    Effect of heat treatment on the microstructure and mechanical properties of AZ80M magnesium alloy fabricated by wire arc additive manufacturing

    2022-09-26 03:08:26YngyngGuoGofengQunMertCelikinLingoRenYuhngZhnLinglingFnHouhongPn
    Journal of Magnesium and Alloys 2022年7期

    Yngyng Guo,Gofeng Qun,*,Mert Celikin,Lingo Ren,Yuhng Zhn,Lingling Fn,Houhong Pn,*

    a Key Laboratory of Advanced Technologies of Materials,Ministry of Education,School of Materials Science and Engineering,Southwest Jiaotong University,Chengdu,Sichuan 610031,PR China

    b School of Mechanical and Materials Engineering,University College Dublin,Belfield,Dublin 4,Ireland

    cCenter for Advancing Materials Performance from the Nanoscale,State Key Laboratory for Mechanical Behavior of Materials,Xi’an Jiaotong University,Xi’an 710049,PR China

    Abstract To maximize the benefits of wire arc additive manufacturing(WAAM)processes,the effect of post-deposition heat treatment on the microstructure and mechanical properties of WAAM AZ80M magnesium(Mg)alloy was investigated.Three different heat treatment procedures(T4,T5 and T6)were performed.According to the results,after T4 heat treatment,the microsegregation of alloying elements was improved with the eutectic structure dissolved.Samples after T5 heat treatment inherited the net-like distribution of secondary phases similar to the as-deposited sample,where the eutectic structure covering the interdendritic regions and the β-phase precipitated around the eutectic structure.After T6 heat treatment,the tiny β-phases re-precipitated from the matrix and distributed in inner and outer of the grains.The hardness distribution of the samples went through T4 and T6 heat treatment was more uniform in comparison to that of T5 heat treated samples.The tensile test showed that the T6 heat treatment improved the strength and ductility,and the anisotropy between horizontal and vertical can be eliminated.Moreover,T4 treated samples exhibited highest ductility.

    Keywords:Wire arc additive manufacturing;AZ80M magnesium alloy;Heat treatment;Microstructure;Mechanical properties.

    1.Introduction

    Being the lightest structural metal(1.74 g/cm3),magnesium(Mg)alloys have the characteristics of high specific strength,excellent damping performance and electromagnetic shielding performance,and have great potential for weight reduction and energy saving.However,aluminum(Al)alloys with higher density(2.7 g/cm3)are still the preferred choice for lightweight design in the fields of aircraft,automobile and high-speed trains even though Mg alloys have a wide range of application prospects[1].One of the main factors limiting the use of Mg alloys is the poor formability due to hexagonal close-packed(HCP)crystal structure and strong heat dissipation tendency,making the traditional manufacturing processes like forging and rolling at room temperature unfeasible.Additionally,Mg casting process is accompanied by defects such as coarse grains,shrinkage cavity and slag inclusion,which makes the performance of the formed parts difficult to meet the requirements[2,3].Therefore,there is an urgent need for new methods to manufacture integral Mg alloy parts.

    Wire arc additive manufacturing(WAAM)is an innovative technology developed in the past few years,for which manufacturing industry has shown great interest.WAAM used electric arc as the heat source and metallic wire as the feed material,the energy and the material usage efficiencies of WAAM were much higher(up to 10 kg/h deposition rates can be achieved)than the other additive manufacturing processes such as Selective Laser Melting(SLM)[4].More valuably,the WAAM process can be operated in open air as localized inert gas shielding is only required around the slowly moving fusion zone,which means that the WAAM can be used to fabricate large size structures up to several meters in dimension without the limitation of equipment workbench[5].WAAM have already been applied to various metallic materials,such as titanium(Ti)[6–8],steel[9,10],aluminum(Al)[11–13]and nickel(Ni)[14,15]alloys and their intermetallic composites(IMC)[5,16,17].A few studies on the WAAM of Mg alloys have been reported in recent years.WAAM was preliminarily applied to fabricate AZ31 Mg alloy by Guo et al.[18]and it was determined that the use of pulsed frequency resulted in the change of weld pool oscillations and cooling rate,further led to the change of the grain size,orientation,as well as the tensile properties.WAAM based on cold metal transfer(CMT)process of AZ31 Mg alloy proposed has shown non-homogenous microstructure,hence tensile properties present anisotropic characteristics because of the epitaxial columnar dendritic growth along the building direction[19].

    Since the high heat input and rapid solidification nature of the WAAM deposition process,the materials fabricated exhibit a layered structure and the formation of non-equilibrium phases significantly restricts the service performance of the components.The layer-by-layer deposition resulted in serious thermal accumulation,and the arc energy not only caused partial melting and heat treatment of the previously deposited layers but also extended a non-isothermal heat treatment effect up to three to four layers below the deposited bead[20].This can significantly influence the microstructure and the mechanical properties of the WAAM materials,leading to anisotropy.Tensile anisotropy in the horizontal and vertical directions of the WAAM components were reported when fabricated 5A06 Al[11],316L SS[9]and AZ80M Mg alloys[21].

    Recent studies focused on the ways to avoid or decrease anisotropy in WAAM materials as it is crucial for widening the application range.To optimize the mechanical properties,Ma et al.[16]carried out post-deposition heat treatments which resulted in more uniform microstructure and minimized tensile anisotropy in WAAMγ-TiAl IMC.Gu et al.[12,22]applied a hybrid technique of inter-layer rolling and heat treatment to WAAM Al alloys,which resulted in improved microstructural homogeneity and weakened anisotropy of mechanical properties.Fu at al.[10]developed an hybrid deposition and micro-rolling(HDMR)process to eliminate the anisotropy of the WAAM bainitic steel upon the multi-layer and multi-pass deposition.However,up to now,there is no report on the post-deposition heat treatment of WAAM Mg alloys.AZ80 is widely used because of its good strength,corrosion resistance and plastic processing properties.Moreover,microalloying has been reported to be beneficial for improved mechanical and thermal performance of Mg-Al-based systems.Y can not only refine the grains in the Mg alloys but also improve the thermal stability of the Mg alloys through forming a new stable secondary phase Al2Y in Mg-Al alloys[23];the addition of trace Ca can improve the ignition pointand high temperature oxidation resistance of Mg alloy and reduce the burning loss of elements in the melting process[24].In this study,customized AZ80M(AZ80 with Y+Ca microalloying)was chosen as the raw material.The objective was to understand the effect of various heat treatments(T4,T5 and T6)on the microstructural evolution and mechanical properties of WAAM AZ80M Mg alloy,which could lay the foundation for the application of WAAM Mg alloys.

    2.Experimental procedure

    Extruded substrate dimensions were 8 mm thickness,80 mm width and 300 mm length.The same chemical composition AZ80M wire with a diameter of 1.6 mm was used as filler metal.The chemical composition details of AZ80M Mg alloy are listed in Table 1.

    Table 1The chemical composition of AZ80M Mg alloy(wt.%).

    The schematic of the manufacturing process of arc additive process is shown in Fig 1a.The gas tungsten arc welding(GTAW)equipment used was a WSE-315D power supply with pulse current mode.The welding torch was fixed on the welding trolley to realize one-way reciprocating movement,and the deposition path was unidirectional.The output type of the welding power was AC pulse,and the main process parameters were given in Table 2.Each sample was deposited with 50 layers,and a typical deposited thin-wall component is shown in Fig.1b.

    Referring to the conventional heat treatment methods[25],the post-deposition heat treatment of the AZ80M Mg alloy included solution treatment(T4),direct artificial aging treatment(T5)and solution+artificial aging treatment(T6).The process details are given in Table 3.The heat treatment experiment was carried out in air by using medium temperature resistance furnace.

    Table 2The process parameters of WAAM AZ80M Mg.

    Table 3The parameters of heat treatment process.

    Table 4Chemical composition of different position marked in Fig.3 obtained by EDS.

    Microstructural characterization and mechanical testing of the deposited wall were conducted after removing the edge zone.Samples for the observation of the microstructure were cut along the building direction.After grinding and polishing,the samples were etched using picric acid(4.2 g picric acid,10 ml acetic acid,10 ml distilled water,100 ml alcohol).The samples were analyzed by A1 Zeiss optical microscope and Quanta FEG 250 scanning electron microscope(SEM)equipped with energy dispersive spectroscopy(EDS).The accelerating voltage was set to be 15 kV.The phase composition was analyzed by PANalytical X′Pert Pro with Cu Kα1 radiation(λ=0.154 nm),and the selected parameters were 40 kV,40 mA with the angle range of 2θ=20-80°(scan step size

    0.013°,time per step 8.67 s and scan type was continuous).

    Fig.1.Schematic of the WAAM system(a)and appearance of single pass 50 layers specimen(b).

    Fig.2.Sampling of WAAM AZ80M wall(a)the tensile sample orientation and sampling position;(b)sampling characteristics for tensile test;(c)sample size for tensile test.

    The deposited component was subjected to tensile testing with samples oriented in two different directions as shown in Fig 2a,(i)parallel(horizontal samples)and(ii)perpendicular(vertical samples)to the deposition direction.As the thickness of the deposited wall was between 8–11 mm,three sheet samples were cut form each tensile sampling location(Fig.2b).Sampling feature and size of the specimen are shown in Fig.2c.The tensile testing was carried out on MTS-CMT5105 universal testing machine with strain rate of 1 mm/min.The Vickers hardness testing was carried out using the HVT-1000A microhardness tester with a load of 1.96 N and a holding duration of 15 s.Each sample was tested for 36 points in a 6×6 array on the section of the sample with an interval of 0.2 mm.The hardness distribution map was drawn after removing the noise and invalid points(such as the points on the porosity).

    3.Results and discussion

    3.1.Microstructural characterization

    The microstructure of WAAM AZ80M under different heat treatment are shown in Fig.3.It can be seen from Fig.3a that as deposited AZ80M Mg alloy possesses a typical ascast microstructure with both interdendritic and intradendritic second phases.SEM analysis(Fig.3b)shows coring effect along the dendrites as well as discontinuous particle-like interdendritic phases.Consistently,according to EDS analysis results(Table 4),the interdendritic second phases were determined to be the divorced eutectic structures ofα-Mg andβ-Mg17Al12along with Ca/Y concentrated particles with high thermal stability due to their limited solubility formed by nonequilibrium solidification during the arc deposition process.Fig.3c and d show the microstructure after T4 heat treatment.It can be seen from Fig.3c that most of the secondary interdendritic phases with low thermal stability(β-Mg17Al12)were dissolved back to the Mg matrix lead to the disappearance of the net-like structure.Mainly Ca and Y concentrated particles were remained after T4 treatment due to their higher thermal stability.Ca,as a microalloying element,could replace Mg atom inβ-Mg17Al12to enhance covalent bond strength and noncovalent bond strength of Mg-Mg atom,so as to improve the thermal stability ofβphase[24].SEM analysis upon T4 heat treatment(see Fig.3d)showed that the size and quantity of the gray white granular eutectic phase were significantly smaller than that of as-deposited condition.On the other hand,the microstructural analysis after T5 heat treatment(shown in Fig.3e and f)indicated that additional second phases formed adjacent to the interdendritic and intradendritic second phases.SEM observation(Fig.3f)showed,in addition to the existence of the original divorced eutectic structure,discontinuous precipitation(DPs)with different morphology was present,which is a typical morphology for DPs ofβ-Mg17Al12(in Table 3)[25].Microstructural evolution upon T6 heat treatment are shown in Fig.3g and h.It was found that due to the solution treatment,secondary phases are mainly dissolved which allowed the observation of fine equiaxed grain structure.Moreover,the ageing treatment caused the formation of more evenly distributed smaller continuous precipitates(CPs)in comparison to T5 condition.Even though bulk secondary phases were mainly disappeared leaving only Ca/Y rich particles,discontinuous interdendriticβ-Mg17Al12precipitation was still present along with thermally induced fine intradendritic precipitates.

    Fig.4 shows the element distribution of WAAM AZ80M Mg alloy under different heat treatment conditions obtained by EDS mapping.The element with the most obvious change should be Al and Zn,which is also the main alloying element of AZ80M.As shown in Fig.4a,the distribution of Al and Zn elements in the AD sample was uneven,with higher concentration in the secondary dendrite and grain boundary,but less in the matrix.After T4 and T6(Fig.4a and d)heat treatment,the distribution of Al and Zn elements became more evenly distributed,while no obvious change in T5 sample(Fig.4c).Moreover,the distribution of Ca and Y had no obvious change because of the formation of(Mg,Al)2Ca/Al2Y phases with higher melting point and higher thermal stability[26].

    Metallic parts prepared by WAAM have layered structure,which have also been reported in Al alloys[27]and steel[28].The main reason for the formation of such inhomogeneity is that the microstructure after solidification is determined by the temperature gradient inside and outside the melt pool and the cooling rate,while the different positions of the deposition layer have different heating and cooling rates.Therefore,the effect of different heat treatment on the layered structure of WAAM AZ80M Mg alloy was also studied.Fig.5 shows the layered structures under different heat treatment states.As shown in Fig.5a,the layered structure in as-deposited sample is obvious,and the interlayer region was composed of columnar dendrites,fine equiaxed crystals and coarse equiaxed crystals.Moreover,there are large quantitative micropores in the interlayer region,which would affect mechanical performance.After T4 heat treatment(Fig.5b),with the partial dissolution of eutectic structure,the original layered structure characteristics got blurred and cannot be easily identified.The layered structure of deposition after T5 heat treatment(Fig.5c)became more obvious,and the degree of solute segregation is enhanced.After T6 heat treatment(Fig.5d),the layered structure becomes fuzzy because of the solid solution,while the aggregation characteristics of the DPs still reflect the original layer interface.

    Fig.3.OM and SEM images with EDS results of WAAM AZ80M alloys:(a)and(b)in AD condition;(c)and(d)in T4 condition;(e)and(f)in T5 condition;(g)and(h)in T6 condition.

    Fig.6 is the X-ray diffraction pattern of WAAM AZ80M Mg alloy upon different heat treatments.The main phases are;α-Mg matrix,β-Mg17Al12and a small amount of Al2Y.It can be seen from Fig.6 that the positions of the characteristic peaks were the same,but the biggest difference of the spectra was the peak position(35.9-2θ)of the highest peak ofβ-Mg17Al12phase under different heat treatment conditions.In comparison to the as-deposited(AD)sample slight shift to the lower angles was found for T4 and T6 indicating lattice expansion.However,T5 sample indicated a larger shift to the higher 2θvalue resulted from a lattice contraction ofβ-Mg17Al12phase.There might be several reasons for this difference between T5-treated sample and the others.One might be related to the variation in composition ofβ-phase due to additional solution treatment for T4 and T6 samples.On the other hand,the presence of residual stress can also lead to the contraction of the lattice.More detailed analysis needs to be pursued for determining the main factor[29].

    3.2.Mechanical properties

    Fig.4.Elements distribution of the WAAM AZ80M alloy obtained by EDS map scanning:(a)as-deposited,(b)T4,(c)T5 and(d)T6 condition.

    Fig.5.Microstructure of the interlayer zone:(a)as-deposited,(b)T4,(c)T5 and(d)T6 condition.

    Fig.7 shows the microhardness values distribution of the WAAM AZ80M Mg alloy under different heat treatment conditions.The hardness value was 55.47 HV for T4,78.4 HV for T5 condition,66.94 HV for T6,and 62.42 HV for AD condition.In comparison to the hardness value of as-deposited alloy,it decreased by 11% for T4,and increased by 26% and 7% for T5 and T6 heat treatment,respectively.In addition,there were differences in the hardness distribution within the material under different heat treatment conditions.With the increase in the content of the second phases in an alloy,the deformation resistance and the hardness of the material can be effectively improved.The hardness distribution of T4 and T6 was more uniform,while that of T5 was more uneven when compared with that of AD condition.This phenomenon was consistent with the results of SEM.

    Fig.6.XRD diffraction patterns of the WAAM AZ80M alloy.

    The ultimate tensile strength(UTS)and elongation(EL)results of the WAAM AZ80M Mg alloy under different heat treatment conditions are shown in Fig.8.The tensile properties of AD samples presented anisotropic characteristics.In vertical direction(UTS:224 MPa,EL:13%),the UTS and EL was 64 MPa and 2% lower than those in horizontal direction(UTS:288 MPa,EL:15%),respectively.According to the variations of UTS and EL shown in Fig.8,after different heat treatment,the mechanical performances of the WAAM AZ80M Mg alloy were improved in different aspects.The EL of T4 sample increased by 60%in horizontal direction and increased by 23% in vertical direction than that of AD samples,which means solution treatment can improve the ductility.Compared to the AD samples,the UTS of the T5 sample in horizontal decreased by 6%,and increased by 15%in vertical,but the EL decreased significantly both in the horizontal and vertical directions.Though,the anisotropy after T5 heat treatment seems to be the least pronounced,considering the error bar(the deviation range of strength and plasticity test results in different directions),the effect of T5 heat treatment was not optimal.The UTS and EL of the T6 samples were 292 MPa and 16% in horizontal direction,and 283 MPa and 14%in vertical direction,respectively.Compared with AD state,both strength and plasticity were improved,and the difference between horizontal direction and vertical direction was obviously weakened.The comprehensive performance was better for several heat treatments.It can be concluded that both T4 and T6 heat treatment can improve WAAM AZ80M alloy mechanical performance and reduce anisotropy.

    Fig.7.Microhardness distribution of WAAM AZ80M alloys(a)as-deposited,(b)T4,(c)T5 and(d)T6 condition.

    Fig.8.Tensile properties of WAAM AZ80M Mg alloy under different treatment conditions

    Fig.9.The effect of interlayer defects on tensile strength’s anisotropy.

    Fig.10.The side view result of the tensile samples in vertical direction:(a)as-deposited,(b)T4,(c)T5 and(d)T6 condition.

    Fig.11.Fracture feature for WAAM AZ80M alloys:(a)as-deposited,(c)T4,(e)T5 and(g)T6 in horizontal direction;(b)as-deposited,(d)T4,(f)T5 and(h)T6 in vertical direction.

    However,the mechanical performance improvement of WAAM AZ80M by heat treatment was restricted by the micropores in the interlayer region.The existence of pores may limit the application of WAAM to a great extent,however,it was difficult to avoid the porosity[30],since the WAAM of Mg alloys was based on the traditional welding process.As shown in Fig.9,the effective bearing area along the vertical direction will be significantly reduced due to the interlayer defects.As shown in Fig.5,there were still a lot of porosity defects in the interlayer area of the WAAM AZ80M Mg alloy even if different heat treatments were carried out,which greatly reduced the improvement in mechanical performance of the alloy by heat treatment.The heat treatment can change the microstructure but cannot eliminate the pores formed in the layer by layer deposition process.

    The difference of tensile properties in horizontal and in vertical directions of heat-treated WAAM AZ80M Mg alloy was related to its microstructure.It was necessary to reduce the inhomogeneity of the vertical structure as much as possible.T4 treatment reduced the amount and size of eutectic structure and increased plasticity.In T5 heat treatment,the precipitates were preferentially distributed along the dendritic boundaries due to the heredity of the element distribution characteristics of the deposited alloy,and the changes of the amount,shape and distribution of the precipitates were the important factors leading to the strengthening of the alloy.After solution+aging treatment(T6),the alloy elements were more evenly dissolved,and the precipitates were more evenly distributed.

    The side view results of the vertically fractured samples are shown in Fig.10.For as-deposited and T5 vertical tensile specimens,the fracture occurred at the boundary between the interlayer region(Fig.10a and c),and the cracks along the eutectic structure were observed around the port(as shown by the arrow).The fractures of T4 and T6 samples occurred on the grain boundary,no obvious cracks were found around the fracture,and the grains around the fracture had been deformed(Fig.10b and d).

    Fig.11 shows the fracture morphologies of the WAAM AZ80M magnesium alloys under different conditions and directions.On the fracture surface of the AD-H sample(Fig.11a),there were dimples of uneven size,particles and small secondary cracks at the bottom of the dimple,while the dimples at the fracture surface of the vertical sample(Fig.11b)were significantly less than those of the horizontal sample.After T4 heat treatment,the dimples on the horizontal sample’s fracture(Fig.11c)became uniform and the toughness characteristics were enhanced,while the dimples on the vertical sample fracture(Fig.11d)were relatively shallow and accompanied by a small number of cleavage steps.The fracture of the horizontal sample(Fig.11e)treated with T5 was composed of rough small particles and curved tear edges,and both sides of the tear edges were composed of cleavage steps of different sizes,while the fracture of the vertical sample(Fig.11f)was mainly composed of tearing edges and cleavage steps,and there was a fracture platform,showing the characteristics of brittle fracture.After T6 heat treatment,the dimples on the fracture surfaces of the horizontal and vertical samples(Fig.11g and h)decreased with the tear edges increased.This is because the effective binding area between phase andα-Mg dispersed on the matrix increased,which enhanced the binding force with the matrix and thus increased the strength of the material.

    4.Conclusion

    In this study,WAAM AZ80M Mg alloy was produced based on GTAW process,and three different kinds of heat treatment methodologies(T4,T5 and T6)were conducted to the WAAM fabricated AZ80M Mg alloy.The microstructure and mechanical properties of as-deposited and post heattreated samples were investigated.The conclusions can be drawn as following.

    1.The microstructure of the as-deposited state was mainly equiaxed dendrite,and the second phase was distributed along the interdendritic regions to form a network structure.The average microhardness was 62.4 HV,and the horizontal direction and the vertical direction had tensile asymmetry.

    2.T4 heat treatment made the eutectic phase dissolved and eliminated the inhomogeneity of some interlaminar structure,the hardness value decreased to 55.7 HV,and the UTS both in horizontal and vertical decreased but the EL increased significantly.

    3.T5 treatment inherited the characteristics of the dendritic structure,and the discontinuous precipitation distributed along the eutectic phases.The average microhardness was 78.4 HV but unevenly distributed.The UTS was improved but EL decreased significantly.

    4.T6 treatment formed continuous precipitation in the grains,and effectively improved the microstructure uniformity.The average microhardness was 66.9 HV.Both the UTS and EL in horizontal and vertical direction improved,and the anisotropy was somewhat reduced.

    Declaration of Competing Interest

    None.

    Acknowledgment

    This work was supported by the China Scholarship Council[grant numbers:201907000039],the National Key Research and Development Plan of China[grant number 2017YFB0305905].The authors acknowledge the financial support from the 2020 open projects[grant numbers:KLATM202003]of Key laboratory of Advanced Technologies of Materials,Ministry of Education China,Southwest Jiaotong University.

    美女视频免费永久观看网站| 国产成人av激情在线播放| 五月天丁香电影| 有码 亚洲区| 大码成人一级视频| 国产精品.久久久| 欧美亚洲日本最大视频资源| 日本av手机在线免费观看| 在线观看美女被高潮喷水网站| 黄色毛片三级朝国网站| 亚洲四区av| 99久久综合免费| 欧美成人午夜精品| 人妻人人澡人人爽人人| 熟女电影av网| 欧美 亚洲 国产 日韩一| 一级片免费观看大全| 成人毛片a级毛片在线播放| 亚洲av国产av综合av卡| 丝袜人妻中文字幕| 香蕉国产在线看| 国产精品秋霞免费鲁丝片| 日韩中文字幕视频在线看片| 国产一区亚洲一区在线观看| 欧美日韩亚洲国产一区二区在线观看 | 巨乳人妻的诱惑在线观看| 亚洲欧美色中文字幕在线| 大陆偷拍与自拍| 一区二区av电影网| 国产成人a∨麻豆精品| 晚上一个人看的免费电影| 国产毛片在线视频| 大香蕉久久成人网| 日韩成人av中文字幕在线观看| 国产日韩欧美视频二区| 老汉色av国产亚洲站长工具| 香蕉国产在线看| 久久久久久久久免费视频了| 免费黄网站久久成人精品| 美女高潮到喷水免费观看| 男人操女人黄网站| 丝袜美足系列| 亚洲第一av免费看| 1024视频免费在线观看| 人人澡人人妻人| 天堂俺去俺来也www色官网| 免费看不卡的av| 日韩av在线免费看完整版不卡| 国产亚洲午夜精品一区二区久久| 亚洲五月色婷婷综合| 少妇的逼水好多| 1024视频免费在线观看| 国产人伦9x9x在线观看 | 免费观看a级毛片全部| 天堂8中文在线网| 啦啦啦啦在线视频资源| 国产成人精品在线电影| 可以免费在线观看a视频的电影网站 | 777久久人妻少妇嫩草av网站| 美女午夜性视频免费| 久久99一区二区三区| 精品久久蜜臀av无| 亚洲欧美精品综合一区二区三区 | 日韩大片免费观看网站| 亚洲国产精品成人久久小说| 亚洲第一青青草原| 一区在线观看完整版| 91在线精品国自产拍蜜月| 国产精品久久久久久久久免| 亚洲成人av在线免费| 十分钟在线观看高清视频www| av电影中文网址| 国产亚洲av片在线观看秒播厂| 丝袜美腿诱惑在线| 色哟哟·www| 日韩 亚洲 欧美在线| 午夜免费观看性视频| 精品人妻偷拍中文字幕| 伦理电影免费视频| 精品国产超薄肉色丝袜足j| 高清视频免费观看一区二区| 日本色播在线视频| 亚洲第一av免费看| 国产在线视频一区二区| 少妇人妻久久综合中文| 午夜老司机福利剧场| 久久久国产欧美日韩av| 久久久久久久久久久久大奶| 校园人妻丝袜中文字幕| 亚洲国产精品国产精品| 母亲3免费完整高清在线观看 | 国产xxxxx性猛交| 国产福利在线免费观看视频| 黑人猛操日本美女一级片| 久久久久国产精品人妻一区二区| 免费在线观看完整版高清| 男人操女人黄网站| 中文字幕精品免费在线观看视频| 男女无遮挡免费网站观看| 久久免费观看电影| 亚洲 欧美一区二区三区| 天天躁夜夜躁狠狠躁躁| 精品国产一区二区三区久久久樱花| 一本—道久久a久久精品蜜桃钙片| 亚洲av免费高清在线观看| h视频一区二区三区| 91午夜精品亚洲一区二区三区| www.熟女人妻精品国产| 欧美成人精品欧美一级黄| 亚洲中文av在线| 国产一区二区在线观看av| 热re99久久国产66热| 一区二区三区激情视频| 国产日韩一区二区三区精品不卡| 1024视频免费在线观看| 视频在线观看一区二区三区| 少妇被粗大猛烈的视频| 91aial.com中文字幕在线观看| av又黄又爽大尺度在线免费看| 国产高清国产精品国产三级| 王馨瑶露胸无遮挡在线观看| 女性被躁到高潮视频| 国产精品久久久久久精品古装| 中文字幕制服av| 久久久久久久亚洲中文字幕| 国产色婷婷99| 免费大片黄手机在线观看| 丝袜美腿诱惑在线| 免费播放大片免费观看视频在线观看| 777米奇影视久久| 国产1区2区3区精品| 黄网站色视频无遮挡免费观看| 国产野战对白在线观看| 久久久久久人妻| 免费观看a级毛片全部| 哪个播放器可以免费观看大片| 青青草视频在线视频观看| 熟妇人妻不卡中文字幕| 精品人妻偷拍中文字幕| av国产精品久久久久影院| 国产在线一区二区三区精| 欧美xxⅹ黑人| 国产日韩一区二区三区精品不卡| 老女人水多毛片| 精品人妻偷拍中文字幕| av卡一久久| 亚洲第一av免费看| 两性夫妻黄色片| 王馨瑶露胸无遮挡在线观看| 热99久久久久精品小说推荐| av免费在线看不卡| 国产精品国产三级国产专区5o| www.av在线官网国产| 最近最新中文字幕免费大全7| 午夜激情av网站| 欧美日本中文国产一区发布| 国产亚洲欧美精品永久| 在线亚洲精品国产二区图片欧美| 亚洲欧美一区二区三区黑人 | 亚洲国产看品久久| 国产极品粉嫩免费观看在线| 亚洲国产精品成人久久小说| 国产在线免费精品| 男女高潮啪啪啪动态图| 伊人久久国产一区二区| 天天躁夜夜躁狠狠久久av| xxxhd国产人妻xxx| 美女中出高潮动态图| 街头女战士在线观看网站| 精品国产国语对白av| 国产淫语在线视频| 最新中文字幕久久久久| 最近2019中文字幕mv第一页| 国产男女超爽视频在线观看| 成人18禁高潮啪啪吃奶动态图| 亚洲图色成人| 亚洲人成电影观看| 中文字幕精品免费在线观看视频| 亚洲精华国产精华液的使用体验| 亚洲精品乱久久久久久| 国产精品蜜桃在线观看| 免费女性裸体啪啪无遮挡网站| 精品一区在线观看国产| 中文字幕制服av| 最近最新中文字幕大全免费视频 | 欧美另类一区| 精品亚洲乱码少妇综合久久| a级毛片在线看网站| 日日摸夜夜添夜夜爱| 一级爰片在线观看| 最新中文字幕久久久久| 最近的中文字幕免费完整| 国产欧美亚洲国产| av天堂久久9| 韩国精品一区二区三区| 只有这里有精品99| 老司机亚洲免费影院| 国产精品二区激情视频| 久久久久视频综合| 如何舔出高潮| 永久网站在线| 卡戴珊不雅视频在线播放| 久久狼人影院| 七月丁香在线播放| 国产精品蜜桃在线观看| 婷婷色麻豆天堂久久| 少妇猛男粗大的猛烈进出视频| 日韩电影二区| 十分钟在线观看高清视频www| 日韩中文字幕欧美一区二区 | 美女高潮到喷水免费观看| 日本猛色少妇xxxxx猛交久久| 三上悠亚av全集在线观看| 纵有疾风起免费观看全集完整版| 久久国产亚洲av麻豆专区| 两个人免费观看高清视频| 最新中文字幕久久久久| 啦啦啦啦在线视频资源| 男女边摸边吃奶| 精品国产国语对白av| 国产精品不卡视频一区二区| 国产野战对白在线观看| 免费高清在线观看视频在线观看| 免费日韩欧美在线观看| 亚洲人成77777在线视频| 久久久精品94久久精品| 亚洲国产精品国产精品| 日韩中字成人| 亚洲一区中文字幕在线| 久久女婷五月综合色啪小说| 天堂8中文在线网| 国产色婷婷99| 色吧在线观看| 国产一级毛片在线| 1024视频免费在线观看| 久久久久网色| 久久女婷五月综合色啪小说| av国产精品久久久久影院| 秋霞伦理黄片| 亚洲精品乱久久久久久| 国产乱人偷精品视频| 汤姆久久久久久久影院中文字幕| 国产精品久久久久久精品电影小说| 黄色一级大片看看| 亚洲情色 制服丝袜| 欧美精品高潮呻吟av久久| 日本色播在线视频| 最近的中文字幕免费完整| 国产精品av久久久久免费| 久久人人爽av亚洲精品天堂| 午夜免费男女啪啪视频观看| 七月丁香在线播放| 黑人巨大精品欧美一区二区蜜桃| 观看av在线不卡| a 毛片基地| 午夜福利在线免费观看网站| 91在线精品国自产拍蜜月| 日韩欧美一区视频在线观看| 最新的欧美精品一区二区| 人人澡人人妻人| 精品国产一区二区三区久久久樱花| 18在线观看网站| 欧美国产精品一级二级三级| 国产精品久久久久久精品电影小说| 青春草视频在线免费观看| 男女边摸边吃奶| 校园人妻丝袜中文字幕| 亚洲美女搞黄在线观看| 中文字幕另类日韩欧美亚洲嫩草| 久久久久视频综合| 亚洲av免费高清在线观看| 一区福利在线观看| 91国产中文字幕| 我的亚洲天堂| 国产在线一区二区三区精| 天天操日日干夜夜撸| 久久午夜综合久久蜜桃| 国产一级毛片在线| 丝袜美腿诱惑在线| 欧美中文综合在线视频| 精品国产超薄肉色丝袜足j| 成人亚洲精品一区在线观看| av免费在线看不卡| 免费黄色在线免费观看| 国产成人精品福利久久| 夫妻午夜视频| 男人舔女人的私密视频| 在线天堂最新版资源| 色哟哟·www| 肉色欧美久久久久久久蜜桃| 又大又黄又爽视频免费| 我的亚洲天堂| 三级国产精品片| 久久久久国产网址| 久久久久久伊人网av| a级毛片黄视频| 欧美人与善性xxx| 久久久精品国产亚洲av高清涩受| 精品国产国语对白av| 亚洲欧洲日产国产| 精品99又大又爽又粗少妇毛片| 国产有黄有色有爽视频| www.熟女人妻精品国产| 纯流量卡能插随身wifi吗| 欧美激情高清一区二区三区 | 少妇人妻久久综合中文| 国产精品久久久久久精品电影小说| 亚洲男人天堂网一区| 亚洲伊人久久精品综合| 美女国产高潮福利片在线看| 久久亚洲国产成人精品v| 亚洲欧洲国产日韩| 欧美国产精品va在线观看不卡| 18禁国产床啪视频网站| 人人妻人人澡人人看| 国产精品熟女久久久久浪| 国产精品国产av在线观看| av福利片在线| 成年人午夜在线观看视频| 91精品三级在线观看| 日本vs欧美在线观看视频| 久久精品夜色国产| 在线天堂中文资源库| 大码成人一级视频| 热re99久久精品国产66热6| 国产av精品麻豆| 亚洲国产精品一区三区| 久久久国产欧美日韩av| 国产精品国产三级专区第一集| 国产精品久久久久久av不卡| 日韩精品免费视频一区二区三区| 日本色播在线视频| 2021少妇久久久久久久久久久| 亚洲国产精品999| 一本—道久久a久久精品蜜桃钙片| 日韩一区二区三区影片| 大陆偷拍与自拍| 人人澡人人妻人| 91成人精品电影| 亚洲精品,欧美精品| 王馨瑶露胸无遮挡在线观看| 精品视频人人做人人爽| 青草久久国产| 日韩欧美精品免费久久| 久久精品aⅴ一区二区三区四区 | av国产精品久久久久影院| 国产淫语在线视频| 日韩伦理黄色片| 国产 精品1| 国产精品.久久久| 国产亚洲午夜精品一区二区久久| 一级黄片播放器| 久久久久久久久久久免费av| 久久久国产一区二区| 天天躁夜夜躁狠狠躁躁| 亚洲伊人久久精品综合| 国产日韩欧美亚洲二区| 一本—道久久a久久精品蜜桃钙片| 91成人精品电影| 色吧在线观看| 男人添女人高潮全过程视频| 男女边吃奶边做爰视频| 亚洲欧美成人精品一区二区| 人人妻人人添人人爽欧美一区卜| 捣出白浆h1v1| 国产1区2区3区精品| 国产精品.久久久| 91精品国产国语对白视频| 岛国毛片在线播放| videossex国产| 最近中文字幕2019免费版| 午夜91福利影院| 九草在线视频观看| 亚洲婷婷狠狠爱综合网| 日本免费在线观看一区| 曰老女人黄片| 亚洲精品久久久久久婷婷小说| 日韩一区二区三区影片| 国产免费又黄又爽又色| 国产成人91sexporn| 十八禁高潮呻吟视频| 菩萨蛮人人尽说江南好唐韦庄| 精品亚洲乱码少妇综合久久| 久久久久视频综合| 精品一品国产午夜福利视频| 丰满乱子伦码专区| 欧美黄色片欧美黄色片| 一二三四中文在线观看免费高清| 欧美日韩综合久久久久久| 性色avwww在线观看| 国产精品av久久久久免费| 我要看黄色一级片免费的| 国产成人精品久久久久久| 亚洲一区中文字幕在线| 2022亚洲国产成人精品| 亚洲国产欧美日韩在线播放| 最黄视频免费看| 国产精品免费视频内射| 日韩人妻精品一区2区三区| 一级黄片播放器| 久久精品亚洲av国产电影网| 狠狠精品人妻久久久久久综合| 如日韩欧美国产精品一区二区三区| 亚洲国产欧美日韩在线播放| 菩萨蛮人人尽说江南好唐韦庄| 国产亚洲av片在线观看秒播厂| av又黄又爽大尺度在线免费看| 日韩精品免费视频一区二区三区| 青春草亚洲视频在线观看| 欧美+日韩+精品| 久久久久久久精品精品| 夫妻性生交免费视频一级片| 色婷婷久久久亚洲欧美| 1024视频免费在线观看| 国产精品久久久久久久久免| 日本vs欧美在线观看视频| 国产一区有黄有色的免费视频| 中文字幕色久视频| 秋霞伦理黄片| 我的亚洲天堂| 99re6热这里在线精品视频| 亚洲情色 制服丝袜| 青春草视频在线免费观看| 国产黄频视频在线观看| 欧美日韩视频精品一区| 不卡av一区二区三区| 99re6热这里在线精品视频| 欧美国产精品一级二级三级| 午夜影院在线不卡| 久久这里只有精品19| 日韩 亚洲 欧美在线| 男女下面插进去视频免费观看| 亚洲国产欧美网| 女性生殖器流出的白浆| 日本爱情动作片www.在线观看| 国产淫语在线视频| 99久久中文字幕三级久久日本| 久热久热在线精品观看| 老鸭窝网址在线观看| 婷婷色综合www| 国产成人精品在线电影| 亚洲精品久久午夜乱码| 午夜福利一区二区在线看| 久久久久视频综合| av线在线观看网站| 日本色播在线视频| 一区二区三区激情视频| 男女边摸边吃奶| a 毛片基地| 最近最新中文字幕大全免费视频 | 免费高清在线观看日韩| av在线播放精品| 18禁国产床啪视频网站| 多毛熟女@视频| 男女无遮挡免费网站观看| 女人精品久久久久毛片| 黑人巨大精品欧美一区二区蜜桃| 69精品国产乱码久久久| 婷婷色av中文字幕| 免费人妻精品一区二区三区视频| 一级毛片黄色毛片免费观看视频| 成人午夜精彩视频在线观看| 男女高潮啪啪啪动态图| 99国产精品免费福利视频| 国产免费视频播放在线视频| 免费观看在线日韩| 狂野欧美激情性bbbbbb| 制服诱惑二区| videos熟女内射| 亚洲精品国产一区二区精华液| 欧美老熟妇乱子伦牲交| 美女福利国产在线| 寂寞人妻少妇视频99o| 亚洲精品成人av观看孕妇| 波多野结衣一区麻豆| 国产乱人偷精品视频| 免费久久久久久久精品成人欧美视频| 91精品三级在线观看| 欧美日韩国产mv在线观看视频| 人成视频在线观看免费观看| 成人二区视频| 亚洲精品乱久久久久久| 国产伦理片在线播放av一区| 亚洲国产欧美网| 中文天堂在线官网| 晚上一个人看的免费电影| 七月丁香在线播放| 蜜桃在线观看..| 男男h啪啪无遮挡| 永久免费av网站大全| 一区二区三区激情视频| 国产成人91sexporn| 国产av一区二区精品久久| 一区二区三区四区激情视频| 亚洲av日韩在线播放| 日韩一区二区三区影片| 少妇人妻久久综合中文| 久久久欧美国产精品| 国产1区2区3区精品| 最近最新中文字幕大全免费视频 | 国精品久久久久久国模美| 久久人妻熟女aⅴ| 国产成人aa在线观看| 欧美bdsm另类| 精品视频人人做人人爽| 国精品久久久久久国模美| 国产免费福利视频在线观看| 超碰97精品在线观看| 一本—道久久a久久精品蜜桃钙片| 亚洲欧美成人精品一区二区| 欧美日韩国产mv在线观看视频| 日韩av不卡免费在线播放| 18禁观看日本| 免费久久久久久久精品成人欧美视频| 免费大片黄手机在线观看| 五月天丁香电影| 日本色播在线视频| 欧美97在线视频| 色视频在线一区二区三区| 肉色欧美久久久久久久蜜桃| 热re99久久精品国产66热6| 桃花免费在线播放| 欧美老熟妇乱子伦牲交| 美国免费a级毛片| 只有这里有精品99| 午夜福利视频在线观看免费| 久久人人爽av亚洲精品天堂| 黄频高清免费视频| 欧美亚洲日本最大视频资源| 中文精品一卡2卡3卡4更新| 亚洲在久久综合| 亚洲四区av| 男人操女人黄网站| 亚洲三级黄色毛片| 国产成人免费无遮挡视频| 男的添女的下面高潮视频| 中文字幕亚洲精品专区| 男女边吃奶边做爰视频| 90打野战视频偷拍视频| 狂野欧美激情性bbbbbb| 亚洲伊人久久精品综合| 欧美激情 高清一区二区三区| av国产久精品久网站免费入址| 婷婷色麻豆天堂久久| 99久久人妻综合| 中文字幕最新亚洲高清| 国产有黄有色有爽视频| 亚洲成人一二三区av| 中文精品一卡2卡3卡4更新| 在线天堂中文资源库| 欧美日韩av久久| 搡女人真爽免费视频火全软件| 国产午夜精品一二区理论片| 精品国产国语对白av| 免费高清在线观看视频在线观看| av在线老鸭窝| 看免费av毛片| 交换朋友夫妻互换小说| 99久久人妻综合| 成人18禁高潮啪啪吃奶动态图| 中文字幕另类日韩欧美亚洲嫩草| 国产精品久久久久久精品古装| av网站在线播放免费| 国产精品久久久久成人av| 黄片无遮挡物在线观看| 国产又爽黄色视频| 国产成人免费无遮挡视频| 亚洲精品自拍成人| 精品99又大又爽又粗少妇毛片| 欧美另类一区| 午夜福利在线免费观看网站| 一区二区三区激情视频| 亚洲国产欧美在线一区| 免费大片黄手机在线观看| 一二三四在线观看免费中文在| 久久这里只有精品19| 尾随美女入室| 午夜日韩欧美国产| 黑丝袜美女国产一区| 在现免费观看毛片| 亚洲精品日韩在线中文字幕| 中文字幕制服av| 亚洲综合色网址| 亚洲精品美女久久久久99蜜臀 | 亚洲美女视频黄频| 午夜影院在线不卡| 制服人妻中文乱码| 亚洲成色77777| 亚洲一区中文字幕在线| 欧美日韩成人在线一区二区| 丝瓜视频免费看黄片| 成人国产av品久久久| 亚洲av电影在线进入| 天堂俺去俺来也www色官网| 亚洲av福利一区| 人人妻人人澡人人爽人人夜夜| 亚洲欧美日韩另类电影网站| 爱豆传媒免费全集在线观看| 黄色一级大片看看| 一边摸一边做爽爽视频免费| 在线观看三级黄色| 亚洲成色77777| 国产无遮挡羞羞视频在线观看| 有码 亚洲区| 精品国产露脸久久av麻豆| 老汉色∧v一级毛片| 国产男女内射视频| 人体艺术视频欧美日本| 国产成人欧美| 国产精品欧美亚洲77777| 欧美人与善性xxx| 久久精品国产综合久久久| 亚洲国产精品999| 电影成人av| 毛片一级片免费看久久久久|