    Search for Effective Catalysts for the Development of Engines Based on the Products of Catalytic Decomposition of N2O

    2021-03-08 08:32:24Boryaev
    火炸藥學(xué)報(bào) 2021年1期

    A.A.Boryaev

    (Saint-Petersburg State University of Architecture and Civil Engineering, 4 Vtoraya Krasnoarmeyskaya St., Saint-Petersburg 190005, Russia)

    Abstract:The paper presents requirements for the N2O decomposition catalyst and provides justification for the selection of components to develop its formulation. The methods to study the physical and chemical as well as catalytic properties of catalysts were developed, and the results of experimental studies on the properties of catalysts with different composition in the laboratory conditions were presented. The activity of samples of compact metal catalysts as well as samples of supported metal and oxide catalysts in the nitrous oxide decomposition reaction was studies. The methodology for determining the activity of catalysts in the decomposition reaction of N2O is presented, as well as the design of an experimental reactor for determining the activity of the catalyst by the minimum temperature for the onset of the decomposition reaction of N2O. In the course of the study, the following series of catalyst activity are determined in the N2O decomposition reaction up to a temperature of 600℃: based on platinum group metals applied to the aluminum oxide carrier — Rh>Ru>Ir>Pt>Pd; based on simple oxides applied to the aluminum oxide carrier —CoO>Cr2O3, MnO2>CuO>ZrO2>NiO>Fe2O3. The following activity series for the most promising carriers are also determined: by the onset temperature of decomposition, ZrO2>Al2O3-CaO>Al2O3-ZrO2>Al2O3-AlN>θ-Al2O3>Al2O3-SiO2>SiO2>α-Al2O3; by the rate constants of N2O decomposition, Al2O3-SiO2>Al2O3-AlN>ZrO2>Al2O3>Al2O3-ZrO2>Al2O3-CaO>α - Al2O3>SiO2. The paper presents the results of selecting the active component and carriers for the supported catalyst. The author proposes formulations of the nitrous oxide decomposition catalyst for bench testing in simulated engines.

    Keywords:nitrous oxide; engines; catalyst; properties;formulation

    Introduction

    Due to toughening requirements for the environmental safety of propellants, N2O has recently gained increasing attention as an environmentally-friendly and, at the same time, high-energy monopropellant. The use of N2O, which has a saturated vapor pressure of 5MPa (at 20℃), allows us to implement new design solutions when creating a spacecraft control propulsion system. However, the use of N2O in space equipment is currently constrained by the lack of a highly-efficient decomposition catalyst. The development of such a catalyst is a complex task, which is due to the requirements for the engine operating conditions, on the one hand, the thermodynamic and chemical properties of nitrous oxide itself, on the other hand[1].

    The paper presents the developed requirements for the N2O decomposition catalyst, provides experimental justification for the choice of active components and carriers to conduct an experimental assessment of their catalytic properties, and describes the developed methods to study physical and chemical as well as catalytic properties of catalyst samples and conditions of their achievement. Based on the results of experimental studies, the formulation of nitrous oxide decomposition catalysts for engines was selected.

    1 Requirements for the catalyst and justification for the choice of components to develop its formulation

    1.1 Requirements for the catalyst with regard to conditions of its operation in the engine

    High catalytic activity is one of the main requirements for a catalyst. The N2O decomposition catalyst shall initiate the process at the lowest possible temperature. Analysis of the literature data on the activity of various chemicals in the N2O decomposition reaction demonstrates[2]that the best samples of catalysts begin to show their activity at temperatures above 300℃, and decompose nitrous oxide with a noticeable speed only when the temperature increases further. Moreover, its auto-catalytic decomposition is carried out at temperatures much higher than the minimum onset temperature of decomposition. This means that currently it is almost impossible to develop an engine based on the decomposition of such a thermally stable compound as N2O, which could be started without catalyst preheating. Therefore, it is necessary to develop a catalyst that would initiate the decomposition process at the lowest possible temperature (~300℃). A catalyst for nitrous oxide decomposition with high activity can be developed by applying an active component (AC) to a thermally stable carrier of a certain chemical nature with a developed surface (at least 20-30m2/g), which are determined during the formulation elaboration.

    When N2O is decomposed, a significant amount of heat is released, and, as a result, depending on the decomposition degree, the temperature in the catalyst layer will vary in a wide range and can reach ~1500℃:

    2N2O = 2 N2+O2+163.3kJ

    (1)

    Therefore, another important requirement for the catalyst is its capability to maintain its constant activity throughout the entire resource, i.e. the catalyst should be thermally stable up to a temperature of 1500℃. One of the products of N2O decomposition is oxygen, which can interact with the AC, thus contributing to changes in the catalyst activity. Therefore, the catalyst should be chemically stable up to the above temperature as well. An important catalyst characteristic is its grain size. Reducing the size of the catalyst grain will help increase the access of the precursor to the catalyst surface. Based on the requirements for the engine, the thermodynamics and chemical properties of the nitrous oxide decomposition process[1-2], it can be assumed that the developed catalyst should:

    (1)Be a supported catalyst in the form of rounded pellets (0.8-1.25mm in size), with a developed specific surface area (at least 20-30m2/g), a heterogeneous porous structure, and both micro- (1-10nm) and macro- (more than 100nm) pores and transport pores (up to 100nm);

    (2)Ensure the minimum onset temperature of N2O decomposition in terms of activity;

    (3)Be thermally and chemically stable up to a temperature of 1200℃ in the atmosphere of N2O and its decomposition products; its properties, as the resource is exhausted, should not undergo significant changes that would lead to a noticeable decrease in its activity and performance.

    1.2 Choosing the catalyst type and promising active components

    From the analysis of the literature data[2], it is known that metal and supported metal and oxide catalysts can be used for N2O decomposition. Supported catalysts are catalysts where the AC is distributed on the surface of a specially selected carrier. Compact metal catalysts (usually block catalysts-briquettes compressed from a catalytically active metal wire) have some advantages over supported ones. For example, they are characterized by high thermal conductivity, which makes it possible to organize effective redistribution of heat in the reactor, plasticity, significant mechanical and erosive strength increasing the service life of such catalysts.

    1.2.1 Metal (compact) catalysts

    (1) Choosing the catalyst type

    Compact metal block catalysts can be of several types: cellular metal-ceramic catalysts and catalysts in the form of “metal rubber” (compressed metal and catalytically active wire in the form of a briquette). Based on the operating conditions, metal catalysts of the “metal rubber” type are the most promising. These catalysts are made by the special laying of metal wire spirals in a press-die. Their manufacturing technology is simple, and it makes it possible to get blocks with reproducible properties. The total surface of such catalysts can be adjusted by changing the wire diameter, and the porous structure can be adjusted by the size of the briquette pressing.

    (2) Active components for compact catalysts

    From the above requirements for N2O decomposition catalysts and features of the technology for the manufacturing of metal catalysts of the “metal rubber” type, it follows that the materials taken to manufacture catalysts of this type should meet the following requirements:

    Have a melting point above 1500℃;

    Be plastic and madein the form of a wire with a diameter of 0.1-0.4mm;

    Not interact with oxygen up to a temperature of 1200℃.

    The following list shows some metals arranged in ascending order with regard to their melting point (℃), which are of interest for research in terms of their activity[3]:

    Ni(1463), Co(1495), Fe(1539), Pd(1550), Pt(1770),Zr(1852), Cr(1890), V(1960), Rh(1966), Ru(2427), Ir(2454), Nb(2539), Mo(2620), Re(3170), W(3410), Os(3227).

    Not all of the above metals, despite their high melting point, are stable in an oxidizing environment (especially in an oxygen environment)[4-5].

    Zirconium and niobium interact with O2intensively at temperatures above 200℃, and at 700℃, they burn to form ZrO2and NbO2. In a highly dispersed form, they are pyrophoric.

    Mo, W and Re metals are stable under normal conditions in the O2atmosphere. However, when heated above the “red heat” temperature -400℃ (and for Re-above 300℃)-even compact metals are oxidized easily. In terms of their oxidation ability (MeO3is mainly formed), they can be arranged as follows: Mo>W>Re.

    Re is characterized by the formation of easily volatile Re2O7oxide. It should be noted that at high temperatures (~1000℃), MoO3and WO3oxides sublimate.

    When heated in the air up to a temperature of 500℃, Ni and Co are oxidized easily in a compact form (covered with oxide films), and Fe interacts with wet O2at room temperature. It should be noted that these metals are pyrophoric in the air in their highly dispersed state.

    Vanadium becomes brittle when heated in the air above 300℃ (O2dissolution in the metal is observed); at 600-700℃, the metal is oxidized intensively to form V2O5, which partially dissociates and partially sublimates above 700℃.

    Chromium is one of the most stable metals in the O2atmosphere. When a compact metal is heated, the formation of surface oxide is observed, and only at a temperature of about 2000℃, it starts to burn in O2to form a thermally stable Cr2O3oxide.

    All metals of the platinum group (except Os, which is easily oxidized at 120℃ to the very volatile and poisonous oxide OsO4), when heated in the air, form an oxide film that protects the compact metal against further oxidation. However, in a highly dispersed state, when they are calcined in an oxygen atmosphere, the formation of oxides is observed.

    For instance, when heated in the air (up to 450℃), the compact Ru is oxidized (a surface oxide film is formed); in a highly dispersed form, oxidation occurs at 100℃ with the formation of volatile RuO4(Tevaporation=60℃) and RuO2, which dissociates at 930-950℃ and sublimates.

    Compact palladium is oxidized at 600-700℃, with the formation of PdO; in a highly dispersed form, oxidation occurs at a lower temperature.

    Iridium is very stable to oxygen but in a highly dispersed state at a temperature above 600℃, it is also able to form an unstable oxide-Ir2O3, which easily dissociates into Ir and very stable oxide IrO2. At temperatures above 1100℃, its partial dissociation into Ir and O2is observed. Some researchers note the volatility of this oxide. It should be noted that the introduction of Ir in Pt, Pd, Ni and other alloys increases their hardness and corrosion resistance.

    When dispersed Rh is heated in the air up to 600-800℃, the formation of Rh2O3oxide is also observed, which, similar to iridium oxide at temperatures above 1100℃, decomposes into Rh and O2.

    Pt has the greatest resistance to oxidation; it shows no noticeable oxidation even during melting. However, in a highly dispersed form, when it is heated in an O2atmosphere at 700℃, we observed the formation of a PtO oxide film. Pt-based alloys have high corrosion resistance.

    Thus, taking into account the above data on the O2influence on the state of the metal, we can state that, depending on the temperature, the considered metals under the conditions of N2O decomposition will have different degrees of oxidation. In the initial (~300℃) and final states (above 1000℃), some metals will be in the metallic state, and in the intermediate temperature range-in the oxidized form.

    Based on the properties of the metals discussed above, metals in the form of a Pt wire and its alloys with Rh andIr, as well as Ni and its alloy with chromium (nichrome) can be taken as precursors for catalysts of the “metal rubber” type for research in the N2O decomposition reaction.

    1.2.2 Supported catalysts

    It is necessary to select an active component and an appropriate carrier to create a supported catalyst.

    (1) Choosing promising carriers

    As mentioned above, N2O decomposition catalyst carriers should meet some stringent requirements:

    The melting point of the precursors and the carrier itself-above 2000℃;

    Inertia in the atmosphere of N2O and its decomposition products-up to 1500℃;

    The specific surface area and phase state-stable up to 1200℃;

    The initial specific surface area-at least 20-30m2/g;

    Total pore volume-at least 0.26cm3/g;

    Porous structure-heterogeneous with a set of micro-, macro-, and transport pores;

    Mechanically strong and resistant to heat shock and vibration overload;

    Pellets-rounded shape, with a size in the range of 0.8-1.25mm.

    Taking into account the above requirements, the following high-temperature oxides and compounds could be used as carriers.

    Carriersbasedonaluminumoxide.Currently, carriers based on aluminum oxide having several modifications, the stability of which is different at high temperatures, are the most common in catalysis[6].

    The most widely used carrier is based on γ-Al2O3. Its manufacturing technology is developed in detail, and its properties are well studied. The carrier can be obtained with a specific surface area of 120-300m2/g and a heterogeneous porous structure with a total pore volume of 0.3-0.7cm3/g. However, the carrier based on γ-Al2O3is of no interest for the N2O decomposition process since in the operating temperature range of 700-1200℃ it will undergo polymorphic transformations into the final product α-Al2O3:

    γ-Al2O3→ θ-Al2O3→ α-Al2O3

    According to our research, the transformations are accompanied by an increase in the primary particles of γ-Al2O3and, as a result, a decrease in the specific surface area, porous structure and carrier pellet strength is observed.

    α-Al2O3is corundum, the most stable form of aluminum oxide (Tmelting~2150℃), which has sufficient mechanical strength and stability in the reaction products. However, the carrier based on it has a small specific surface area (~1m2/g) and a low total pore volume (~0.2cm3/g); therefore, it is impossible to obtain a highly active catalyst supported by such a carrier. In this regard, α-Al2O3is also not considered as a promising carrier for the N2O decomposition catalyst.

    In our opinion, the θ-Al2O3form is promising since it is resistant to sintering up to 1000℃. At the final temperature of its production of 750℃, it can have a specific surface area of 80-120m2/g, and a heterogeneous porous structure (a typical pore pattern is shown in Fig. 1) and a total pore volume of 0.30-0.40cm3/g. During heat treatment up to 1200℃, the carrier pellets do not shrink due to the introduction of a certain amount of α-Al2O3into its composition during production. In the finished form, the carrier is a mixture of (γ+θ+α)-Al2O3. In Fig.1 shows the porous structure of three batches of a carrier with the composition(γ+θ+α)-Al2O3, which were manufactured using the same technology (sample 1, sample 2 and sample 3).

    Fig. 1 Porous structure of three different samples of the carrier with the composition (γ + θ + α) -Al2O3 of different production batches

    Some methods are known to reduce the rate of the phase transition of γ-Al2O3to α-Al2O3. One of them is based on the introduction of alkaline earth metal compounds in the production process, which, by introducing into the octahedral voids of γ-Al2O3, inhibit the process of transition to α-Al2O3. Based on this principle, the aluminum oxide carrier stabilized with calcium oxide retains a high specific surface area (~60m2/g) and a heterogeneous porous structure during heat treatment at 1100℃ for 3 hours. Such a carrier can be recommended for preparing the N2O decomposition catalyst based on it.

    Carriersbasedonaluminumnitride. Another promising carrier is a carrier based on aluminum nitride having a high melting point (~2000℃). Its mechanical strength and macroporous structure are based on a framework made of the aluminum nitride sintered at 1700℃, and the specific surface and microporous structure are provided by the aluminum oxide formed during the hydrolysis of the framework surface and subsequent heat treatment at a final temperature of 650℃. The aluminum oxide formed on the framework surface not only contributes to the development of the specific surface but also protects the framework against the chemical interaction with salt solutions during the AC application. Such a carrier can have a specific surface area of 60-120m2/g, a heterogeneous porous structure and a total pore volume of 0.28-0.34cm3/g with the high mechanical strength of pellets.

    Carriersbasedonzirconiumoxide. A carrier based on zirconium oxide with a melting point of 2700℃ can be promising for creating a catalyst. Two modifications of ZrO2are known: monoclinic and tetragonal. The monoclinic modification is stable up to 1000℃, and at higher temperatures, it reversibly passes into the tetragonal modification. Therefore, despite the high thermal stability, at temperatures above 1000℃, the carrier based on it may undergo changes in the specific surface, porous structure and mechanical strength. Nevertheless, due to the high activity of ZrO2in the N2O decomposition reaction, this carrier is of considerable interest in research.

    In our opinion, a zirconium carrier, where aluminum hydroxide is used as a binding agent, can be more promising. The carrier obtained in this way is a mixture of Al2O3-ZrO2. This high-temperature carrier has a developed specific surface, a porous structure, and a sufficiently high mechanical strength. In addition to the above carriers, carriers based on aluminum oxides with silicon oxide may be of interest.

    Based on the above, we selected the following carriers for research:

    (γ+θ+α) -Al2O3;CaO-Al2O3;Al2O3/AlN;ZrO2;ZrO2-Al2O3;SiO2-Al2O3

    (2) Choosing promising active components

    Metals. The analysis of the properties of the most promising metals to create the N2O decomposition catalyst showed[2]that almost all of them will be oxidized during the reaction, depending on the temperature of the catalyst under the action of the released oxygen. The platinum group metals Pt, Rh, and Ir will have the lowest exposure to O2. Their oxidation temperature in a highly dispersed form is above 700℃. It should be noted that, at temperatures above 1000℃, the formed oxides will dissociate into Me and O2. Palladium and ruthenium are oxidized at a lower temperature from 500-600℃. All other metals are oxidized up to a temperature of 400℃. Therefore, during a test of any supported metal catalyst, the active component will turn into an oxide. However, it is of interest to determine the activity of the catalyst, where the metals of the Pt group with different Me content will be used in the initial form as the AC. Such metals are: Rh, Ir, Pt, Ru, and Pd.

    Oxides. It is known from the analysis of the literature data[2]that such oxides of transition metals of group VIII as Rh, Ir, Co, Fe, and Ni show the greatest activity in the N2O decomposition reaction; the onset temperature of the reaction based on them is 200-400℃. The oxides of Cu, Mn, W, Mo, and Cr show a slightly lower activity; the minimum reaction temperature on such catalysts is 400-500℃. In terms of their activity as well as thermal and chemical stability in the temperature range of 400-1000℃, the oxides of the above metals are of interest for research to determine the possibility of developing the N2O decomposition catalyst based on them (including their mixtures) for operation in a micro-engine with a thrust of 1 N.

    Thus, for the development of the supported catalyst, the requirements for the carrier are formulated and some carriers are selected, based on which the N2O decomposition catalyst can be created. These carriers include high-temperature aluminum oxide carriers containing θ-form and stabilized with calcium oxide, aluminum nitride carriers, zirconium oxide carriers, and aluminum and silicon oxide carriers.

    Oxides of the following metals were selected as active components to search for the catalyst composition at the first stage: Rh,Ir, Co, Ni, Fe, Cr, Mn, Cu, Pt, Pd, and Ru.

    2 Methods to study the physical and chemical as well as catalytic properties of catalysts

    2.1 Methods to determine physical and chemical properties

    To study the physical and chemical properties of catalysts, we used the following methods:

    (1)Thetotalspecificsurfaceareaof the samples was determined by a chromatographic method based on changes in the volume of argon absorbed by the catalyst surface from the flow of a gas mixture with helium of a given concentration (volume ratio 5%-7%) at the temperature of liquid nitrogen and its subsequent desorption when the temperature increased to 25-30℃.

    (2)Thepourdensitywas determined by measuring the volume of the vibro-packed catalyst sample weight and calculated as the sample weight/volume ratio.

    (3)Thetotalporevolumewas determined by the volume of distilled water absorbed by a certain weight of the sample during its “titration” and calculated as the ratio of the absorbed liquid volume to the sample weight.

    (4)Thespecificsurfaceareaof metals and their dispersion were determined by gas chromatography during oxygen-hydrogen titration of the catalyst surface.

    (5)Theamountoftheactivecomponentadded to the catalyst was determined by the calculation method based on the difference between the weight of the taken carrier and the weight of the finished catalyst.

    (6)Theporousstructureof carrier samples was studied by mercury porosimetry.

    (7)Thephasecompositionwas studied by X-ray diffraction method.

    2.2 Method to determine the catalyst activity in the N2O decomposition reaction

    To determine the catalyst activity, it was required to develop some new methods.

    2.2.1 Determining the activity by the minimum onset temperature of the reaction in a flow-through unit

    One of the main tasks was to create a highly active and thermally stable N2O decomposition catalyst that would initiate the decomposition process in the engine with minimum external energy consumption. The minimum onset temperature of N2O decomposition was taken as a measure of the catalytic activity, with chromatographic analysis of its decomposition products. The method for determining this indicator makes it possible to determine the activity of the studied samples and choose the most promising ones for more detailed research and development of the catalyst composition based on them. Fig. 2 shows the layout of a flow-through unit used to determine the activity of catalysts.

    The operation of the installation is carried out in three stages:

    (1)Stage 1-preparation for testing.

    (2)Stage 2-testing.

    (3)Stage 3-bringing the installation to its original position (end of tests).

    Below is a description of the operation of the installation at stage 2-testing.

    The catalyst in the amount of 10cm3(layer height of 25-30mm) with a grain size of 0.8-1.25mm was loaded in reactor 18, which is a quartz tube with a false bottom. The amount of catalyst that was selected when varying the sample weight from 5 to 15cm3makes it possible to determine the onset temperature of the reaction most accurately. In our opinion, the reactor diameter (~18mm) and the volume of the catalyst loaded into the reactor will be close to the parameters of the engine being developed. Pure nitrous oxide was used as the working medium, which made it possible to simulate the operation of the catalyst in the engine, as well as determine the beginning of decomposition more accurately since the use of pure nitrous oxide produces a much greater amount of heat per unit of time than when its mixtures aredecomposed.

    To create the conditions for the reaction in a reactor with ideal displacement and heating of the working gas flow (N2O) entering the catalyst, we poured 10cm3of quartz glass pellets with a size of 2-3 mm onto the catalyst layer, having previously found out that the fraction of decomposed N2O on the quartz is insignificant up to a temperature of 600℃.

    Fig. 2 Layout of a flow-through unit for determining the activity of the catalysts in N2O decomposition: 1, 2-cylinders; 3, 4-reducing units; 5, 6, 7-gas flow adjusters; 8, 9-manostats; 10, 12, 14-flowmeters; 11-mixer; 13-multi-way valve; 17, 23-valves; 18-reactor with a heater; 21-controller recorder; 24, 25-desiccators; 20, 26-thermostats; 22-control trap

    The temperature in the middle of the catalyst layer was measured with a chromel-copel thermocouple installed directly in the layer (when determining the activity up to 600℃) or a chromel-alumel thermocouple (when heating the catalyst to 1200℃).

    The reactor, on the outer surface of which achromel-alumel thermocouple was fixed in the catalyst zone for automatic control of its heating rate, was placed in a cylindrical furnace. After installing the reactor, gas lines were connected to it. After checking the unit for tightness, which was determined by changes in the pressure of supplied helium in the system, nitrous oxide was supplied to it. The N2O flow rate through the reactor was 100cm3/min (0.0033g/s), which was selected when changed from 80 to 170cm3/min. The gas from the cylinder, passing through flow meter 10, mixer 11, desiccator 24 for moisture sorption, entered the reactor. From the reactor, the gas was released into the atmosphere after passing desiccator 24 and a chromatograph. After setting the flow rate of nitrous oxide, the reactor heating was switched on. The heating rate was 5deg/min and it was automatically maintained throughout the experiment by voltage thermostat 26. As the reactor was heated, every 20℃ (every 4minutes), the composition of the exhaust gases was determined chromatographically. At the first stage of research, when the most active components were selected for the development of the catalyst composition, the maximum heating temperature of the reactor was 600℃. After reaching 600℃ (the first determination of activity), the reactor heating was automatically switched off, and it was cooled. As the cooling process progressed, the exhaust gases were analyzed every 5minutes to determine the decomposition reaction end temperature. After cooling the reactor to a temperature of 100℃, the heating was switched on and the catalyst activity was re-determined as described above (second determination). The activity of compact metal catalysts was determined at the same facility, where the activity of pellet catalysts was determined, but in that case a model reactor with a diameter of 10 mm was used. The temperature, at which the appearance of oxygen and nitrogen was observed in the composition of the exhaust gases, was taken as the minimum onset temperature of the reaction.

    Based on the data on the gas medium composition, we calculated the degree of decomposition depending on the heating temperature of the catalyst and determined the kinetic characteristics of the studied carriers and catalysts to the degree of N2O decomposition equal to 0.3.

    To determine the kinetic characteristics, we used first-order equation (2), which was transformed into equation (3) by integration and resolution with respect tokas well as Arrhenius equation (4).

    dx/dτ=k(1-x)

    (2)

    k=1/τ·ln[1/(1-x)]

    (3)

    k=k0·е-E/RT,

    (4)

    where:kis the rate constant, cm3/g·s;τis the contact time expressed as the ratio of the catalyst weight to the N2O volume flow rate, reduced to the catalyst temperature, g·s/cm3;k0is the pre-exponential multiplier, cm3/g·s;Eis the activation energy of the catalytic process, J/mol;Ris the universal gas constant equal to 8.315J/mol·K;Т is the catalyst temperature, K;xis the degree of N2O decomposition, calculated based on the experimental data of chromatographic analysis, according to the following equation:

    x =CN/(100% -1/2·CN)

    (5)

    where:CNis the nitrogen concentration, %; 1/2·CNis the oxygen concentration expressed in terms of nitrogen concentration (ratio of the nitrogen concentration to the oxygen concentration in N2O decomposition products is 2), %.

    By using experimental valuesτandx, we calculated the rate constant based on equation (3). The pre-exponential multiplier and activation energy were calculated based on the obtained values of the rate constant and catalyst temperature using equation (4) and the least-squares method. To compare the catalytic activity of the studied carriers and catalysts, the rate constants were calculated at a certain temperature.

    2.2.2 Determining the activity by the minimum onset temperature of the reaction in a differential reactor

    The N2O decomposition reaction is accompanied by the release of a significant amount of heat. However, to initiate this process, the catalyst should be heated to a certain temperature at which the reaction begins. For its determination, we for the first time applied the differential method widely used in the study of solids. The onset temperature of the catalytic reaction in the catalyst layer was determined using a differential thermocouple by comparing the temperatures in the catalyst layer and the inert carrier, through which N2O was passed. The beginning of the reaction is indicated by the deviation of the controller recorder line from the zero value.

    As the heating temperature of the catalyst and the carrier increases, the degree of N2O decomposition will increase as well, which is accompanied by an increase in the catalyst layer temperature and, therefore, a large deviation from the zero line. As the temperature rises in the catalyst layer, the conditions, under which N2O is completely converted into reaction products, are reached. As soon as these conditions are reached, the rate of temperature rise in the catalyst layer should become constant and the recorder will show a straight line. The observed temperature differences in the layer of the catalyst and the inert carrier depend on the rate of heat supply to the reactor: at a high rate, the deviation from the zero line is observed more clearly.

    The layout of the unit for such studies differs from the layout of the reactor considered above. It is shown in Fig.3. The unit represents a quartz tube with a false bottom, which is divided by an impermeable quartz partition into two cells. An inert carrier (in our case, quartz glass pellets) with a size of 0.8-1.25mm and a weight of 5 g is placed in one cell, and the same amount of the studied catalyst of the same fractional composition is placed in another cell. In the middle of the layer of the inert carrier and the catalyst, a differentialchromel-copel thermocouple is installed, connected to the recording device. The reactor is installed in a furnace, the temperature of which can be increased at a given rate (in our case, 10deg/min) by means of an automatic regulator. Then the reactor is connected to the gas lines. The unit is checked for tightness under the pressure of helium, which is pre-fed into the system. After checking the tightness, the helium is replaced with N2O and the unit is purged with nitrous oxide at a rate of 100cm3/min, which passes after the reactor through the chromatograph and is released into the atmosphere. Then, the reactor heating is switched on; as the temperature rises, the composition of the exhaust gases is determined every 5minutes. The beginning of the reaction is recorded by the deviation of the controller recorder and confirmed by the data of chromatographic analysis. A typical thermogram of the process is shown in Fig. 4.

    This method was used to confirm the data on the reaction onset temperature obtained in a flow-through unit since it did not allow for the determination of the decomposition degree (and, therefore, kinetic parameters of the process) due to the passage of a part of N2O through the inert carrier layer.

    Fig. 3 Layout of a reactor with a differential thermocouple

    Fig. 4 Thermogram for determining the beginning of the decomposition reaction using a differential thermocouple: 1-differential curve, 2-sample heating curve

    3 Results of the experimental determination of catalyst properties

    3.1 Activity of compactmetal catalysts

    3.1.1 Conditions of sample preparation

    To obtain compact metal catalysts of the “metal rubber” type, the following precursors were selected in the form of a wire with a diameter of 0.2mm:

    (1)Pl-99 platinum;

    (2)PlRd-10 platinum-rhodium alloy (10% Rh);

    (3)PlI-10 platinum-iridium alloy (10%Ir);

    (4)Np-2 nickel;

    (5)N80Kh20 nickel-chrome alloy (20% Cr).

    Catalyst samples in the form of porous briquettes were made by pressing workpieces from a wire spiral of each material, specially laid in press-dies with a diameter of 10mm. The conditions of workpiece pressing were selected so that the height of the briquette would be 20mm. The length of the wire for the manufacturing of a single sample in all cases was equal to 8m. This technology made it possible to obtain samples with the same surface (determined by the diameter and length of the wire) and the same porosity (determined by the height of the briquette and the pressing force). Before the test, a recess was made in the center of the metal briquettes to a depth of 10mm to install the thermocouple.

    3.1.2 Results of the experimental determination of activity. Activity series

    All test samples were subjected to heat treatment in the air at a temperature of 600℃ for 3 hours before the test. The platinum-based briquettes did not change by color or by weight. The annealing colors, which indicate the formation of a thin oxide film on the surface of the wire, appeared on the nichrome briquettes. However, the briquette weight did not change. And only the nickel-based briquettes underwent significant changes: their metallic color turned green, and the briquette weight increased by 1.5%. It indicates the wire oxidation.

    The activity of the prepared samples was determined by the method described above; the final temperature of sample heating in the N2O flow was 800℃, i.e. below the onset temperature of homogeneous decomposition. It was found that the metal catalysts are arranged in the following series according to the onset temperature of the N2O decomposition process:

    Nickel(510℃)>Pt, Pt-Rh, Pt-Ir (~560℃)>nichrome (710℃).

    The N2O decomposition degree at 800℃ was as follows: for nickel -0.34; for Pt and its alloys with Rh and Ir -0.26, for nichrome -0.03, i.e. the lowest decomposition rate was observed with nichrome.

    An examination of the catalysts after testing showed that the platinum-based samples did not change their color, although there was some weight loss (~0.1%).

    The nichrome-based samples turned green; their weight increased, indicating the wire surface oxidation.

    The most significant changes were observed in the nickel-based samples: they turned green and their weight increased by 4.5%. It indicates the significant oxidation of the nickel wire. Therefore, the relatively high activity of nickel-metal catalysts can be explained by the formation of nickel oxide, which shows noticeable activity in the N2O decomposition reaction.

    Thus, for the output layer catalysts, we can recommend platinum-based catalysts, which are active in the reaction under consideration and almost do not undergo significant changes up to 800℃.

    3.2 Experimental studies and selection of carriers for catalysts

    It is known that the carriers in the supported catalysts are quite inert themselves. However, they cannot be considered only as a mechanically strong heat-resistant framework with a developed specific surface area and a certain porous structure. According to some studies[2], the nature and properties of the carrier significantly affect the activity of the supported catalyst: they can increase or decrease the activity, or interact with the active component to form a chemical compound. At the first stage of carrier selection for research, the most promising heat-resistant carriers of the following composition were selected:

    (1)aluminum oxide stabilized by Ca compounds (Al2O3-CaO,Tcalc—1100℃);

    (2)aluminum nitride coated with γ-Al2O3(Al2O3-AlN framework carrier,Tcalc—650℃);

    (3)zirconium oxide (ZrO2,Tcalc—1100℃);

    (4)zirconium oxide-aluminum oxide (Al2O3-ZrO2,Tcalc—800℃);

    (5)aluminum-silicon oxide (Tcalc—1100℃);

    (6)aluminum oxide (calcined, α-Al2O3,Tcalc-more than 2000℃):

    (7)aluminum oxide (heat-resistant, γ+θ+α-Al2O3,Tcalc—750℃);

    (8)quartz (SiO2,Tcalc—1200℃).

    The study of the physical and chemical properties of carriers showed (Table 1) that they differ significantly both in their specific surface area (from 110 to 1m2/g), and in their total pore volume (from 0.7 to 0.1cm3/g), and, hence, in their porous structure.

    Table 1 Physical and chemical properties of various high-temperature carriers

    To assess their possible contribution to the catalyst activity, the activity of these carriers in the N2O decomposition reaction was determined using the method described above. Fig. 5 shows the Arrhenius dependencies for some carriers, calculated by a first-order equation.

    Table 2 provides data describing the catalytic activity of carriers, which shows that they have a very long induction period. By the onset temperature of the reaction, the studied carrier samples can be arranged in the following series:

    ZrO2> Al2O3-CaO>Al2O3-ZrO2>Al2O3-AlN>θ-Al2O3>Al2O3-SiO2>SiO2>α-Al2O3

    As can be seen, the carrier based on zirconium oxide is the most active. The reaction of N2O decomposition on it begins at 280℃. The least activity was shown by the carrier, which is aluminum oxide calcined at a temperature above 2000℃, having a specific surface area of 0.5m2/g. The reaction of N2O decomposition on it begins only at 460℃.

    Fig. 5 Dependence of lnk on the temperature for various sample carriers in the N2O decomposition reaction

    From Table 2, it is also seen that the activation energy on the carrier samples varies widely: from 100 (Al2O3-CaO) up to 185kJ/mol (Al2O3-AlN). Therefore, when moving to higher temperatures, the activity series should change. It is confirmed by the calculated data for the rate constant at 900℃. It can be seen that at this temperature, the carriers in the N2O decomposition reaction are arranged (in terms of activity) in the following series:

    Al2O3-SiO2>Al2O3-AlN>ZrO2>Al2O3>Al2O3-ZrO2>Al2O3-CaO>α-Al2O3>SiO2

    It should be noted that since the catalyst weight is taken into account when calculating the rate constant, the carrier with the lowest pour density (Al2O3-SiO2) becomes the most active.

    Thus, based on the obtained results, the most promising carriers are the following:

    (1)Aluminum oxide carrier, based on which a series of catalyst samples was prepared for the first stage of work;

    (2)Carriers based on Al2O3- ZrO2and Al2O3-AlN.

    Despite its high activity in the N2O decomposition reaction, the zirconium oxide carrier is not of practical interest due to the destruction of catalysts during preparation and its scarcity.

    A test sample of the Al2O3-SiO2composition, which showed high activity in the N2O decomposition reaction, deserves consideration.

    Table 2 Properties of carriers in the N2O decomposition reaction

    3.3 Activity of supported metal and oxide catalysts

    3.3.1 Conditions for the preparation of supported single-component catalysts and their properties

    To obtain catalysts using a ready-made carrier, we selected the method of repeated dip ensuring the full absorbency. The size, shape and porous structure of the catalyst are set by the carrier, which is important to ensure the reproducibility of the catalyst properties. In addition, this method makes it possible to use the AC to the maximum extent, whereas, in deposited catalysts, its part is shielded by the carrier and is not available for reagents. When the carrier is dipped, the pore volume filling is carried out due to capillary forces and completed in a very short time. The amount of the AC added to the catalyst depends on the total pore volume of the carrier and the concentration of the dipping solution. To obtain highly concentrated catalysts (more than 5% AC), several dips are carried out. Before each next dip, the dipped carrier is heat-treated to remove the solvent from the carrier pores and convert the AC salt to an insoluble state. The number of dipping / heat treatment cycles is repeated until the required amount of the AC is applied. To reduce the number of dips, heat treatment can be carried out in a hydrogen atmosphere, as a result of which the AC is reduced to metal.

    To obtain comparative data on the activity of various metals and oxides, all the studied samples were prepared using a single batch of the high-temperature aluminum oxide carrier, which was a mixture of (γ+θ+α)-Al2O3in terms of phase composition. At the final temperature of heat treatment up to 750℃, it had a specific surface area of 110m2/g, a total pore volume of 0.34cm3/g, a heterogeneous porous structure with a set of micro-, macro-, and transport pores. Its porous structure is shown in Fig. 1 (sample No. 2). For the preparation of samples, a carrier of a rounded shape with a pellet size of 0.8-1.25mm was used.

    Solutions of the following compounds were taken as the initial AC salts: H2PtCl6; PdCl3, Pd(NO3)2; RhCl3; RuOHCl3; H2IrCl6; Cu(NO3)2; Co(NO3)2; Ni(NO3)2; H2CrO4; Mn(NO3)2, Fe(NO3)3.

    The AC content in the prepared catalysts varied from 3.5 to 36%. The high initial AC concentration in the catalyst is due to the fact that a part of the AC (up to 5%) can interact with the carrier during the preparation of the catalyst (especially during heat treatment). The observed interaction is especially typical for metals of the iron subgroup. It leads to a loss of catalyst activity. The preparation of catalysts in such a wide range of concentrations is due to the fact that the activity with an increase in the AC content for many reactions passes through the maximum, which has its own value for each AC. Therefore, to develop the catalyst composition, it is necessary to determine the optimal AC concentration. Heat treatment of the dipped carriers was carried out at a temperature of 300-350℃. After the application of the set amount of the AC, the platinum group metals were reduced at a temperature of 400-450℃. Table 3 shows the physical and chemical properties of the prepared samples.

    To bring all samples to the same initial state, they were subjected to heat treatment in the air at a temperature of 600℃ for 3 hours before testing.

    Table 3 Physical and chemical properties of the prepared samples of supported catalysts

    3.3.2 Results of the experimental determination of single-component catalyst activity

    Following the selected method, each catalyst sample was pre-heated in the air at 600℃ for 3 hours and then it was exposed to N2O for 5 hours during the experiment. During the first two hours, the degree of N2O conversion was determined in the mode of programmable heating of the furnace from 20 to 600℃ (first determination). Then the activity of the sample in the mode of free cooling to temperatures of 100-200℃ (with no reaction) was determined, and then, the programmable furnace heating was switched on again, and the dependence of the N2O decomposition degree on the temperature (second determination) was determined again for the same sample both during heating and cooling.

    The study of the activity of the prepared catalysts showed (Table 4 and Fig. 6) that in the continuous heating mode, the curve of the dependence of the N2O decomposition degree on the temperature has a clear S-shape. It means that the induction period of the decomposition process is observed at a relatively low temperature.

    Fig. 6 Dependence of the N2O decomposition degree on the temperature for the following samples: Rh2O3/Al2O3; Cr2O3/Al2O3;ZrO2

    With a further increase in the temperature, the rate of conversion increases sharply. When the decomposition degree reaches 0.9, it begins to change much more slowly as the temperature increases. For most samples, the induction period was overlong, which made it difficult to determine the onset temperature of the reaction accurately. Therefore, a temperature, at which the decomposition degree reaches the value of 0.05, was adopted for the comparison. The comparison of the activities of the supported catalysts showed that the samples prepared based on Pt-group metals that were subjected (like all the studied ones) to standard pre-treatment (3 hours, 600℃, in the air) were more active than the catalysts prepared based on other transition metals (Figs. 6 and 7). Therefore, these two groups of catalysts will be considered separately below.

    CatalystsbasedonPt-groupmetals

    As can be seen from the data presented in Table 5 in order of ascending temperature values, at which the degree of N2O decomposition on the catalyst reaches the values of 0.05 and 0.2 (for comparison, the catalysts containing 13%-15% AC were selected), the activity of the samples is higher at the second determination. According to thermal gravimetric studies, this is due to further oxidation of the metal surface, i.e. the activity of Pt-group metal oxides is higher than that related to pure metals.

    The comparison of data on the activity of various catalysts in the N2O decomposition reaction made it possible to arrange the studied samples in the following series:Rh>Ru>Ir>Pt>Pd.

    The obtained series was confirmed experimentally by the differential method.

    Table 4 Activity of various active components applied to the aluminum oxide carrier in the N2O d ecomposition reaction (second heating)

    Rhodium (15%Rh/Al2O3), as the most active metal, begins to decompose N2O at 250℃, and at 320℃, the decomposition degree reaches a value of 0.05 (first determination). At a temperature of 350℃, the N2O decomposition degree reaches 20%. At re-starting, N2O decomposition begins at 200℃, and the decomposition degree of 0.05 and 0.2 is reached at 260 and 305℃, respectively.

    The experiments showed that Pd is the least active of Pt-group metals. The decomposition reaction based on it (first determination) begins at a temperature of 360℃, and the decomposition degree of 0.05 is reached at 455℃. In a repeated experiment, the initial decomposition temperature decreases by 50℃ and the decomposition degree of 0.05 is reached at 420℃ (Tables 4 and 5). The obtained results are confirmed by data on the activation energy (E) and pre-exponential multiplier (K0), which were calculated by the decomposition degree up to 0.3 at a temperature of 350℃ and not complicated by autocatalysis processes. To compare the catalysts by the degree of their activity, an intermediate temperature of 500℃ was selected, for which, using experimental data onEandK0, the value of the rate constantK500was calculated with the Arrhenius equation.

    As can be seen from Table 5, the studied catalysts differ in these indicators significantly. The activation energy value for the studied catalyst samples is in the range from 174kJ/mol (for Pd) to 118 kJ/mol (for Ir). The comparison of the activation energy values, obtained under the conditions of the first and second experiments,and data on changes in the weight of the sample during the tests allows us to conclude that the oxidation of the catalyst surface leads to a decrease in the activation energy. For a rhodium catalyst, a decrease in the activation energy by 60 kJ/mol leads to the fact that already at 260℃ the degree of N2O decomposition on a “trained” (oxidized) sample reaches the value ofx=0.05, and at 305℃ -0.2 (second determination). The same behavior is typical for all platinum metals. For a ruthenium catalyst, a decrease in the activation energy after training in N2O is 90kJ/mol. Accordingly,the onset temperature of the decomposition reaction decreases by 100℃.

    The study of the influence of Pt-group metals concentration on the activity showed (Table 4) that the maximum activity is achieved when their content is different in the catalyst. Thus, Ir catalysts are characterized by a continuous increase in activity up to an increase in the AC content up to 36%.

    Fig. 7 Dependence of ln k on the temperature for the following samples: Rh2O3/Al2O3;Cr2O3/Al2O3;ZrO2

    Table 5 Activity of supported catalysts based on platinum group metals in the N2O decomposition reaction; first and second determinations; AC content (13%-15%); carrier-aluminum oxide

    For Rh catalysts, the maximum activity is reached at the values of up to 20% AC, and it does not depend much on the AC concentration. It should be noted that according to the results of Rh spectral analysis, the catalysts contained copper impurities, which were apparently introduced into the catalyst from the original AC salt. Removal of copper compounds by washing with weak nitric acid increased the catalyst activity significantly. It seems that this abnormal behavior of rhodium catalysts with an increase in the Me concentration is due to the presence of Cu impurity, which, as shown by spectral analysis methods, is located on the catalyst surface and, thus, blocks its activity.

    We also determined the influence of the initial salt on the activity of palladium catalysts: the catalysts prepared from the palladium nitrate are more active than those obtained from the palladium chlorides. The maximum activity of Ru samples (Table 6) is observed in a sample containing 7% AC. At the second determination, the onset temperature of decomposition is 220℃, and at 270℃, the decomposition degree reaches 0.2. Pt-containing catalysts are characterized by a slight increase in activity: the onset temperature of decomposition decreases by 20℃ with an increase in the AC concentration from 5 to 13%.

    Table 7 shows the physical and chemical properties of the catalyst samples after their testing in N2O. Since the final temperature of aluminum oxide carrier heat treatment is 750℃, tests in N2O up to a temperature of 600℃ did not significantly affect the value of the total pore volume and specific surface area, while the pour density increased slightly, which indicates the oxidation of the AC.

    Table 6 Influence of metal (Ru, Pt) concentration on the catalyst activity in the N2O decomposition reaction

    Table 7 Physical and chemical properties of the supported catalysts before and after testing in the N2Odecomposition reaction; AC content 13%-15% wt; carrier-aluminum oxide

    Catalystsbasedonmetaloxides

    Transition metal (Co, Ni, Mn, Cu, Cr, Fe) oxides are quite active in the N2O decomposition reaction and have high thermal and chemical stability[2]. To select the AC catalyst, we prepared a series of oxide catalysts containing up to 30% AC in terms of metal on the same aluminum oxide carrier as the Pt-group catalysts. As the test results showed, the behavior of oxide catalysts is fundamentally different from the behavior of catalysts based on platinum group metals: for example, their activity does not increase after the first experiment in N2O up to a temperature of 600℃. The activation energy from experiment 1 to experiment 2 almost does not change, which allows us to conclude that the phase composition of the catalyst surface is constant, which is confirmed by the data on the properties of the catalyst after the test (Table 7). The exception is a sample based on manganese oxide. After the first experiment in N2O, its activation energy decreases by 30 kJ/mol, thus, resulting in an increase in the onset temperature of the decomposition reaction by 15℃.

    Table 8 presents experimental values of the activity of the catalysts in the N2O decomposition reaction (experiment 2), which shows that by the minimum onset temperature of N2O decomposition, the oxides can be arranged in the following series:

    Co3O4(415℃)

    Table 8 Activity of metal oxides applied to the aluminum oxide carrier in the N2O decomposition reaction

    The highest activation energy is observed in samples based onCuO and Cr2O3(187-176kJ/mol), followed by a catalyst based on Fe2O3(163kJ/mol); activation energies for samples based on MnO2, NiO and Co3O4are close to each other (133-143kJ/mol). Therefore, when moving to higher temperatures, the activity series changes slightly. And already at 500℃, we get the following sequence (the value of the rate constant correlates to the temperature, at which the degree of conversion reaches 0.2):

    CuO>MnO2, Co3O4,Cr2O3>NiO>Fe2O3

    Thus, in terms of activity in the N2O decomposition reaction, the studied supported oxide catalysts are inferior to samples based on rhodium, iridium, and ruthenium. It seems that their activity is largely determined by the properties of the aluminum oxide carrier.

    4 Conclusion

    Oxides of the following metals were selected as active components for bench testing of the composition of the supported catalyst in a simulated engine: Rh,Ir, Co. It is recommended to use the following carriers as catalyst carriers: Al2O3-SiO2; Al2O3-AlN; ZrO2; Al2O3. Pt and its alloys with Rh and Ir, as well as Ni and its alloy with chromium (nichrome) in the form of a wire are recommended as precursors for catalysts of the “metal rubber” type in the output layer. In the future, it is recommended to produce enlarged samples of the selected catalytic systems for bench testing of simulated engines. After the tests, it is required to conduct a comprehensive examination of the tested catalyst samples to finally select catalyst formulation and composition.

    Conflictofinterest

    The author confirms that the provided information contains no conflicts of interest.

    亚洲国产精品sss在线观看| 亚洲av第一区精品v没综合| 欧美三级亚洲精品| 可以免费在线观看a视频的电影网站| 亚洲精品美女久久久久99蜜臀| 成人永久免费在线观看视频| 精品久久久久久久久久久久久| 欧美成狂野欧美在线观看| 亚洲性夜色夜夜综合| 又粗又爽又猛毛片免费看| 成人18禁在线播放| 丝袜人妻中文字幕| 午夜福利免费观看在线| 色噜噜av男人的天堂激情| 国产在线精品亚洲第一网站| 性欧美人与动物交配| 久久人妻av系列| 亚洲国产精品久久男人天堂| 国产区一区二久久| 亚洲欧美精品综合久久99| 国产日本99.免费观看| 亚洲色图av天堂| 国产麻豆成人av免费视频| 国内毛片毛片毛片毛片毛片| 亚洲av电影在线进入| 国产精品一及| 99精品欧美一区二区三区四区| 女生性感内裤真人,穿戴方法视频| 国产精品,欧美在线| 一进一出抽搐gif免费好疼| 欧美日韩国产亚洲二区| 日韩欧美在线二视频| 欧美成狂野欧美在线观看| 极品教师在线免费播放| 免费高清视频大片| 午夜影院日韩av| 国产视频一区二区在线看| 午夜精品一区二区三区免费看| 午夜激情福利司机影院| 亚洲国产欧洲综合997久久,| 国产亚洲av高清不卡| 91大片在线观看| 蜜桃久久精品国产亚洲av| 久久草成人影院| 成人三级做爰电影| 久久性视频一级片| 又大又爽又粗| 五月玫瑰六月丁香| 一进一出抽搐gif免费好疼| 亚洲av片天天在线观看| 91国产中文字幕| 日本精品一区二区三区蜜桃| 色哟哟哟哟哟哟| 丁香六月欧美| 好男人在线观看高清免费视频| 久久久水蜜桃国产精品网| 久久久国产成人精品二区| 色播亚洲综合网| 亚洲黑人精品在线| 亚洲成人中文字幕在线播放| 亚洲人成网站在线播放欧美日韩| 好看av亚洲va欧美ⅴa在| 成人欧美大片| 成人三级做爰电影| 久9热在线精品视频| 亚洲七黄色美女视频| 国产免费av片在线观看野外av| 亚洲中文字幕一区二区三区有码在线看 | www.www免费av| 午夜福利免费观看在线| 亚洲全国av大片| 亚洲av成人一区二区三| 国产单亲对白刺激| 欧美成狂野欧美在线观看| 好男人在线观看高清免费视频| 一个人免费在线观看电影 | 少妇粗大呻吟视频| 黄色 视频免费看| www.自偷自拍.com| 人妻夜夜爽99麻豆av| 在线a可以看的网站| 免费无遮挡裸体视频| 搡老熟女国产l中国老女人| 成人一区二区视频在线观看| xxx96com| 最新美女视频免费是黄的| 国产久久久一区二区三区| 狂野欧美白嫩少妇大欣赏| 麻豆av在线久日| 亚洲精品粉嫩美女一区| 999精品在线视频| 啦啦啦韩国在线观看视频| 欧美日韩一级在线毛片| 男女视频在线观看网站免费 | 在线观看日韩欧美| 最近最新中文字幕大全免费视频| 婷婷六月久久综合丁香| 久久精品夜夜夜夜夜久久蜜豆 | 国产三级黄色录像| 极品教师在线免费播放| 五月伊人婷婷丁香| 18禁观看日本| 日韩中文字幕欧美一区二区| 超碰成人久久| 亚洲av成人一区二区三| 成人18禁高潮啪啪吃奶动态图| 最新在线观看一区二区三区| 亚洲成人久久爱视频| 18禁裸乳无遮挡免费网站照片| 国产亚洲av嫩草精品影院| 操出白浆在线播放| 午夜免费激情av| 18美女黄网站色大片免费观看| 日日干狠狠操夜夜爽| 亚洲狠狠婷婷综合久久图片| 亚洲精品美女久久av网站| 香蕉av资源在线| 女人高潮潮喷娇喘18禁视频| 国产精品久久久久久久电影 | 亚洲七黄色美女视频| 亚洲七黄色美女视频| 亚洲狠狠婷婷综合久久图片| 久久香蕉国产精品| 九色成人免费人妻av| 美女大奶头视频| 香蕉av资源在线| 国产欧美日韩一区二区三| 午夜免费成人在线视频| 丁香欧美五月| 丰满人妻一区二区三区视频av | 老熟妇乱子伦视频在线观看| 丁香六月欧美| 不卡av一区二区三区| 国产伦一二天堂av在线观看| 国产熟女xx| 熟妇人妻久久中文字幕3abv| 亚洲成av人片在线播放无| 亚洲欧美日韩高清在线视频| 人人妻人人看人人澡| 国产熟女午夜一区二区三区| 免费搜索国产男女视频| 日韩高清综合在线| e午夜精品久久久久久久| 中出人妻视频一区二区| 狂野欧美激情性xxxx| av片东京热男人的天堂| 欧美色欧美亚洲另类二区| 日韩欧美在线二视频| 美女扒开内裤让男人捅视频| 成熟少妇高潮喷水视频| 国内久久婷婷六月综合欲色啪| 久久久久久久久免费视频了| 国产99久久九九免费精品| 男女那种视频在线观看| 99热这里只有精品一区 | 亚洲成人国产一区在线观看| 国产亚洲精品av在线| 老司机深夜福利视频在线观看| 亚洲午夜理论影院| 免费观看精品视频网站| 亚洲av中文字字幕乱码综合| 亚洲中文日韩欧美视频| 久久久久久久久中文| 手机成人av网站| 黄色成人免费大全| 身体一侧抽搐| 午夜影院日韩av| 草草在线视频免费看| 91麻豆精品激情在线观看国产| 黄片小视频在线播放| 国产又色又爽无遮挡免费看| www.999成人在线观看| 淫秽高清视频在线观看| 久久精品成人免费网站| 欧美成狂野欧美在线观看| 女警被强在线播放| 两个人看的免费小视频| 亚洲成a人片在线一区二区| 久久香蕉激情| 美女 人体艺术 gogo| 国产69精品久久久久777片 | 黄频高清免费视频| 母亲3免费完整高清在线观看| 亚洲欧美日韩高清专用| 亚洲男人的天堂狠狠| 中文字幕精品亚洲无线码一区| 免费在线观看成人毛片| 热99re8久久精品国产| 黄片大片在线免费观看| 在线看三级毛片| 精品第一国产精品| 亚洲午夜理论影院| 99国产精品一区二区三区| 亚洲熟女毛片儿| 亚洲精品一区av在线观看| av在线播放免费不卡| 一级a爱片免费观看的视频| 久久精品国产清高在天天线| 亚洲av成人av| av在线天堂中文字幕| 成人午夜高清在线视频| 精品欧美国产一区二区三| 久久精品成人免费网站| 男女视频在线观看网站免费 | 午夜成年电影在线免费观看| 看免费av毛片| 欧美日本视频| 国产精品免费视频内射| 久久欧美精品欧美久久欧美| 久久99热这里只有精品18| 亚洲人成77777在线视频| 免费看美女性在线毛片视频| 青草久久国产| 黄片大片在线免费观看| 亚洲人成伊人成综合网2020| 欧美国产日韩亚洲一区| www.熟女人妻精品国产| 日日爽夜夜爽网站| 国产99久久九九免费精品| 国产激情偷乱视频一区二区| 亚洲午夜精品一区,二区,三区| 精品福利观看| 人妻夜夜爽99麻豆av| 亚洲欧美日韩无卡精品| 两个人免费观看高清视频| 91成年电影在线观看| 国产成人影院久久av| 美女 人体艺术 gogo| 精品欧美一区二区三区在线| 国产av一区在线观看免费| 国产成人av激情在线播放| 一区二区三区国产精品乱码| 国产精品1区2区在线观看.| 妹子高潮喷水视频| 国产男靠女视频免费网站| 精华霜和精华液先用哪个| 精品国产美女av久久久久小说| 亚洲熟妇熟女久久| 欧美性猛交黑人性爽| 久久精品aⅴ一区二区三区四区| 1024香蕉在线观看| 欧美性猛交╳xxx乱大交人| 午夜免费激情av| 婷婷丁香在线五月| 国产成人精品久久二区二区免费| 亚洲国产高清在线一区二区三| 成人三级黄色视频| 黄色视频,在线免费观看| 真人一进一出gif抽搐免费| 又爽又黄无遮挡网站| 欧美久久黑人一区二区| 国产成人精品久久二区二区免费| 精品国产亚洲在线| 两个人免费观看高清视频| 亚洲七黄色美女视频| 可以在线观看的亚洲视频| 国产成人啪精品午夜网站| 亚洲一区二区三区不卡视频| 老熟妇乱子伦视频在线观看| 美女大奶头视频| 一级a爱片免费观看的视频| 欧美午夜高清在线| 精品乱码久久久久久99久播| 亚洲狠狠婷婷综合久久图片| 欧美成人性av电影在线观看| 午夜精品久久久久久毛片777| 成熟少妇高潮喷水视频| 欧美日本视频| 国产乱人伦免费视频| 亚洲成人中文字幕在线播放| 国产高清有码在线观看视频 | 一本精品99久久精品77| 人妻夜夜爽99麻豆av| 波多野结衣高清作品| 午夜老司机福利片| 色av中文字幕| 欧洲精品卡2卡3卡4卡5卡区| 日韩国内少妇激情av| 免费看a级黄色片| 色噜噜av男人的天堂激情| 人成视频在线观看免费观看| 国产高清videossex| 成人av一区二区三区在线看| 丝袜美腿诱惑在线| 蜜桃久久精品国产亚洲av| 亚洲一区二区三区色噜噜| 成在线人永久免费视频| 99久久精品国产亚洲精品| 天天一区二区日本电影三级| 91麻豆精品激情在线观看国产| 可以在线观看的亚洲视频| 国产伦在线观看视频一区| 精品久久久久久,| 亚洲aⅴ乱码一区二区在线播放 | 精品电影一区二区在线| videosex国产| 亚洲第一欧美日韩一区二区三区| 精品少妇一区二区三区视频日本电影| 国产欧美日韩精品亚洲av| 99久久精品国产亚洲精品| 激情在线观看视频在线高清| 欧美黄色片欧美黄色片| 久久这里只有精品19| 激情在线观看视频在线高清| 丰满人妻一区二区三区视频av | 亚洲人成网站在线播放欧美日韩| 亚洲av美国av| 一级作爱视频免费观看| 欧美乱码精品一区二区三区| 色噜噜av男人的天堂激情| 一本久久中文字幕| 国产激情欧美一区二区| 2021天堂中文幕一二区在线观| 日韩av在线大香蕉| 亚洲人成网站高清观看| 18禁观看日本| 久久香蕉国产精品| 亚洲欧美精品综合久久99| 精品不卡国产一区二区三区| 天堂动漫精品| 亚洲人与动物交配视频| 色综合婷婷激情| 男人舔奶头视频| 欧美日韩乱码在线| www.精华液| 三级国产精品欧美在线观看 | 嫩草影院精品99| 老司机福利观看| 成年版毛片免费区| 五月玫瑰六月丁香| 国产成人aa在线观看| 国产亚洲精品综合一区在线观看 | 狂野欧美激情性xxxx| 午夜激情av网站| 长腿黑丝高跟| e午夜精品久久久久久久| 国产乱人伦免费视频| 美女黄网站色视频| 久99久视频精品免费| 欧美乱色亚洲激情| 久久亚洲精品不卡| 男插女下体视频免费在线播放| 久久久久久久久中文| www日本黄色视频网| 俺也久久电影网| 99国产精品99久久久久| 最好的美女福利视频网| 欧美zozozo另类| 中文字幕最新亚洲高清| 久久久久久人人人人人| 午夜亚洲福利在线播放| 国产av一区在线观看免费| 999久久久精品免费观看国产| 99国产综合亚洲精品| 婷婷丁香在线五月| 久久香蕉精品热| 一个人免费在线观看的高清视频| 午夜成年电影在线免费观看| 精品电影一区二区在线| 99国产综合亚洲精品| 亚洲国产精品久久男人天堂| 三级国产精品欧美在线观看 | 一本久久中文字幕| 亚洲一区二区三区不卡视频| 亚洲片人在线观看| 久久这里只有精品19| 精品国产亚洲在线| 中文字幕熟女人妻在线| 国产成人啪精品午夜网站| 久久精品国产清高在天天线| 午夜激情福利司机影院| 熟妇人妻久久中文字幕3abv| 香蕉av资源在线| 亚洲成a人片在线一区二区| 一二三四在线观看免费中文在| 国产精品九九99| 国产精品久久电影中文字幕| 妹子高潮喷水视频| 国内毛片毛片毛片毛片毛片| 国产久久久一区二区三区| 成人av一区二区三区在线看| 亚洲av熟女| 丁香六月欧美| 国产又色又爽无遮挡免费看| 真人一进一出gif抽搐免费| 欧美乱码精品一区二区三区| 丰满的人妻完整版| e午夜精品久久久久久久| 不卡一级毛片| 母亲3免费完整高清在线观看| 精品久久久久久久人妻蜜臀av| 久久这里只有精品中国| 老司机午夜十八禁免费视频| 欧美三级亚洲精品| 久久香蕉国产精品| 久久这里只有精品19| 久热爱精品视频在线9| 国内毛片毛片毛片毛片毛片| 久久国产精品人妻蜜桃| 日韩欧美精品v在线| 亚洲人与动物交配视频| 亚洲自偷自拍图片 自拍| 久久久水蜜桃国产精品网| 欧美另类亚洲清纯唯美| 午夜福利高清视频| 国产精品 国内视频| 9191精品国产免费久久| 他把我摸到了高潮在线观看| 在线观看免费午夜福利视频| 国产精品久久久久久久电影 | 国产亚洲精品av在线| 亚洲,欧美精品.| 国产高清videossex| 亚洲欧美日韩无卡精品| 国产麻豆成人av免费视频| 国产视频一区二区在线看| 久久久久久国产a免费观看| 国产片内射在线| 天天躁狠狠躁夜夜躁狠狠躁| 男插女下体视频免费在线播放| 亚洲va日本ⅴa欧美va伊人久久| 国产亚洲欧美在线一区二区| 天堂影院成人在线观看| 亚洲国产精品999在线| 狂野欧美白嫩少妇大欣赏| 中文亚洲av片在线观看爽| а√天堂www在线а√下载| 免费一级毛片在线播放高清视频| 香蕉av资源在线| 成人亚洲精品av一区二区| 999久久久国产精品视频| 嫁个100分男人电影在线观看| 亚洲最大成人中文| 国产精品日韩av在线免费观看| 亚洲欧洲精品一区二区精品久久久| 丁香欧美五月| 精品无人区乱码1区二区| 妹子高潮喷水视频| 99久久无色码亚洲精品果冻| 午夜日韩欧美国产| 黄片小视频在线播放| 亚洲精品国产一区二区精华液| 2021天堂中文幕一二区在线观| 一本一本综合久久| av免费在线观看网站| 日本a在线网址| 中文字幕av在线有码专区| 欧美黑人欧美精品刺激| 亚洲欧美日韩高清在线视频| 日韩国内少妇激情av| 国产精品自产拍在线观看55亚洲| 亚洲av熟女| 可以在线观看毛片的网站| 免费高清视频大片| 精品久久久久久久久久免费视频| 一区福利在线观看| aaaaa片日本免费| 黄色 视频免费看| 久久久精品欧美日韩精品| 国产1区2区3区精品| 国产精品综合久久久久久久免费| 午夜精品久久久久久毛片777| 国产一级毛片七仙女欲春2| 亚洲欧美日韩高清专用| 999久久久精品免费观看国产| 两性夫妻黄色片| 国产一区二区三区视频了| 亚洲一码二码三码区别大吗| 精品高清国产在线一区| videosex国产| 99久久99久久久精品蜜桃| 舔av片在线| 窝窝影院91人妻| 国产欧美日韩精品亚洲av| 淫妇啪啪啪对白视频| 国产精品香港三级国产av潘金莲| 国产日本99.免费观看| 国产精品免费视频内射| 性色av乱码一区二区三区2| 搞女人的毛片| 日日干狠狠操夜夜爽| 亚洲av中文字字幕乱码综合| 九九热线精品视视频播放| 在线国产一区二区在线| 久久香蕉国产精品| 国产探花在线观看一区二区| 亚洲成人国产一区在线观看| 国产片内射在线| 日韩精品免费视频一区二区三区| 首页视频小说图片口味搜索| 亚洲乱码一区二区免费版| 亚洲免费av在线视频| 日韩精品青青久久久久久| 99久久国产精品久久久| 两个人的视频大全免费| 国产真实乱freesex| 免费在线观看影片大全网站| 最近在线观看免费完整版| 在线观看www视频免费| 一本一本综合久久| 悠悠久久av| 在线观看日韩欧美| 午夜福利高清视频| 国产日本99.免费观看| 亚洲乱码一区二区免费版| 免费看日本二区| 精品久久久久久,| 久久久国产成人精品二区| 日韩欧美精品v在线| 成熟少妇高潮喷水视频| 国产高清videossex| 男女午夜视频在线观看| 99久久国产精品久久久| 国产爱豆传媒在线观看 | 可以在线观看毛片的网站| 波多野结衣高清作品| 免费在线观看日本一区| 久久精品影院6| 精品国内亚洲2022精品成人| 99久久无色码亚洲精品果冻| 欧美激情久久久久久爽电影| 69av精品久久久久久| 久久久久国产精品人妻aⅴ院| 日本免费a在线| 久久久久免费精品人妻一区二区| 国产精品自产拍在线观看55亚洲| 中文字幕av在线有码专区| a级毛片a级免费在线| 精品高清国产在线一区| 国产亚洲欧美在线一区二区| 天堂av国产一区二区熟女人妻 | bbb黄色大片| 成人国产一区最新在线观看| 非洲黑人性xxxx精品又粗又长| ponron亚洲| 国产麻豆成人av免费视频| 又粗又爽又猛毛片免费看| 1024手机看黄色片| 日本免费一区二区三区高清不卡| 欧美人与性动交α欧美精品济南到| 精品国产亚洲在线| 欧美日韩福利视频一区二区| 国产爱豆传媒在线观看 | ponron亚洲| 很黄的视频免费| 久久久国产欧美日韩av| 成年女人毛片免费观看观看9| 在线视频色国产色| 久久草成人影院| 在线观看一区二区三区| 日韩欧美在线二视频| 国产免费av片在线观看野外av| 成人亚洲精品av一区二区| 草草在线视频免费看| www.熟女人妻精品国产| 美女大奶头视频| 欧洲精品卡2卡3卡4卡5卡区| 91麻豆精品激情在线观看国产| 国产在线精品亚洲第一网站| 变态另类丝袜制服| 亚洲中文日韩欧美视频| 亚洲人成77777在线视频| 成人欧美大片| 亚洲国产欧洲综合997久久,| 国内久久婷婷六月综合欲色啪| 亚洲成人中文字幕在线播放| 亚洲欧美激情综合另类| 成人av一区二区三区在线看| av超薄肉色丝袜交足视频| 韩国av一区二区三区四区| 日韩欧美一区二区三区在线观看| 亚洲免费av在线视频| 亚洲精品中文字幕在线视频| 国产精品 国内视频| 无限看片的www在线观看| 天堂√8在线中文| 午夜成年电影在线免费观看| 一级a爱片免费观看的视频| 丰满人妻熟妇乱又伦精品不卡| 亚洲18禁久久av| 久久 成人 亚洲| 中文字幕熟女人妻在线| 熟妇人妻久久中文字幕3abv| 夜夜爽天天搞| 一级黄色大片毛片| 女警被强在线播放| 亚洲成人精品中文字幕电影| 久久这里只有精品19| 巨乳人妻的诱惑在线观看| 中文在线观看免费www的网站 | 国产成人aa在线观看| av中文乱码字幕在线| 亚洲精品国产一区二区精华液| 黄片小视频在线播放| 国产激情欧美一区二区| 精品国产乱码久久久久久男人| 国产黄片美女视频| 国产av又大| 男女午夜视频在线观看| 亚洲第一电影网av| 床上黄色一级片| 亚洲最大成人中文| 久久久久九九精品影院| 欧美+亚洲+日韩+国产| www国产在线视频色| 午夜免费观看网址| 天堂av国产一区二区熟女人妻 | 国产久久久一区二区三区| 国产精品一区二区三区四区久久| 在线观看舔阴道视频| 69av精品久久久久久| 妹子高潮喷水视频| 桃色一区二区三区在线观看| 国产又色又爽无遮挡免费看| 久久热在线av|