier,doi:10.1016/j.jallcom.2007.02.038.

    [27]T.Kokubo,H.Takadama,Biomaterials 27(15)(2006)2907–2915,doi:10.1016/J.BIOMATERIALS.2006.01.017.

    [28]V.M.Posada,J.Ramírez,J.P.Allain,A.R.Shetty,P.Fernández-Morales,J.Mater.Eng.Perform.29(1)(2020)681–690,doi:10.1007/s11665-020-04566-7.

    [29]J.M.Rúa,A.A.Zuleta,J.Ramírez,P Fernández-Morales,Surface Coat.Technol.360(2019)213–221,doi:10.1016/j.surfcoat.2018.12.106.

    [30]H.Bayani,S.M.H.Mirbagheri,Mater.Charact.113(2016)168–179,doi:10.1016/j.matchar.2016.01.017.

    [31]J.Zhou,W.O.Soboyejo,Mater.Sci.Eng.A 369(1–2)(2004)23–35,doi:10.1016/j.msea.2003.08.009.

    [32]M.Yazdimamaghani,M.Razavi,D.Vashaee,K.Moharamzadeh,A.R.Boccaccini,L.Tayebi,Mat.Sci.Eng.C(2017)Elsevier Ltd,doi:10.1016/j.msec.2016.11.027.

    [33]M.Stamenovi′c,S.Puti′c,M.Zrili′c,L.J.Milovi′c,J.Pavlovi′c-Krsti′c,Metalurgija 50(3)(2011)197–200.

    [34]Z.Wu,W.A.Curtin,Nature 526(7571)(2015)62–67,doi:10.1038/nature15364.

    [35]P.R.Onck,R.van Merkerk,J.T.M.De Hosson,I.Schmidt,Adv.Eng.Mater.6(6)(2004)429–431,doi:10.1002/adem.200405156.

    [36]P.R.Onck,R.van Merkerk,A.Raaijmakers,J.T.M.De Hosson,J.Mater.Sci.40(22)(2005)5821–5828,doi:10.1007/s10853-005-4996-7.

    [37]N.I.Zainal Abidin,B.Rolfe,H.Owen,J.Malisano,D.Martin,J.Hofstetter,A.Atrens,Corros.Sci.75(2013)354–366,doi:10.1016/J.CORSCI.2013.06.019.

    [38]M.H.Kang,T.S.Jang,S.W.Kim,H.S.Park,J.Song,H.E.Kim,H.D.Jung,Mater.Sci.Eng.C 62(2016)634–642,doi:10.1016/J.MSEC.2016.01.085.

    [39]N.I.Zainal Abidin,A.D.Atrens,D.Martin,A.Atrens,Corros.Sci.53(11)(2011)3542–3556,doi:10.1016/J.CORSCI.2011.06.030.

    [40]A.Atrens,G.L.Song,M.Liu,Z.Shi,F.Cao,M.S.Dargusch,Adv.Eng.Mater.17(4)(2015)400–453,doi:10.1002/ADEM.201400434.

    [41]X.B.Chen,N.Birbilis,T.B.Abbott,Corros.Sci.55(2012)226–232,doi:10.1016/J.CORSCI.2011.10.022.

    [42]X.B.Chen,N.Birbilis,T.B.Abbott,Corros.Sci.53(6)(2011)2263–2268,doi:10.1016/J.CORSCI.2011.03.008.

    [43]S.Hiromoto,A.Yamamoto,Electrochim.Acta 54(27)(2009)7085–7093,doi:10.1016/J.ELECTACTA.2009.07.033.

    后天国语完整版免费观看| 青草久久国产| 亚洲欧美日韩另类电影网站| xxx96com| 国产一区在线观看成人免费| 一级片免费观看大全| 中文字幕精品免费在线观看视频| 日韩视频一区二区在线观看| 人妻丰满熟妇av一区二区三区 | 久久热在线av| 男女下面插进去视频免费观看| 村上凉子中文字幕在线| 欧美日韩精品网址| 制服人妻中文乱码| 免费在线观看黄色视频的| 日本a在线网址| 亚洲精品一二三| 法律面前人人平等表现在哪些方面| 黄片小视频在线播放| 黑人巨大精品欧美一区二区mp4| 久久草成人影院| 亚洲欧美一区二区三区黑人| 日韩欧美一区二区三区在线观看 | 亚洲全国av大片| videos熟女内射| 亚洲精品一二三| 人妻一区二区av| 欧美成人午夜精品| 中文字幕av电影在线播放| 亚洲欧美激情综合另类| 一夜夜www| 国产一卡二卡三卡精品| 激情视频va一区二区三区| 最近最新中文字幕大全电影3 | 亚洲国产看品久久| 麻豆乱淫一区二区| 亚洲一区二区三区不卡视频| 免费女性裸体啪啪无遮挡网站| 亚洲,欧美精品.| 一级a爱片免费观看的视频| 大型黄色视频在线免费观看| 精品久久久久久久久久免费视频 | 国产亚洲精品第一综合不卡| 黄色毛片三级朝国网站| 丝袜美腿诱惑在线| 欧美精品高潮呻吟av久久| 亚洲精品一卡2卡三卡4卡5卡| 国产在线精品亚洲第一网站| 老司机午夜十八禁免费视频| 天堂中文最新版在线下载| 在线观看免费视频网站a站| 亚洲午夜精品一区,二区,三区| av福利片在线| 精品乱码久久久久久99久播| 国产成人系列免费观看| aaaaa片日本免费| 男人的好看免费观看在线视频 | 十分钟在线观看高清视频www| 又大又爽又粗| 亚洲七黄色美女视频| 久久久水蜜桃国产精品网| 一a级毛片在线观看| 欧美 日韩 精品 国产| 亚洲精品一卡2卡三卡4卡5卡| 一区二区三区国产精品乱码| 高清av免费在线| aaaaa片日本免费| 制服诱惑二区| а√天堂www在线а√下载 | 亚洲综合色网址| 亚洲一卡2卡3卡4卡5卡精品中文| 色94色欧美一区二区| 18禁国产床啪视频网站| 国产精品久久久av美女十八| 久久久久久久国产电影| 国产一区二区三区视频了| 麻豆成人av在线观看| av电影中文网址| 亚洲国产欧美网| 精品国内亚洲2022精品成人 | 亚洲一区中文字幕在线| 国精品久久久久久国模美| 大码成人一级视频| 日本a在线网址| 欧美激情极品国产一区二区三区| 国产xxxxx性猛交| 国产精品影院久久| 精品福利观看| 精品高清国产在线一区| 午夜免费鲁丝| 人人妻人人添人人爽欧美一区卜| 熟女少妇亚洲综合色aaa.| 波多野结衣一区麻豆| 母亲3免费完整高清在线观看| 国产成+人综合+亚洲专区| 久99久视频精品免费| 视频在线观看一区二区三区| 国产av精品麻豆| 欧美日本中文国产一区发布| 久久久国产欧美日韩av| 悠悠久久av| 水蜜桃什么品种好| 精品久久久精品久久久| 国产亚洲欧美精品永久| 成人国语在线视频| 后天国语完整版免费观看| 老鸭窝网址在线观看| 精品国产一区二区三区久久久樱花| 国产欧美日韩精品亚洲av| 亚洲国产精品sss在线观看 | 老司机午夜十八禁免费视频| 首页视频小说图片口味搜索| 精品午夜福利视频在线观看一区| 最新在线观看一区二区三区| 91麻豆av在线| 黑人欧美特级aaaaaa片| 国产成人欧美在线观看 | 欧美性长视频在线观看| 亚洲精品av麻豆狂野| 丰满人妻熟妇乱又伦精品不卡| e午夜精品久久久久久久| 中文欧美无线码| 麻豆av在线久日| 69av精品久久久久久| 国产精品自产拍在线观看55亚洲 | 操美女的视频在线观看| 欧美乱妇无乱码| 国产精品一区二区精品视频观看| 一级片'在线观看视频| 亚洲人成电影观看| av网站免费在线观看视频| 嫁个100分男人电影在线观看| 国产有黄有色有爽视频| 精品视频人人做人人爽| 午夜精品国产一区二区电影| 欧美不卡视频在线免费观看 | 欧美 亚洲 国产 日韩一| 午夜精品在线福利| 久久狼人影院| 久久中文看片网| 亚洲av美国av| 婷婷精品国产亚洲av在线 | 啦啦啦 在线观看视频| 欧美+亚洲+日韩+国产| 国产精品亚洲一级av第二区| 精品国产超薄肉色丝袜足j| 建设人人有责人人尽责人人享有的| 下体分泌物呈黄色| 中文亚洲av片在线观看爽 | 国产精品久久久久久人妻精品电影| 99国产精品免费福利视频| 久久天堂一区二区三区四区| 国产精品香港三级国产av潘金莲| av在线播放免费不卡| 国产成人系列免费观看| 丝瓜视频免费看黄片| 又紧又爽又黄一区二区| 亚洲精品一卡2卡三卡4卡5卡| a级毛片黄视频| 欧美 亚洲 国产 日韩一| 国产成+人综合+亚洲专区| 美女视频免费永久观看网站| 国产一区在线观看成人免费| 午夜福利在线免费观看网站| 久久久久久久久久久久大奶| 别揉我奶头~嗯~啊~动态视频| 欧美日韩福利视频一区二区| 别揉我奶头~嗯~啊~动态视频| av超薄肉色丝袜交足视频| 成年人黄色毛片网站| 午夜精品久久久久久毛片777| 国产成人免费观看mmmm| 夫妻午夜视频| 看黄色毛片网站| 一级毛片精品| 国产亚洲精品一区二区www | 国产高清激情床上av| 人人妻,人人澡人人爽秒播| ponron亚洲| 欧美+亚洲+日韩+国产| 伊人久久大香线蕉亚洲五| 国产精品综合久久久久久久免费 | 国产一区在线观看成人免费| 国产一区在线观看成人免费| 精品亚洲成国产av| 午夜福利欧美成人| 天天躁狠狠躁夜夜躁狠狠躁| 国产免费av片在线观看野外av| 亚洲男人天堂网一区| 99国产综合亚洲精品| 久久久久久久精品吃奶| 色精品久久人妻99蜜桃| 黄片大片在线免费观看| 性少妇av在线| 久久久国产成人精品二区 | 久久这里只有精品19| 欧美国产精品一级二级三级| 久久 成人 亚洲| 女性被躁到高潮视频| 97人妻天天添夜夜摸| 老熟女久久久| 十八禁网站免费在线| 满18在线观看网站| 久久99一区二区三区| 19禁男女啪啪无遮挡网站| 亚洲中文av在线| 中文字幕人妻丝袜制服| 久久九九热精品免费| 精品熟女少妇八av免费久了| 欧美另类亚洲清纯唯美| 看片在线看免费视频| 午夜激情av网站| 女人被躁到高潮嗷嗷叫费观| 国产91精品成人一区二区三区| 日本a在线网址| av网站免费在线观看视频| 波多野结衣一区麻豆| 最新的欧美精品一区二区| 91国产中文字幕| 国产区一区二久久| 日韩欧美在线二视频 | 极品少妇高潮喷水抽搐| av欧美777| 国产免费现黄频在线看| 免费在线观看黄色视频的| 91精品国产国语对白视频| 超碰97精品在线观看| 欧美精品高潮呻吟av久久| 99国产精品免费福利视频| 亚洲国产精品一区二区三区在线| 国产av又大| 可以免费在线观看a视频的电影网站| 欧美精品av麻豆av| 丝袜美足系列| 天堂俺去俺来也www色官网| 国产精品久久久av美女十八| 高清视频免费观看一区二区| 精品免费久久久久久久清纯 | 啦啦啦视频在线资源免费观看| 亚洲专区字幕在线| 婷婷成人精品国产| 日本欧美视频一区| 捣出白浆h1v1| 天天操日日干夜夜撸| 精品熟女少妇八av免费久了| 欧美国产精品一级二级三级| 久久精品亚洲精品国产色婷小说| 久久久精品区二区三区| 亚洲国产毛片av蜜桃av| 亚洲成av片中文字幕在线观看| 狠狠婷婷综合久久久久久88av| 嫁个100分男人电影在线观看| 老司机福利观看| xxx96com| av电影中文网址| 精品一区二区三区视频在线观看免费 | 久久久久久久国产电影| 日韩欧美一区二区三区在线观看 | 精品熟女少妇八av免费久了| www.精华液| 咕卡用的链子| 国产一区二区三区视频了| av欧美777| 日韩欧美免费精品| 成人黄色视频免费在线看| 777米奇影视久久| 亚洲中文日韩欧美视频| 日韩中文字幕欧美一区二区| 天堂俺去俺来也www色官网| 巨乳人妻的诱惑在线观看| 国产男女超爽视频在线观看| 99香蕉大伊视频| 正在播放国产对白刺激| 久久精品亚洲熟妇少妇任你| videos熟女内射| 久久香蕉国产精品| 亚洲五月天丁香| 夜夜夜夜夜久久久久| 国产精品电影一区二区三区 | 老司机影院毛片| 黄片大片在线免费观看| 69精品国产乱码久久久| 校园春色视频在线观看| 成人18禁高潮啪啪吃奶动态图| 丝袜美足系列| 日本黄色视频三级网站网址 | 一级作爱视频免费观看| 老司机亚洲免费影院| 美女国产高潮福利片在线看| 国产一区二区三区视频了| 少妇被粗大的猛进出69影院| 色精品久久人妻99蜜桃| 伦理电影免费视频| 天堂俺去俺来也www色官网| 国产不卡一卡二| 亚洲九九香蕉| 精品午夜福利视频在线观看一区| 黑人欧美特级aaaaaa片| 高清欧美精品videossex| 久久国产乱子伦精品免费另类| av有码第一页| 一区在线观看完整版| 国产精品欧美亚洲77777| 脱女人内裤的视频| 曰老女人黄片| 在线观看一区二区三区激情| 黄色视频,在线免费观看| 男人的好看免费观看在线视频 | 人妻一区二区av| 色精品久久人妻99蜜桃| 热99re8久久精品国产| 亚洲精品久久午夜乱码| 麻豆成人av在线观看| 在线视频色国产色| 岛国毛片在线播放| 久久久久久久精品吃奶| 色婷婷av一区二区三区视频| 人人妻人人添人人爽欧美一区卜| 欧美乱色亚洲激情| 三上悠亚av全集在线观看| 高清视频免费观看一区二区| av超薄肉色丝袜交足视频| 91麻豆av在线| 久久精品亚洲熟妇少妇任你| 极品少妇高潮喷水抽搐| 美女高潮到喷水免费观看| 18禁裸乳无遮挡免费网站照片 | 日本黄色日本黄色录像| a级毛片在线看网站| 最近最新中文字幕大全电影3 | 人妻丰满熟妇av一区二区三区 | 一进一出好大好爽视频| 亚洲精华国产精华精| 99久久综合精品五月天人人| 亚洲欧美日韩另类电影网站| videos熟女内射| 成年动漫av网址| a级片在线免费高清观看视频| 人成视频在线观看免费观看| 久久久久久久久免费视频了| 欧美精品亚洲一区二区| 好男人电影高清在线观看| 男女床上黄色一级片免费看| tocl精华| 淫妇啪啪啪对白视频| 国产亚洲精品一区二区www | 男人的好看免费观看在线视频 | 国产精品国产av在线观看| 精品福利永久在线观看| 亚洲国产中文字幕在线视频| 亚洲精品国产区一区二| av有码第一页| 国产精品一区二区在线观看99| 成人黄色视频免费在线看| 国产片内射在线| 在线十欧美十亚洲十日本专区| 国产精品久久久久成人av| 欧美日韩精品网址| 亚洲全国av大片| 久久天堂一区二区三区四区| 国产av精品麻豆| 男人的好看免费观看在线视频 | 久久国产精品男人的天堂亚洲| 国内毛片毛片毛片毛片毛片| 别揉我奶头~嗯~啊~动态视频| 国产精品一区二区免费欧美| 老熟妇仑乱视频hdxx| 中文字幕人妻丝袜一区二区| 一级,二级,三级黄色视频| 久久影院123| 悠悠久久av| 亚洲精品国产精品久久久不卡| 一级,二级,三级黄色视频| 91大片在线观看| 12—13女人毛片做爰片一| 女人久久www免费人成看片| 久久久久视频综合| 韩国av一区二区三区四区| 日本五十路高清| 久久精品人人爽人人爽视色| 国产成人av教育| 一级毛片高清免费大全| 久久精品aⅴ一区二区三区四区| 久久精品91无色码中文字幕| 免费观看精品视频网站| 久久人人97超碰香蕉20202| 黄色视频不卡| 超色免费av| 色综合欧美亚洲国产小说| 曰老女人黄片| 日韩精品免费视频一区二区三区| 一夜夜www| 精品午夜福利视频在线观看一区| 亚洲精品一卡2卡三卡4卡5卡| 女同久久另类99精品国产91| 老汉色av国产亚洲站长工具| 欧美另类亚洲清纯唯美| 黄色 视频免费看| 成熟少妇高潮喷水视频| 曰老女人黄片| 成年动漫av网址| 国产精品成人在线| 啦啦啦视频在线资源免费观看| 国产亚洲精品第一综合不卡| cao死你这个sao货| 久久热在线av| 午夜福利视频在线观看免费| a级毛片在线看网站| 久久影院123| 好男人电影高清在线观看| 国产成人精品无人区| 国产片内射在线| 三上悠亚av全集在线观看| 俄罗斯特黄特色一大片| www.熟女人妻精品国产| 日本五十路高清| 午夜精品在线福利| 欧美日韩国产mv在线观看视频| 久久亚洲精品不卡| 波多野结衣一区麻豆| 精品福利观看| 日本黄色日本黄色录像| 精品久久蜜臀av无| 久久国产精品影院| 天堂动漫精品| 老司机福利观看| 欧美日韩av久久| 在线免费观看的www视频| 亚洲熟女精品中文字幕| 91九色精品人成在线观看| 国产淫语在线视频| 制服诱惑二区| 两性午夜刺激爽爽歪歪视频在线观看 | 人妻 亚洲 视频| 大香蕉久久成人网| 女人爽到高潮嗷嗷叫在线视频| 另类亚洲欧美激情| 午夜老司机福利片| 国产精品一区二区精品视频观看| 国产亚洲欧美在线一区二区| 国产激情久久老熟女| 丝袜在线中文字幕| 少妇裸体淫交视频免费看高清 | 好男人电影高清在线观看| 亚洲va日本ⅴa欧美va伊人久久| 国产精品电影一区二区三区 | 日本wwww免费看| 久久久久国产精品人妻aⅴ院 | 国产激情久久老熟女| 欧美 日韩 精品 国产| 免费女性裸体啪啪无遮挡网站| 久久ye,这里只有精品| 伊人久久大香线蕉亚洲五| 久久99一区二区三区| 两个人看的免费小视频| 丝瓜视频免费看黄片| 国产成人精品无人区| 我的亚洲天堂| 波多野结衣av一区二区av| 视频在线观看一区二区三区| 窝窝影院91人妻| 天天躁狠狠躁夜夜躁狠狠躁| 18在线观看网站| 亚洲午夜理论影院| 国产又色又爽无遮挡免费看| 香蕉国产在线看| 欧美日韩国产mv在线观看视频| 国产av一区二区精品久久| 国产欧美日韩综合在线一区二区| 无限看片的www在线观看| 一进一出好大好爽视频| 18禁黄网站禁片午夜丰满| 色老头精品视频在线观看| 天堂动漫精品| 久久久久视频综合| 亚洲精品国产区一区二| 午夜亚洲福利在线播放| 9色porny在线观看| 波多野结衣av一区二区av| 欧美精品一区二区免费开放| 国产成+人综合+亚洲专区| 欧美激情 高清一区二区三区| e午夜精品久久久久久久| 国产亚洲精品久久久久久毛片 | 国产在线精品亚洲第一网站| 午夜福利欧美成人| 亚洲免费av在线视频| 精品电影一区二区在线| a级毛片在线看网站| 91九色精品人成在线观看| 巨乳人妻的诱惑在线观看| 国产极品粉嫩免费观看在线| 久久久久久免费高清国产稀缺| 久久久久久久久久久久大奶| 亚洲va日本ⅴa欧美va伊人久久| 女人久久www免费人成看片| 成人影院久久| 国产成人系列免费观看| 久久久精品国产亚洲av高清涩受| 精品国产超薄肉色丝袜足j| 视频在线观看一区二区三区| 国产亚洲精品一区二区www | 欧美国产精品一级二级三级| 久久国产精品男人的天堂亚洲| 99香蕉大伊视频| 侵犯人妻中文字幕一二三四区| 香蕉丝袜av| 在线国产一区二区在线| 高清视频免费观看一区二区| 久久久国产一区二区| 黑人巨大精品欧美一区二区蜜桃| 黄片大片在线免费观看| 亚洲午夜精品一区,二区,三区| 一夜夜www| 欧美乱码精品一区二区三区| 999精品在线视频| 久久天躁狠狠躁夜夜2o2o| 亚洲va日本ⅴa欧美va伊人久久| 色94色欧美一区二区| 成人精品一区二区免费| 国产一区二区三区综合在线观看| av天堂久久9| 亚洲国产看品久久| 成年女人毛片免费观看观看9 | 18禁国产床啪视频网站| 99久久综合精品五月天人人| 免费黄频网站在线观看国产| 亚洲人成电影免费在线| 亚洲中文字幕日韩| 一级,二级,三级黄色视频| 欧美不卡视频在线免费观看 | 婷婷丁香在线五月| 女人高潮潮喷娇喘18禁视频| 国产欧美日韩一区二区精品| 久久久精品区二区三区| 这个男人来自地球电影免费观看| 亚洲国产精品合色在线| 在线看a的网站| 久久精品亚洲熟妇少妇任你| 免费女性裸体啪啪无遮挡网站| 黑人操中国人逼视频| 亚洲精品国产精品久久久不卡| 人人澡人人妻人| 久久中文看片网| 最新美女视频免费是黄的| 亚洲第一青青草原| 正在播放国产对白刺激| 91麻豆精品激情在线观看国产 | 国产精品亚洲av一区麻豆| 久久人人97超碰香蕉20202| 青草久久国产| 亚洲五月色婷婷综合| 夜夜爽天天搞| 欧美 亚洲 国产 日韩一| 亚洲av电影在线进入| 99国产精品99久久久久| 十八禁网站免费在线| 一级毛片精品| 99国产精品免费福利视频| 9色porny在线观看| 亚洲第一青青草原| 在线播放国产精品三级| 午夜福利一区二区在线看| 亚洲精品国产一区二区精华液| 国产一区有黄有色的免费视频| 最新在线观看一区二区三区| 丝瓜视频免费看黄片| 一进一出抽搐动态| 国产欧美日韩一区二区三区在线| 麻豆国产av国片精品| ponron亚洲| 国产精品秋霞免费鲁丝片| 天天躁狠狠躁夜夜躁狠狠躁| 欧美日韩亚洲国产一区二区在线观看 | 国产精品国产高清国产av | 免费一级毛片在线播放高清视频 | 国产精品永久免费网站| 国产一卡二卡三卡精品| 亚洲欧美日韩高清在线视频| 亚洲av电影在线进入| 久久精品国产综合久久久| 亚洲九九香蕉| 色播在线永久视频| videosex国产| 热re99久久国产66热| 久久久国产精品麻豆| 看片在线看免费视频| 黄色视频不卡| 久久国产亚洲av麻豆专区| 啦啦啦 在线观看视频| 看免费av毛片| 老汉色av国产亚洲站长工具| 人人妻人人添人人爽欧美一区卜| 午夜福利,免费看| 欧美成人免费av一区二区三区 | 久久中文看片网| 最新美女视频免费是黄的| 亚洲视频免费观看视频| 国产精品欧美亚洲77777| 亚洲片人在线观看| 国产成人啪精品午夜网站| 久热这里只有精品99| 高清在线国产一区| 国产欧美日韩一区二区三| 正在播放国产对白刺激| 亚洲精品一二三| 9色porny在线观看| 国产精品二区激情视频| 人人澡人人妻人| 国产一区二区三区综合在线观看| 亚洲精品av麻豆狂野| 欧美日韩中文字幕国产精品一区二区三区 | 一级片'在线观看视频| 啦啦啦免费观看视频1| 熟女少妇亚洲综合色aaa.|