    Mesoscale fracture behavior of Longmaxi outcrop shale with different bedding angles:Experimental and numerical investigations

    2020-04-17 13:48:16JinpingZuoJingfngLuRojinGhndrizJintoWngYnhongLiXioynZhngJunLiHongtoLi

    Jinping Zuo ,Jingfng Lu ,Rojin Ghndriz ,Jinto Wng ,Ynhong Li ,Xioyn Zhng ,Jun Li ,Hongto Li

    a School of Mechanics and Civil Engineering,China University of Mining and Technology,Beijing,100083,China

    b State Key Laboratory of Coal Resources and Safe Mining,China University of Mining and Technology,Beijing,100083,China

    c Department of Mechanical Engineering,University of Massachusetts,Dartmouth,02747,USA

    Keywords:Longmaxi shale Three-point bending test Fracture toughness Fracture energy Crack propagation Anisotropic cohesive damage Extended finite element method(XFEM)

    A B S T R A C T The mechanical properties and fracturing mechanism of shale containing beddings are critically important in shale gas exploitation and wellbore stability.To investigate the effects of shale bedding on crack behavior and fracturing mechanism,scanning electron microscope(SEM)with a loading system was employed to carry out three-point bending tests on Longmaxi outcrop shale.The crack initiation and propagation of Longmaxi shale were observed and recorded by taking photos during loading.The cracking paths were extracted to calculate the crack length through a MATLAB program.The peak load,fracture toughness and fracture energy all increase with the bedding angle from 0°to 90°.The crack length and energy were also found to increase with the bedding angle in the range of 0°-60°and then drop slightly.The fracturing mechanism of shale includes the main crack affected by the bedding angle and disturbed by randomly distributed particles.The main cracking path was accompanied by several microcrack branches which could form an interconnected crack system.When the main crack encounters larger sedimentary particles,it will deflect around the particles and then restore to the initial direction.A numerical technique using extended finite element method(XFEM)coupled with anisotropic cohesive damage criteria was developed,which is able to capture the dependence of crack propagations on bedding angle and sedimentary particles.This study sheds light on understanding and predicting mesoscale fracture behavior of shale with different bedding angles.

    1. Introduction

    High-quality,eco-friendly economic development in China puts huge demands on shale gas.The large-scale commercial development for shale gas in China was initiated in 2009.Following the USA and Canada,China has become the third country that has realized the industrial shale gas production(Dong et al.,2016).The shale gas production increased from 25 million m3in 2012 to more than 9 billion m3in 2017,showing a promising prospect of shale gas development in China(Ma et al.,2018).

    Hydraulic fracturing is a key technology widely applied in shale gas exploitation and production. A fully developed fracture network caused by hydraulic fracturing provides a guarantee for increasing shale gas production.However,the formation mechanism of fracture network has not been well understood.The failure mechanism of shale is intricate,because the preexisting bedding acting as weak plane exerts complex impacts on mechanical properties of shale.It has been proved that Young’s modulus(Niandou et al.,1997;Ambrose,2014),Poisson’s ratio(Ambrose,2014),fracture toughness(Lee et al.,2015;Chandler et al.,2016;Luo et al.,2018),shear strength(Heng et al.,2015),compressive strength(Kovrizhnykh et al.,2017)and permeability(Yu et al.,2013)vary with the bedding angle,indicating that crack behaviors are strongly influenced by bedding plane.Evolution of fracture network has been investigated experimentally(Guo et al.,2014;Zhang et al.,2017a)and numerically(Kim and Moridis,2015;Zhang et al.,2017b).The bedding plane may be dominant in fracturing when shale is under certain stress conditions.For example,experimental results obtained by Guo et al.(2014)indicated that when the horizontal in situ stress difference is less than 9 MPa,hydraulic fracture can easily propagate along with the natural fractures,forming a fracture network.

    Fig.1.Distribution of lower Silurian Longmaxi shale gas layer in Sichuan Basin,China.

    Table 1 X-ray diffraction results of Longmaxi shale.

    Fig.2.Microstructure and mineral composition of Longmaxi shale by SEM energy spectrum analysis.

    To investigate the effects of bedding on crack propagation,a number of laboratory tests have been conducted, considering different bedding angles.By performing semicircular bend tests on Marcellus shale containing calcite-filled veins,Lee et al.(2015)found that as the approaching angle became more oblique to the induced fracture plane,the induced fractures were more likely to divert into the vein.Chandler et al.(2016)conducted the modified short rod tests on Mancos shale and found a tendency for deviation toward the bedding-parallel orientation for cracks propagating nonparallel to bedding.In situ observations on crack behaviors are expected to reveal the failure mechanism of rock,which shows both the local and global deformation.Morgan(2017)used digital image correlation(DIC)method to determine crack behaviors and found a significant influence of bedding plane on the cracking pattern of Opalinus shale.Taking in situ observation technique based on scanning electron microscope (SEM), the fracturing mechanism of marble(Zuo et al.,2015),basalt(Zuo et al.,2014a),siltstone(Zuo et al.,2014b),granite(Zuo et al.,2017)and sandstone(Zuo et al.,2010,2016)was investigated.So far,researches on the cracking process of shale at meso-scale are rather limited.Cui and Han(2018)observed the crack growth of Longmaxi shale using SEM and discussed the fracturing mechanism.However,they did not take the bedding angle into consideration.

    Fig.3.(a)Longmaxi shale block with dimensions of 300 mm×300 mm×300 mm,and(b)Sampling angle.

    Table 2 Physico-mechanical properties of Longmaxi shale.

    Fig.4.Sizes of three-point bending specimen(unit:mm).

    In this paper,three-point bending tests have been carried out on the Longmaxi outcrop shale,considering different angles between bedding plane and loading direction.The process of crack initiation and propagation was observed using SEM with a loading system.Mechanical properties,such as peak load,fracture toughness and fracture energy,were analyzed,with respect to the bedding angle.To model the cracking process of Longmaxi shale within different bedding angles, the extended finite element method (XFEM)coupled with an anisotropic cohesive zone model(CZM)was utilized in this study,which agreed well with the experimental observations. Besides, the effects of particle inclusion on crack behaviors were discussed through simulations of a single edge notch tension model.

    2. Experimental methods

    2.1. Sample preparation

    Longmaxi shale gas field in Sichuan Basin,China has been successfully explored in recent years.The Longmaxi outcrop shale specimens used in this research are sampled from Pengshui County in Chongqing,China(Fig.1).Results of X-ray diffraction in Table 1 and SEM energy spectrum analysis in Fig.2 indicate that the main mineral constituents of Longmaxi shale are quartz and calcite cemented by clay contents,which account for about 50% and 30% ,respectively.The main component of clay is illite.

    The outcrop shale block is ash black in color and its sizes are about 300 mm×300 mm×300 mm,as shown in Fig.3a.Physicomechanical properties, including density, uniaxial compressive strength(UCS),elastic modulus(E)and Poisson’s ratio(λ),were tested as per the International Society for Rock Mechanics(ISRM)suggested methods(Ulusay,2015)and are listed in Table 2.The specimen was prepared by cutting a 5-mm thick slice from a large shale block. A cuboid-shaped specimen was made into 25 mm×10 mm×5 mm(length×width×thickness)and the sizes of specimens are list in Table 2.Taking different directions of bedding plane into consideration,the angles between the long edge of the specimen and the bedding plane were set as 0°,30°,45°,60°and 90°,as shown in Fig.3b.A notch was set at the middle of the long edge of the specimen,which was about 4 mm long and 0.4 mm wide.We define θ as the angle between loading direction and bedding plane,as shown in Fig.4.The specimen was named as A°-B.For example,30°-1 denotes specimen group No.1 with θ=30°.

    Fig.5.SEM with a loading system.

    Fig.6.Typical cracking process of specimen 30°-3 and the corresponding load-displacement curve.

    2.2. Experimental procedures

    The experiments were conducted using SEM with a loading system,as shown in Fig.5.Loading tests were performed in the chamber of SEM,which made it possible to observe and record the cracking process during loading.To fix the specimen and avoid it falling from the loading table,a preload of 5 N was applied before loading test.The loading test was conducted in a displacementcontrolled mode at a rate of 10-4mm/s.The observation area was fixed in the vicinity of the preset notch tip.During the loading process,scanning was performed continuously and the corresponding load-displacement data were recorded automatically.Three SEM images could be taken per minute and each test took about 4 min.Therefore,8-9 SEM images were recorded during loading for each specimen.In each θ group,three specimens were tested.

    3. Experimental results

    3.1. Load-displacement curves

    Fig.6 shows a typical process of crack initiation and propagation for specimen 30°-3.The specimen surface before loading is demonstrated in Fig.6a and no visible cracks are found.A small crack initiated at the notch tip when the load increased to 81.6 N(Fig.6b).The crack extended forward in the horizontal direction(Fig. 6c), as the loading proceeded. When the load reached 145.5 N, unstable fracture occurred suddenly and the main crack propagated quickly through the weak bedding plane(Fig.6d).The load upon crack initiation accounted for 56.1% of the peak load.

    Fig.7a shows the load-displacement curves of the 45°group.The peak loads varied due to the heterogeneity of the Longmaxi shale.However,the curves in the range of 0-120 N matched well for specimens 45°-2 and 45°-3.When the peak load was reached,the load dropped abruptly,which indicated brittleness of the Longmaxi shale. The characteristic of brittleness was attributed to the low content of clay and high content of brittle mineral composition(Zou et al.,2010),such as quartz and calcite, which was beneficial to shale gas exploration and development.

    Fig.7.Typical load-displacement curves and the peak loads of all specimens:(a)Load-displacement curves of shale specimens in 45° group; (b) Typical loaddisplacement curves in each test group;and(c)Variation of peak load with respect to different bedding angles.

    Taking the load-displacement curve of the specimen with the median peak load in each test group, we plotted 5 loaddisplacement curves in Fig.7b.Specimen with a bedding angle of 90°showed the highest peak load of 168 N,while the specimen with a bedding angle of 0°had the lowest one of 149.2 N.The peak loads for specimens 30°-3,45°-2 and 60°-2 were slightly increased with increasing bedding angle. However, the displacements corresponding to the peak load for these three specimens were gradually increased.The displacements corresponding to the peak loads were 18.75 μm,22.4 μm and 25.61 μm,for specimens 30°-3,45°-2 and 60°-2,respectively.This was because it was more difficult for crack propagation in a larger angle θ,which needed more energy.When the bedding angle was small,the peak load became low,which is consistent with the result by Lee et al.(2015).

    Fig.8.Fracture toughness corresponding to different bedding angles.

    Fig.7c presents the variation of peak load for different θ values.The average peak load and standard deviation of peak load are listed in Table 2.Although the experimental results are relatively discrete, it is apparent that the peak load increases with θ approximately,as shown in Fig.7c.The average peak load in 0°group was approximately 80% of that in 90°group.Result of 45°group was the most discrete,with a standard deviation of 20.56 N,accounting for 13.6% of the corresponding average peak load.Considering the heterogeneity of rock materials and the small size of the specimen,we believed that the experimental results were reasonable.

    3.2. Fracture toughness corresponding to different θ values

    Stress intensity factor KIis an important index related to crack initiation and propagation.In the framework of fracture mechanics,the critical stress intensity factor is defined as the fracture toughness KIC.To discuss the effect of shale bedding on fracture toughness,linear elastic fracture mechanics was adopted to determine the mode I fracture toughness of Longmaxi shale.For simplicity,we considered the Longmaxi shale as a continuous,homogeneous and isotropic material.According to the handbook for stress analysis of crack(Tada et al.,2000),mode I fracture toughness for single edge notched three-point bending specimen could be determined by.

    where Pmaxis the peak load; l is the effective bean span(l=20 mm);a is the length of the preset notch(a=4 mm);and b and h are the thickness and width of the specimen,respectively.

    Fig.9.Measurement of crack length and its variation:(a)Merged SEM images and the cracking path extracted from SEM images;(b)Relationship between crack length and loading time;and(c)Relationship between crack length and bedding angle.

    Fracture toughness KICcorresponding to different bedding angles is presented in Fig.8.Fracture toughness gradually increased with the bedding angle θ.Similar to the peak load,the fracture toughness in a single test group was discrete,due to the heterogeneity of Longmaxi shale.Discreteness of fracture toughness was slightly different from that of peak load,because the fracture toughness was determined by multiple factors,i.e.peak load,height and thickness of the specimen. The average fracture toughness had a minimum value at the angle of 0°and it reached a maximum value at the angle of 90°,which is in line with the research on Mancos shale by Chandler et al.(2016).The variation of KICindicated that fracturing was more likely to occur,which was proved by the laboratory observations.When the prefabricated notch was parallel to the bedding plane,the crack grew rapidly along the bedding plane.When the notch was perpendicular to the bedding plane,the crack would propagate through the bedding plane.This could be observed from different crack propagation patterns with several inflections in crack propagation paths.The changes of KICwith bedding angle should be taken into consideration and it is very important for effective hydraulic fracturing and stability of shale gas shaft.

    3.3. Crack length

    When loading was completed,the cracking path was recorded by taking several overlapped SEM images at a magnification of×100.The crack is black on SEM images,as shown in Fig.9a.Using the image processing toolbox in MATLAB(MathWorks,2014),we extracted the main cracking path by threshold-based segmentation technique(Gonzalez and Woods,2018).The extracted main cracking path was shown in Fig.9a.By counting the pixels of the cracking path and the scale bar which was 100 μm on SEM images,we obtained the crack length a.Fig.9b shows the crack length of specimen 30°-3 during loading,with respect to loading time.The scale bar in the SEM image was 100 μm long,represented by 50 pixels.Therefore,the accuracy of the method was 2 μm/pixel,which was precise enough to calculate the crack length.The crack length was close to 0 mm until the loading increased to crack initial load,and then it increased significantly.The crack velocity was about 0.017 mm/s.

    Fig. 9c shows the relationship between crack length and bedding angle.Although the crack lengths in the same bedding angle group were scattered,the average crack length gradually increased in the range of 0°-60°,and then decreased when the bedding angle increased from 60°to 90°.The main cracks generally propagated through the bedding plane for the notch having angles of 30°,45°and 60°with respect to the bedding plane.The main cracks propagated along a horizontal path for a specimen with bedding angles of 0°(the notch is parallel to bedding plane)and 90°(the notch is perpendicular to bedding plane).

    3.4. Fracture energy

    The total energy W required to induce rock failure is represented by the area below the load-displacement curve for a single specimen,which represents the work done by the applied load P(Hillerborg,1985):

    Fig.10.Variations of(a)W and(b)GF with respect to bedding angle.

    Table 3 Material parameters used in the numerical model.

    where δfis the central deflection of the specimen when final rupture occurs.The fracture energy GFis defined as the energy required to create a unit area of fracture surface(Guo and Gilbert,2000):

    Fig.11.Schematic diagram of the bilinear traction-separation law.The maximum traction Tmax states the damage initiation criterion,and Gc expresses the critical energy release rate for damage evolution and is equal to the total area of the triangle.

    Fig.12.Comparisons between experimental and numerical results:(a)Inclined beddings,and(b)Vertical and horizontal beddings.

    Fig.13.Contour plot of maximum principal stress(in MPa)showing crack propagation in 60°bedding angle model at peak load.

    where Aligis the area of ligament,determined by crack length a and the thickness of specimen.

    Fig.10a shows the total energy W for different test groups.The energy W increased by 48.7% from 1.94×10-3J in 0°group to 2.89×10-3J in 60°group and then it decreased slightly to 2.85×10-3J.Variation of fracture energy GFwith respect to the bedding angle is shown in Fig.10b,which is different from that of energy W.The fracture energy GFbarely changed in the range of 0°-30°and 60°-90°,which were approximately 74 J/m2and 90 J/m2,respectively,because the trends of energy W and the crack length were similar.The fracture energy GFincreased by 22% from 30°case to 60°case.The trend of fracture energy GFwas different from that of the energy W,because the crack length slightly decreased,which resulted in a decreasing fracture surface.

    4. Numerical modeling of shale specimen with different bedding angles

    4.1. Model formulation

    The finite element models of single edge notch bending(SENB)specimens were created in the commercial software ABAQUS.For computational efficiency,the two-dimensional(2D)plane stress elements(CPS4)were used in the finite element model with displacement-controlled boundary conditions.A 4 mm pre-crack was inserted to the mid-bottom long edge of the 25 mm×10 mm(length×width)full-size model.The beam span was 20 mm long.Five bedding orientation fracture models with regard to the crack propagation direction were studied,including the vertically bedding,horizontally bedding,and obliquely bedding SENB models(θ=30°,45°and 60°).The XFEM coupled with anisotropic CZM was developed to capture fracture of shale with different bedding angles.

    The XFEM technique adopts the partition-of-unity method and expands the piecewise polynomial function space from conventional finite element method into extra“enrichment functions”to model crack propagation,which has been implemented within ABAQUS.It is capable of resolving arbitrary displacement discontinuities due to cracking,without knowing a priori cracking path in the context of bedding orientations.The method also permits a crack to be located inside a finite element.As a result,it can readily handle an evolving crack plane and solution-dependent crack propagation direction without remeshing during simulations.

    The material behaviors are assumed isotropic linear elastic before fracture,with the elastic modulus and Poisson’s ratio given in Table 3.To model fracture behaviors,an anisotropic CZM was developed to characterize the separation of fracture surfaces ruled by an irreversible traction-separation cohesive law under different bedding angles.The bilinear traction-separation law is adopted in this study(Fig.11),which has been used widely to model brittle fracture(Dahi Taleghani et al.,2018;Yang et al.,2019):

    where K denotes the slope of the initial elastic stiffness,δfrepresents the separation at complete rupture,and D is a damage variable to indicate the degradation of material stiffness.

    The anisotropic CZM was developed to capture the effects of bedding angles.Specifically,two damage initiation criteria were implemented through the user subroutine UDMGINI in ABAQUS(Li et al.,2018;Ghandriz et al.,2020).A material orientation was defined to reflect the bedding orientation in the local x-direction of each finite element.Anisotropic cohesive damage initiation and evolution criteria were then utilized to model fracture along with the local bedding orientations (weak planes). To resolve the possible cases of off-axis crack propagation,the maximum principal stress (MAXPS) criterion was also proposed. The failure criteria for weak plane and the MAXPS are defined below:

    Failure criterion 1(for the weak plane):

    Failure criterion 2(for MAXPS):

    where σijdenotes the stress component in local material orientations;σpis the MAXPS;Twi(i=I,II and III)is the maximum strength in the three fracture modes of the weak plane;Tpis the maximum value for MAXPS;and〈〉is the Macaulay bracket operator used to avoid the compressive loading effects,defined as

    where σnis the cohesive traction in the normal(mode I)direction.

    In this study,for simplicity,all the maximum strengths(Twi)were presumed the same as Tw.

    4.2. Results of numerical models with different bedding angles

    Determination of material parameters is important for accurate model predictions.The CZM parameters for the cohesive law were calibrated from experimental data at different bedding angles,which are summarized in Table 3.Fig.12 demonstrates the comparisons between the numerical and experimental results.Overall,the numerical predictions agreed well with the experimental results,which validated the numerical models in capturing shale fracture under different bedding angles.

    Fig.14.The cracking paths for shale specimens with different bedding angles:(a)Specimen 0°-3,(b)Specimen 30°-3,(c)Specimen 45°-3,(d)Specimen 60°-3,and(e)Specimen 90°-1.

    Fig.13 shows the MAXPS contour plots for 60°bedding angle model at the peak load.The crack kinking influenced by the bedding angles was observed with more widespread stress distributions.It should be noted that the numerical model did not take the porosity and the microstructure into consideration but used anisotropic CZM to capture the effects of local bedding angles.Indeed,Table 3 shows that all the material properties(including energy release rate)are the same for models with different bedding angles except the damage initiation stress.A more refined model based on local porosity and microstructures could possibly improve the accuracy and capture the variations in damage initiation stress,which will be considered in the future.

    5. Failure process and fracturing mechanism of longmaxi shale

    Fig.15.Different intergranular fracture modes of shale specimen 60°-1.

    Fig.14 shows the typical SEM images of cracking patterns for specimens with different bedding planes.Cracking paths in all test groups consisted of main crack and several microcracks along the weak bedding plane.The main crack of specimen 0°-3(Fig.14a)propagated in a small angle of 9°from the preset notch.With the increasing bedding angle,the angle between the main crack and the horizontal notch gradually increased from 19°to 56°.It was interesting that inflection points could be observed on the surfaces of specimens with the bedding angles of 45°and 90°(Fig.14 c and e).The main crack might propagate at a certain angle with the horizontal notch(or the bedding plane),but there were some inflection points when the angle between notch and bedding plane was different.From the local enlarged image in Fig.14,it could be found that there were a few microcracks near the main crack.These microcracks were in different directions due to the different scales of bedding and shale structure.Microcracks can form an interconnected pore system in shale(Ma et al.,2016),which is helpful to increase the production of shale gas.Generally,micro-fractures in rocks can be summarized into three categories: intergranular fracture,transgranular fracture,and coupled intergranular and transgranular fracture(Zuo et al.,2017).In this context,as shown in Fig.15a,most of the fractures were intergranular.When the crack met large sedimentary particles,it grew in the direction oblique to the original cracking path,dominated by the particles.But the main crack still propagated along the original path until the specimen failed(Fig.15b).

    The differences between macro-fracture parameters of Longmaxi shale reflected the diversity of fracturing mechanism.The fracturing mechanism of Longmaxi shale with different bedding angles was analyzed.The peak load,fracture toughness and fracture energy generally increased with the increase in bedding angle θ,but the crack length and energy W gradually increased with the bedding angle ranging from 0°to 60°,and then dropped slightly within the bedding angle of 60°-90°.The angle between the preset notch and the cracking path increased with bedding angle,characterized by the inflection points in Fig.14.Therefore,it can be conclusive that the peak load increases with the increasing bedding angle.

    Fig.16.Crack initiation position with different curvatures at the tip of notch.

    The orientation of the main crack varied with the bedding angle,resulting in changes in crack length(Fig.9c).The difference in the location of bedding planes resulted in a variety of cracking path,which exerted great effects on cracking patterns.Fig.16 shows the notch tips after failure at a magnification of×150.Crack initiated at the position with a larger radius of curvature due to the effects of stress concentration and also in the weak cementation between quartz and calcite grains,according to the principle of minimum energy dissipation(Zhou et al.,1997).

    6. Analysis of effect of sedimentary particle

    To investigate the effect of large sedimentary particles on crack behaviors,a single edge notch tension model with single-particle inclusion was created in ABAQUS. No bedding plane wasconsidered in the numerical model since it merely focused on the influence of particle.The 2D plane stress elements(CPS4)were used for computational efficiency and only the MAXPS criterion was used.The mechanical and fracture properties of shale(matrix)and particle(inclusion),as well as their interfaces,are listed in Table 4.

    Table 4 Material parameters for the soft shale(matrix),stiff particle(inclusion),and interface properties.

    Fig.17.Crack propagation in shale with a single sedimentary particle:(a)-(e)PHILSM contour plots showing the cracking process,and(f)Experimental result.

    Fig.18.MAXPS contour plots for fracture simulations in shale(a)With a single stiff particle,and(b)With no particles.

    Fig.19.Simulation results for shale with and without stiff particle.

    The cracking process was illustrated in PHILSM contour plots at different simulation stages and compared with the SEM image,as shown in Fig.17.The PHILSM variable is the signed distance function of the crack surface for better visualization of the cracking path.The numerical model predicted crack deflection around the sedimentary particle and restoration to pre-crack direction after passing the particle,which was similar to the observation in the laboratory test.It should be noted that the interface between shale and particle played a significant role,where a much weaker fracture property(in Table 4)was selected to guide the crack propagation along with the shale-particle interface. This is also consistent with the physical reality that the interface is usually weak and prone to crack growth.The effect of sedimentary particle was further studied by comparing the results of the shale model with and without stiff particle.Fig.18 shows the MAXPS contour plots for both cases.There were more stress concentrations around the particle. The load-displacement curves were plotted and compared in Fig.19.It was found that the existence of particle significantly increased the macroscopic peak load as well as the fracture toughness.This can be explained by the crack deflections which consume more fracture energy.Overall,the numerical study facilitates our understanding of the effects of bedding angles and sedimentary particles on crack propagation and macroscopic fracture response.

    7. Conclusions

    This paper experimentally and numerically studied fracture characteristics of the outcrop shale sampled from Longmaxi,Chongqing,China.The cracking process of Longmaxi shale was observed using SEM with a loading system,and variations of the mechanical parameters of Longmaxi shale were analyzed with respect to the bedding angle.The XFEM coupled with anisotropic CZM was developed to simulate the cracking process,which agreed well with the experimental results.Besides,the effect of particle inclusion on crack behavior was studied numerically using a single edge notch tension model.The findings are summarized as follows:

    (1)As the anisotropy of shale and the number of weak bedding planes within specimen varied,the experimental results of shale with different bedding angles are scattered,while the general tendency could be observed through the average values.The peak load,fracture toughness and fracture energy of shale gradually increased with the bedding angle until the crack length and the energy reached a maximum at an angle of 60°,after which they slightly decreased.

    (2)The main cracking path accompanied by several microcrack branches could form an interconnected crack system.The bedding plane had a significant effect on the fracture pattern of Longmaxi shale.Cracks propagated along weak cementation positions and bedding planes.When the crack encountered large sedimentary grain,it tended to propagate around the grain and branch at the weak bedding plane.Therefore,the effects of bedding should be considered in the design of hydraulic fracturing in shale gas extraction.

    (3)An anisotropic CZM coupled with XFEM was developed and validated to capture cracking of shale with different bedding angles and large sedimentary particles.A feature of the model was that both the anisotropic damage along bedding directions (weak planes) and the MAXPS failure were considered to determine the crack propagation.The effect of sedimentary particles was also studied numerically and it showed a good consistency with experimental findings.Both the peak load and fracture toughness increased due to the crack deflections around sedimentary particles.

    Declaration of Competing Interest

    The authors wish to confirm that there are no known conflicts of interest associated with this publication and there has been no significant financial support for this work that could have influenced its outcome.

    Acknowledgments

    This study was financially supported by National Natural Science Foundation of China(grant No.41877257),Beijing Outstanding Young Scientist Program(Grant No.BJJWZYJH01201911413037),Shaanxi Coal Group Key Project(Grant No.2018SMHKJA-J-03)and Yueqi outstanding scholar Award Program by China University of Mining and Technology(Beijing),China.

    波多野结衣巨乳人妻| 日韩精品中文字幕看吧| 久99久视频精品免费| 嫩草影院精品99| 中文字幕av成人在线电影| 国产老妇女一区| 欧美人与善性xxx| 精品国内亚洲2022精品成人| 国产高清视频在线观看网站| av国产免费在线观看| av在线蜜桃| 波野结衣二区三区在线| 婷婷亚洲欧美| 日韩成人伦理影院| 少妇人妻精品综合一区二区 | 亚洲成av人片在线播放无| 久久精品国产鲁丝片午夜精品| 成人性生交大片免费视频hd| 国产精品爽爽va在线观看网站| avwww免费| 国产精品综合久久久久久久免费| av福利片在线观看| 欧美不卡视频在线免费观看| 欧美日本视频| 一卡2卡三卡四卡精品乱码亚洲| 乱系列少妇在线播放| 亚洲欧美日韩卡通动漫| 超碰av人人做人人爽久久| av国产免费在线观看| 欧美日本亚洲视频在线播放| 成人亚洲欧美一区二区av| 日韩成人伦理影院| 免费观看精品视频网站| 老师上课跳d突然被开到最大视频| 亚洲人成网站在线播| 国产91av在线免费观看| 日本黄色片子视频| 最近在线观看免费完整版| 成人无遮挡网站| 美女cb高潮喷水在线观看| 两个人视频免费观看高清| 欧美日韩乱码在线| 国产男人的电影天堂91| 亚洲精品色激情综合| 我的女老师完整版在线观看| www日本黄色视频网| 自拍偷自拍亚洲精品老妇| 老熟妇仑乱视频hdxx| 一进一出抽搐gif免费好疼| 国产午夜福利久久久久久| 人妻夜夜爽99麻豆av| 免费看日本二区| 一个人免费在线观看电影| or卡值多少钱| 夜夜看夜夜爽夜夜摸| 国产色婷婷99| 久久精品国产亚洲av天美| 日本爱情动作片www.在线观看 | 亚洲自偷自拍三级| 尤物成人国产欧美一区二区三区| 亚洲美女视频黄频| 国内精品美女久久久久久| 尾随美女入室| 亚洲无线观看免费| 可以在线观看毛片的网站| 午夜精品一区二区三区免费看| 99热这里只有精品一区| 亚洲国产色片| 国产精品久久视频播放| 国产精品久久视频播放| 女人十人毛片免费观看3o分钟| 久久久久久伊人网av| 久久人人爽人人爽人人片va| 日本精品一区二区三区蜜桃| 男女做爰动态图高潮gif福利片| 自拍偷自拍亚洲精品老妇| 在线a可以看的网站| 日本一本二区三区精品| 国产真实乱freesex| 亚洲自偷自拍三级| 亚洲av一区综合| 能在线免费观看的黄片| 又爽又黄a免费视频| 赤兔流量卡办理| 在线a可以看的网站| 一级a爱片免费观看的视频| 国产欧美日韩精品亚洲av| 丝袜美腿在线中文| 久久精品国产亚洲网站| 国产探花在线观看一区二区| 网址你懂的国产日韩在线| 国内少妇人妻偷人精品xxx网站| 美女大奶头视频| 亚洲熟妇中文字幕五十中出| 女人十人毛片免费观看3o分钟| 免费在线观看成人毛片| 成人综合一区亚洲| av福利片在线观看| 人妻夜夜爽99麻豆av| 国产精品野战在线观看| 菩萨蛮人人尽说江南好唐韦庄 | 熟妇人妻久久中文字幕3abv| 久久久久免费精品人妻一区二区| 少妇的逼水好多| 精品久久久噜噜| 99热这里只有是精品50| 欧美色欧美亚洲另类二区| 欧美激情在线99| 亚洲欧美成人综合另类久久久 | 大又大粗又爽又黄少妇毛片口| 可以在线观看的亚洲视频| 成人漫画全彩无遮挡| 嫩草影院精品99| or卡值多少钱| 97在线视频观看| 久久99热这里只有精品18| 两个人的视频大全免费| 三级国产精品欧美在线观看| 国产爱豆传媒在线观看| 18禁黄网站禁片免费观看直播| 亚洲av中文av极速乱| 亚洲精品成人久久久久久| 免费av毛片视频| 欧美三级亚洲精品| 精品人妻一区二区三区麻豆 | 国产精品,欧美在线| 日本黄色视频三级网站网址| 久久久久精品国产欧美久久久| 嫩草影院入口| а√天堂www在线а√下载| 九色成人免费人妻av| 波多野结衣高清作品| 天堂动漫精品| 波多野结衣高清作品| 国产国拍精品亚洲av在线观看| 成年女人永久免费观看视频| 综合色av麻豆| 国产黄色小视频在线观看| 亚洲av一区综合| 美女内射精品一级片tv| 麻豆国产av国片精品| 美女高潮的动态| 一卡2卡三卡四卡精品乱码亚洲| 国产中年淑女户外野战色| 99热6这里只有精品| a级毛色黄片| 韩国av在线不卡| 人妻久久中文字幕网| 亚洲欧美成人精品一区二区| 亚洲真实伦在线观看| 国产成人福利小说| 夜夜爽天天搞| 国产av麻豆久久久久久久| 悠悠久久av| 国产亚洲91精品色在线| 国产真实乱freesex| 日韩大尺度精品在线看网址| 亚洲av中文av极速乱| 久久久久久久午夜电影| 毛片女人毛片| 欧美3d第一页| 亚洲三级黄色毛片| 欧美+日韩+精品| 2021天堂中文幕一二区在线观| 国产成年人精品一区二区| 精品久久久久久久末码| 国内久久婷婷六月综合欲色啪| 又黄又爽又免费观看的视频| 男人舔女人下体高潮全视频| 简卡轻食公司| 亚洲av电影不卡..在线观看| 又黄又爽又免费观看的视频| av国产免费在线观看| av在线天堂中文字幕| 国产中年淑女户外野战色| 国产激情偷乱视频一区二区| 国内少妇人妻偷人精品xxx网站| 精品久久久久久久久av| 韩国av在线不卡| 少妇的逼水好多| 天天躁夜夜躁狠狠久久av| 亚洲熟妇熟女久久| 免费人成视频x8x8入口观看| 久久久a久久爽久久v久久| 一级黄色大片毛片| 天堂√8在线中文| 亚洲最大成人手机在线| 99热精品在线国产| 欧美一区二区精品小视频在线| 免费高清视频大片| 乱系列少妇在线播放| 亚洲丝袜综合中文字幕| 日日啪夜夜撸| 在线观看美女被高潮喷水网站| 中文字幕精品亚洲无线码一区| 欧美最黄视频在线播放免费| 国产一级毛片七仙女欲春2| 香蕉av资源在线| 日本一二三区视频观看| 久久久久久久亚洲中文字幕| 我的老师免费观看完整版| 亚洲av成人av| 亚洲人与动物交配视频| 搡老熟女国产l中国老女人| 91午夜精品亚洲一区二区三区| 哪里可以看免费的av片| 97超级碰碰碰精品色视频在线观看| 人人妻人人看人人澡| av在线观看视频网站免费| 国产一区二区三区在线臀色熟女| 国产中年淑女户外野战色| 人人妻人人看人人澡| 日本与韩国留学比较| 欧美性猛交╳xxx乱大交人| 非洲黑人性xxxx精品又粗又长| 99久久精品一区二区三区| 欧美又色又爽又黄视频| 一个人免费在线观看电影| 久久精品国产99精品国产亚洲性色| 国产亚洲精品综合一区在线观看| 色噜噜av男人的天堂激情| 欧美在线一区亚洲| 午夜久久久久精精品| 国产午夜福利久久久久久| 国产成人91sexporn| 亚洲va在线va天堂va国产| 一本精品99久久精品77| 一进一出抽搐gif免费好疼| 菩萨蛮人人尽说江南好唐韦庄 | 最近2019中文字幕mv第一页| 一级毛片aaaaaa免费看小| 成人毛片a级毛片在线播放| АⅤ资源中文在线天堂| 夜夜夜夜夜久久久久| 欧美+日韩+精品| 五月伊人婷婷丁香| 午夜精品在线福利| 欧美+日韩+精品| www日本黄色视频网| 久久天躁狠狠躁夜夜2o2o| 久久久久久久久久久丰满| 欧美区成人在线视频| 国产一区亚洲一区在线观看| 别揉我奶头~嗯~啊~动态视频| 国产激情偷乱视频一区二区| 精品熟女少妇av免费看| 免费看美女性在线毛片视频| 午夜精品国产一区二区电影 | 一进一出抽搐动态| 伊人久久精品亚洲午夜| 床上黄色一级片| 97超级碰碰碰精品色视频在线观看| 国产精品乱码一区二三区的特点| 草草在线视频免费看| 久久久久九九精品影院| 亚洲av五月六月丁香网| 天堂√8在线中文| 日本黄色片子视频| 婷婷亚洲欧美| 精品久久久久久久久av| 国产精品一二三区在线看| 日本-黄色视频高清免费观看| 国产成人福利小说| 又爽又黄无遮挡网站| 看黄色毛片网站| 亚洲美女黄片视频| 国产成人a∨麻豆精品| 免费观看精品视频网站| 无遮挡黄片免费观看| 国产精品久久久久久av不卡| 天堂av国产一区二区熟女人妻| 亚洲成人精品中文字幕电影| 亚洲欧美清纯卡通| 国产在线男女| 亚洲av成人av| 久久久国产成人精品二区| 黄色配什么色好看| АⅤ资源中文在线天堂| 精品一区二区三区视频在线| 白带黄色成豆腐渣| 变态另类丝袜制服| 午夜福利成人在线免费观看| 国产女主播在线喷水免费视频网站 | 九九在线视频观看精品| 欧美性猛交╳xxx乱大交人| 国产精品久久久久久久久免| 亚洲精品一卡2卡三卡4卡5卡| 久久欧美精品欧美久久欧美| 日本五十路高清| 日韩一区二区视频免费看| 91狼人影院| 嫩草影视91久久| 欧美精品国产亚洲| 毛片一级片免费看久久久久| 直男gayav资源| 成人特级黄色片久久久久久久| 精品午夜福利在线看| 午夜免费激情av| 免费人成在线观看视频色| 精品久久久噜噜| 国产男靠女视频免费网站| 亚洲五月天丁香| 中文字幕久久专区| 国产真实伦视频高清在线观看| 18禁在线播放成人免费| 99热这里只有是精品50| 免费看a级黄色片| 校园人妻丝袜中文字幕| 亚洲三级黄色毛片| 国产一区二区在线观看日韩| 亚洲国产色片| 国产爱豆传媒在线观看| 国产精品美女特级片免费视频播放器| 国产午夜福利久久久久久| 一区二区三区免费毛片| 成人亚洲欧美一区二区av| 欧美在线一区亚洲| 国产精品一区二区三区四区免费观看 | 97碰自拍视频| 久久久久久久午夜电影| 国产av一区在线观看免费| 高清午夜精品一区二区三区 | 久久综合国产亚洲精品| 欧美成人免费av一区二区三区| 高清午夜精品一区二区三区 | 综合色av麻豆| 中文字幕人妻熟人妻熟丝袜美| 亚洲精品在线观看二区| 99久国产av精品国产电影| 精品久久久久久久人妻蜜臀av| 亚洲国产精品sss在线观看| 亚洲婷婷狠狠爱综合网| 最近最新中文字幕大全电影3| 国产极品精品免费视频能看的| 黄色视频,在线免费观看| 亚洲人成网站高清观看| 美女大奶头视频| 国产精品嫩草影院av在线观看| 亚洲性久久影院| 国产精品免费一区二区三区在线| 免费看日本二区| 三级国产精品欧美在线观看| 国产精品精品国产色婷婷| 欧美在线一区亚洲| 麻豆一二三区av精品| 亚洲国产精品sss在线观看| 亚洲欧美清纯卡通| 亚洲国产精品国产精品| 大又大粗又爽又黄少妇毛片口| 成人性生交大片免费视频hd| 女的被弄到高潮叫床怎么办| 欧美最黄视频在线播放免费| 久久久久国产网址| 成人av一区二区三区在线看| 男女做爰动态图高潮gif福利片| 成人国产麻豆网| 成人漫画全彩无遮挡| 一进一出抽搐动态| 午夜视频国产福利| 99久久久亚洲精品蜜臀av| 九色成人免费人妻av| 99热6这里只有精品| 国产亚洲精品av在线| 99国产极品粉嫩在线观看| 日本免费a在线| 国产精品伦人一区二区| 久久鲁丝午夜福利片| 国产三级在线视频| 久久久精品欧美日韩精品| 成人二区视频| 国产伦在线观看视频一区| 亚洲成人中文字幕在线播放| 欧美在线一区亚洲| 免费黄网站久久成人精品| 尾随美女入室| 亚洲av中文av极速乱| 听说在线观看完整版免费高清| 99热这里只有是精品在线观看| 国产精品野战在线观看| 国产三级中文精品| 听说在线观看完整版免费高清| 少妇人妻精品综合一区二区 | 国产免费男女视频| 九色成人免费人妻av| 免费黄网站久久成人精品| 日日啪夜夜撸| 简卡轻食公司| 成年女人看的毛片在线观看| 男女之事视频高清在线观看| 国产激情偷乱视频一区二区| 一a级毛片在线观看| 亚洲成人久久爱视频| 两性午夜刺激爽爽歪歪视频在线观看| 亚洲精品粉嫩美女一区| 亚洲精品乱码久久久v下载方式| 日本免费一区二区三区高清不卡| av卡一久久| 国产精品野战在线观看| 精品国产三级普通话版| 久久久久国内视频| 两性午夜刺激爽爽歪歪视频在线观看| 久久久久久久午夜电影| 人妻丰满熟妇av一区二区三区| 一级a爱片免费观看的视频| 亚洲欧美日韩高清专用| 一级黄色大片毛片| 免费看美女性在线毛片视频| 中文字幕久久专区| 久久精品国产清高在天天线| 极品教师在线视频| 大型黄色视频在线免费观看| 一级毛片我不卡| 欧美绝顶高潮抽搐喷水| 成人特级av手机在线观看| 九九爱精品视频在线观看| 最好的美女福利视频网| 亚洲国产色片| 国产女主播在线喷水免费视频网站 | 三级国产精品欧美在线观看| 日本a在线网址| 亚洲成av人片在线播放无| 黄片wwwwww| 国产视频内射| 蜜臀久久99精品久久宅男| 亚洲七黄色美女视频| 日韩一区二区视频免费看| 中文字幕熟女人妻在线| 国产精品国产高清国产av| 精品久久久久久久末码| 精品一区二区三区人妻视频| 久久精品国产亚洲网站| 男人舔女人下体高潮全视频| 又黄又爽又刺激的免费视频.| 国产精品人妻久久久影院| 免费一级毛片在线播放高清视频| 国产高清有码在线观看视频| 国产片特级美女逼逼视频| 伊人久久精品亚洲午夜| 天堂√8在线中文| 一本精品99久久精品77| 18禁黄网站禁片免费观看直播| 最近在线观看免费完整版| 熟女电影av网| 天美传媒精品一区二区| 亚洲人成网站在线观看播放| 免费不卡的大黄色大毛片视频在线观看 | 51国产日韩欧美| 欧美三级亚洲精品| 亚洲av熟女| 国产精品99久久久久久久久| 国产伦精品一区二区三区视频9| 一本久久中文字幕| 色综合色国产| 久久精品影院6| 久久99热6这里只有精品| 两个人的视频大全免费| 久久久久九九精品影院| 一个人看的www免费观看视频| 国产精品久久视频播放| 国产精品综合久久久久久久免费| 国产单亲对白刺激| 国产成人91sexporn| 联通29元200g的流量卡| 综合色丁香网| 欧美日韩综合久久久久久| 99在线视频只有这里精品首页| 欧美又色又爽又黄视频| 欧美高清性xxxxhd video| 99热只有精品国产| 午夜视频国产福利| а√天堂www在线а√下载| 国产视频一区二区在线看| 能在线免费观看的黄片| 婷婷色综合大香蕉| 亚洲av成人精品一区久久| 淫秽高清视频在线观看| 三级经典国产精品| 成人av在线播放网站| 精品人妻视频免费看| 欧洲精品卡2卡3卡4卡5卡区| 99在线人妻在线中文字幕| 欧美日韩国产亚洲二区| 午夜福利在线观看吧| 两个人的视频大全免费| 91精品国产九色| 国产精品免费一区二区三区在线| 免费av观看视频| 欧美zozozo另类| 不卡一级毛片| 男人狂女人下面高潮的视频| 国产精品一及| 国产亚洲精品综合一区在线观看| 六月丁香七月| 日韩一本色道免费dvd| 亚洲欧美精品综合久久99| 97超视频在线观看视频| 91狼人影院| 午夜老司机福利剧场| 久久热精品热| 精品午夜福利视频在线观看一区| 精品乱码久久久久久99久播| av在线亚洲专区| 久久久久国内视频| 日日啪夜夜撸| av黄色大香蕉| 综合色av麻豆| 在线观看66精品国产| 亚洲人与动物交配视频| 国产高清激情床上av| 亚洲丝袜综合中文字幕| 欧美激情在线99| av在线蜜桃| 久久草成人影院| 深夜精品福利| 国产真实伦视频高清在线观看| 啦啦啦啦在线视频资源| 亚州av有码| 伦精品一区二区三区| 一本久久中文字幕| 午夜福利18| 老女人水多毛片| 俄罗斯特黄特色一大片| 亚洲中文字幕日韩| 最新在线观看一区二区三区| 国产伦精品一区二区三区视频9| av黄色大香蕉| 日本精品一区二区三区蜜桃| 日本一本二区三区精品| 久久婷婷人人爽人人干人人爱| 国产精品永久免费网站| eeuss影院久久| 久久久久久久久久久丰满| 久久精品国产清高在天天线| 十八禁国产超污无遮挡网站| 国产精品一及| 老师上课跳d突然被开到最大视频| 日日撸夜夜添| 国产又黄又爽又无遮挡在线| 在线免费观看的www视频| 十八禁国产超污无遮挡网站| 长腿黑丝高跟| 国产伦精品一区二区三区四那| 淫秽高清视频在线观看| 欧美+日韩+精品| 99国产精品一区二区蜜桃av| 欧美最新免费一区二区三区| 18禁裸乳无遮挡免费网站照片| 亚洲人成网站在线播放欧美日韩| 俺也久久电影网| 日本黄色视频三级网站网址| 老司机影院成人| 在线观看av片永久免费下载| 午夜激情欧美在线| 亚洲自拍偷在线| 中文字幕免费在线视频6| 国产真实伦视频高清在线观看| 晚上一个人看的免费电影| 久久精品久久久久久噜噜老黄 | 国产一区二区激情短视频| 亚洲人成网站在线观看播放| 女人十人毛片免费观看3o分钟| ponron亚洲| 国产久久久一区二区三区| 成人特级av手机在线观看| 成人亚洲欧美一区二区av| 夜夜夜夜夜久久久久| 黑人高潮一二区| 日韩,欧美,国产一区二区三区 | 午夜福利在线观看吧| 日本五十路高清| 日本一本二区三区精品| 国产高清有码在线观看视频| 国内少妇人妻偷人精品xxx网站| 国产久久久一区二区三区| 舔av片在线| 午夜福利在线观看免费完整高清在 | 国产乱人偷精品视频| 嫩草影院精品99| 免费观看在线日韩| 人妻久久中文字幕网| a级毛片免费高清观看在线播放| 在线a可以看的网站| 国产视频内射| 国产亚洲91精品色在线| 网址你懂的国产日韩在线| 日本撒尿小便嘘嘘汇集6| 深夜精品福利| 免费无遮挡裸体视频| 精品无人区乱码1区二区| 久久久久久久久久黄片| 又黄又爽又免费观看的视频| 午夜激情福利司机影院| 免费不卡的大黄色大毛片视频在线观看 | 一级毛片电影观看 | 精品久久久噜噜| 色播亚洲综合网| 日本五十路高清| 国产色婷婷99| 18禁在线无遮挡免费观看视频 | 国产大屁股一区二区在线视频| 精品免费久久久久久久清纯| 精品人妻偷拍中文字幕| 国产综合懂色| 天美传媒精品一区二区| 国产乱人视频| 乱码一卡2卡4卡精品| 一区二区三区四区激情视频 | 国产一区二区在线av高清观看| 伦理电影大哥的女人| 99热全是精品| 亚洲熟妇中文字幕五十中出| .国产精品久久| 亚洲一区高清亚洲精品| 亚洲国产欧美人成| 成人特级黄色片久久久久久久|