    Low velocity impact studies of E-glass/epoxy composite laminates at different thicknesses and temperatures

    2020-01-07 09:10:54SreekanthaReddyRamaSubbaReddyVemuriMadhu
    Defence Technology 2019年6期

    T.Sreekantha Reddy,P.Rama Subba Reddy,Vemuri Madhu

    Defence Metallurgical Research Laboratory,Hyderabad,500058,India

    ABSTRACT Low velocity impact experiments were carried out on E-glass/epoxy composite laminates having varying thicknesses at sub zero and elevated temperatures using hemi spherical steel impactor of 16 mm diameter with impact energies in the rage of 50-150 J.The performance of the laminates was assessed in terms of energy absorption,maximum displacement,peak force and failure behaviour.Results indicated that the effect of temperature on energy absorption of the laminate is negligible although the laminates are embrittling at sub zero temperatures.However it has influence on failure behaviour and displacement.Peak force has increased linearly with increase in laminate thickness from 5 to 10 mm.However it got reduced by 25%when temperature was increased from-20°C to 100°C.Based on experimental results,laminate perforation energies were predicted using curve fitting equations.Statistical analysis was carried out using Taguchi method to identify the global effects of various parameters on laminate performance and confirmed that the laminate thickness has significant influence as compared to temperature,for the studied range.

    Keywords:Laminates Glass fibres Impact behaviour Delamination

    1. Introduction

    Glass fibre reinforced composite laminates have gained significant importance in aerospace and defence applications due to their high specific strength,damage tolerance and maturity in processing.They have also been recognised as an alternative energy absorbing materials for replacing steel and light alloy armour materials in impact related applications.In recent times glass fiber reinforced composites are being used as structural and applique armour in various light weight combat systems.However,composites are sensitive to out of plane impact,which can initiate damage even at very low impact energies.Hence,this area was studied extensively by many researchers [1-7]. For instance,studies on effect of temperature and impact energy on laminate performance have shown that the impact energy has minimum role to play on laminate performance whereas lowering the temperature resulted in decrease of damage area[8-12].In another study,F.J.Yang et al.[13]studied the effect of thickness(t)and temperature on critical force to initiate the damage(Pcrit)of glass/epoxy composites and reported that impact force required to initiate damage varies linearly witht3/2and influence of test temperature on damage initiation is complex.Icten et al.[14]studied the impact behaviour of GFRP laminates subjected to a low velocity impact in the temperature range of-60°C to 20°C and found that damage area decreases and threshold energy for perforation increases with decrease in temperature.Pietro Russo et al.[15]examined the lowvelocity impact behaviour of glass/polyurethane composite laminates at-50°C,-25°C&ambient temperatures and reported that lowering of temperature resulted in increase in stiffness and damage.Most of these studies were focused on thin laminates of about 3 mm thickness with impact energies upto 30 J.As the thickness of the laminate increases,the effect of temperature may vary due to increase in number of interfaces.The main objective of the present study is to evaluate the low velocity impact resistance of E-glass/epoxy composite laminate as a function of thickness,temperature and impact energy.Another objective is to predict the perforation threshold energy for different thickness laminates using curve fitting equations,and also to identify the global effects of temperature and thickness on laminate performance through Taguchi statistical analysis.

    2. Experimental

    2.1. Materials

    Composite laminates were prepared from commercially available epoxy resin,hardener(LY556,HY5200).E-glass plain woven roving[0°/90°]having 0.25 mm thickness,360 GSM with warp and weft of 55×50 per 10 cm width was used as reinforcement.Pre-pregs were prepared by hand layup technique followed by curing under hot compression moulding.Cure temperature was maintained at 120°C for 3h followed by 160°C for 2h under 40 bar pressure.Thus laminates of 5 mm,7 mm and 10 mm thickness with an accuracy of±0.1 mm were prepared.Fibre volume fraction(Vf)of the fabricated laminates was determined as per ASTM D 3171 and found to be 0.62±0.02.Mechanical properties like tensile strength,flexural strength and interlaminar shear strength(ILSS)of the laminates were evaluated as per ASTM D 3039,D 790,D 2344, respectively and were found to be 410±10 MPa,450±20 MPa and 50±3 MPa respectively.For low velocity impact tests laminates with dimensions of 150×100 mm were cut using diamond wheel cutting machine.

    2.2. Low velocity impact tests

    Impact tests were performed using instrumented drop weight impact tester which is shown in Fig.1(CEAST-9350).The instrument has got climatic chamber to conduct the tests at different temperature ranges.It has got pneumatic clamping with provision of 76.2 mm diameter opening to position the test specimen.It is equipped with anti rebound mechanism to prevent the multiple hits.A steel impactor having hemi spherical tip of 16 mm diameter was attached to the striker rod.The striker was equipped with force transducer of 45 kN capacity to measure the force exerted by the test specimen on the impactor during the impact.Impactor mass was kept constant(5.277 kg)and required impact energy was achieved by dropping the impactor from a pre-calculated height.The tests were carried out at(-)20°C,(+)25°C&(+)100°C temperature.Prior to the test,the specimens were conditioned at the specified temperature for 1 h to attain the uniform temperature.The chosen impact energies were 50,100 and 150 J to cover the range of perforation and non-perforation. The corresponding impact velocities were 4.34, 6.08 and 7.51 m s-1respectively.Limited experiments were conducted at 200 J impact energy also.Complete experimental parameters are given in Table 1. Data acquisition system was used to record the force-time data at a rate of 500 kHz.Using the force-time data,impact parameters like Peak force(Fmax),absorbed energy(Ea),maximum displacement(Dmax)and impact velocity were calculated using the in-built software of the equipment[16].Minimum of three samples were tested at each energy level for each thickness and temperature.

    2.3. Failure analysis

    Post impacted laminates were observed visually to know the extent of damage and mode of failure[5].Areas of fibre breakage and delamination regions were measured and reported.Delamination regions were formed in distorted circle shape. Hence,perimeter of this shape was measured and area was calculated as an equivalent circle shape.Sterio microscope(Make:Leica micro systems,Model:M165C)and scanning electron microscopy(Make:FEI,Model:Quanta 400)were used to study the failure mode of laminates.

    Table 1Experimental parameters.

    Fig.1.Instrumented drop weight impact tester(Ceast-Instron 9350 model).

    Fig.2.A typical force-displacement curve depicting behaviour at different impact energies.

    2.4. Statistical analysis of results

    Taguchi statistical analysis was performed using Minitab?software tools in order to identify the most influential parameter among thickness,temperature and impact energy on laminate peak force and maximum displacement[17].Three variables viz.thickness,temperature and impact energy each having three levels were chosen as input factors.Peak force(Fmax)and maximum displacement(Dmax)were chosen as performance indices.Analysis trials were carried out using L27 orthogonal array with 27 combinations of process parameters that were selected to assess the influence of different factors.The results of response measures were converted into signal-to-noise(S/N)ratio by using ANOVA.Various S/N ratios exist based on the type of response.The larger the value for response likeFmax,better will be the performance,where as in case ofDmax,lower the value better will be the performance.Hence,it is represented as‘‘larger is better’’or‘‘smaller is better’’in the respective graphs[18].

    3. Results&discussion

    3.1. Force-displacement

    Fig.2 indicates a typical force-displacement curve for rebound and complete perforation instances.Closed loop indicates partial penetration and rebound of impactor,whereas,open curve indicates the complete perforation of the specimen[14].

    Fig.3(a)-(c)illustrates force-displacement curves of laminates having different thickness impacted at-20°C,25°C and 100°C respectively with 100 J impact energy.It is observed that,impactor has rebounded for all the thicknesses except for 5 mm at 150 J which is more than the laminate threshold energy.As the temperature increased number of oscillations in force-displacement curve have reduced at all thickness levels that were studied.This may be due to softening of matrix.

    Table 2 gives maximum displacement values of all the laminates impacted at three incident energies and temperatures. It is observed from Table 2 that the decrease in temperature and increase in laminate thickness has resulted in reduction of displacement. This may be attributed to stiffening of matrix at low temperature and increased laminate resistance at higher thickness.For instance,maximum displacement of 5 mm thickness laminate at 100°C is 10.9 mm and it is decreased by 5.5%and 12.8%at 25°C and-20°C respectively.These observations are in line with the reported literature[11,19].

    Comparison of peak force(Fmax)values of 5 mm,7 mm and 10 mm thickness laminates impacted at different temperatures and impact energies are presented in Fig.4.Peak force which indicates load bearing capacity of material has increased with increase in impact energy and laminate thickness.This may be due to increase of incident energy and laminate resistance.In the case of 5 mm laminate impacted at 50 J energy and 25°C temperature observed peak force was 13.6 kN.This has increased to 15 kN(10.2%)at 100 J and has become constant at 150 J impact energy at which the perforation of laminate was observed.From the figure it can be seen that peak force has increased by 41%and 94%for 7 mm,10 mm laminates respectively over that of 5 mm thick laminate.As far as the temperature effect is concerned,5 mm thick laminates have shown 20-25%reduction in peak force when the testing temperature was increased from-20°C to 100°C.This can be attributed to increased ductility of laminate due to softening of matrix at high temperatures.

    3.2. Energy dissipation at different temperatures

    Fig.5 shows energy-time curves of all the laminates impacted at 100 J energy.In a typical energy-time curve,maximum value in the curve indicates the maximum impact energy absorbed by the laminate,flat portion gives the final absorbed energy and the difference between these two gives the rebound energy or elastic energy[10].It can be seen from the figure that the absorbed energy has decreased and rebound energy has increased with increase in thickness of laminate.This may be due to increased laminate resistance and stiffness at higher thickness.On the other hand effect of temperature is found to be minimal on laminate energy absorption.For instance,5 mm thick laminate absorbed 86,89&86.5 J at-20°C,25°C&100°C respectively.

    Fig.3.Force-displacement curves for 100 J impact energy at three different temperatures.

    Energy profile diagrams(EPD)where absorbed energy is plotted against impact energy, indicate whether the laminates are completely perforated or not at a particular impact energy[20,21].Complete perforation of laminate occurs when the absorbed energy is equal to the impact energy i.e.when the absorbed energy falls on the equal energy line of energy profile diagram.Fig.6 shows energy profile diagrams at three different temperatures.It suggests that 5 mm thick laminates impacted at 150 J energy have completely perforated.The absorbed energies of rest of the laminates are below the equal energy line which means the perforation threshold of these laminates is higher than the studied impact energy range.These laminates were partially penetrated and the excess energy was utilized for rebound of impactor.From EPDs,it is difficult to understand the effect of temperature on laminate energy absorption as the given impact energy is below the laminate threshold energy.Hence,rebound energy(Er)against impact energy(Fig.7)was plotted to get perforation energy threshold(Ep)of each laminate for different temperatures and thickness.Experimental data was fitted in 2nd order polynomial equation.Non-zero roots of this equation give the perforation threshold energy of the laminate.The predicted threshold energy values are given in Table 3.It summarizes that the perforation threshold energy values of 5 mm laminates are similar at all the three temperatures,whereas in the case of 7 mm&10 mm laminates the threshold energies increased with decrease in temperature from 100°C to-20°C.The reason for increase in perforation threshold energies can be related to the glass transition temperature(Tg)of composites.TheTgof E-glass/epoxy composites is 133°C[22].Below theTg,polymer molecules become stiff and behave like a rigid structure due to decrease of Brownian movement and this effect seems to be more prominent at higher laminate thickness[23].The predicted perforation threshold energies were validated by measuring experimentally at 25°C and found to be matching closely.

    Table 2Comparison of maximum displacement values for all the laminates at three different temperatures and impact energies.

    Fig.4.Comparison of Fmax Vs laminate thickness at different temperatures.

    Fig.5.Energy-time curves for 100 J impact energy at three different temperatures.

    3.3. Effect of thickness and temperature on damage behaviour

    Fig.8 shows impacted laminate which depicts various damage modes.Visual observation of impacted laminates revealed that surface cracking,indentation,matrix cracking,bending of laminates,delamination and fibre breakage are found to be prominent damage mechanisms.All these damage modes were confirmed by optical and scanning electron microscopic(SEM)analysis(Fig.9).

    Length of impact surface cracking and diameter of indentation were found to be increased with increase in temperature as well as increase in impact energy.Delamination area is decreased with increase in temperature whereas the amount of fibre breakage at back surface is increased.When compared the effect of thickness on damage modes,it is found that delamination area is increased for 5 mm-7 mm and then decreased for 10 mm laminate,whereas,fibre breakage area is decreased with increase in laminate thickness.Images of all the thickness laminates impacted at different temperatures and impact energies are given in Fig.10 and complete quantitative damage analysis is as follows.

    Fig.6.Energy profile diagrams at three different temperatures.

    Fig.7.Perforation energy threshold diagrams with 2nd order polynomial fit at three different temperatures.

    Table 3Perforation threshold energies(Ep)predicted from curve fitting of Fig.7 and experimentally measured values.

    Fig.8.Photographs of impacted laminates showing various damage modes.

    Fibre breakage area and delamination area of all the laminates impacted at different energies at 25°C were calculated and given in Fig.11.Fibre breakage area has come down at all the impact energies with the increase of thickness.For instance,fibre breakage area for 5 mm, 7 mm&10 mm thick laminates was found to be 5.75,2.15 & 0 cm2respectively, when impacted with 100 J energy.Delamination areas were found to be in the range of 5-45 cm2for the laminates tested in the impact energy regime as shown in Fig.11(b).Damage areas of all the laminates impacted at 3 different temperatures are presented in Table 4.From the table it is observed that the total damage area has decreased as the testing temperature was increased from-20°C to 100°C.As discussed previously this may be due to decreased brittleness of polymer matrix at higher temperature.These observations are in line with the findings of S Benli et al.[24].

    3.4. Statistical analysis by Taguchi method

    Fig.12 shows Taguchi statistical analysis data on effect of various parameters onFmax.It is observed that the thickness has high degree of influence onFmaxwhere as temperature and impact energy has moderate effect.SinceFmaxis‘larger is better’type characteristic,higher thickness and lower temperature will give the betterFmax.Similarly,Fig.13 describes the effect of experimental variables onDmaxand found that the thickness and impact energy have significant influence as compared to temperature.The quantitative result of ANOVA are presented in Table 5.It can be noted that the largeFvalue(statistical value which is different fromFmax)indicates larger influence of that particular parameter on performance indices(Fmax&Dmax).From the table it can be seen that the thickness has highest influence onFmax,whereas,impact energy has major effect onDmax.When we take 95%confidence level i.ep<0.05,it is deciphered thatFmaxwas influenced by all the three parameters andDmaxwas affected by only thickness&impact energy.

    4. Conclusions

    E-glass/epoxy composite laminates were studied under low velocity impact conditions as a function of laminate thickness and temperature(viz.-20,25 and 100°C)on impact parameters like peak force,maximum displacement,perforation threshold energy and damage area.The following conclusions were arrived from this study.

    Fig.9.(a)Optical and(b)-(d)SEM images of 5 mm thick laminate impacted at 150 J

    Fig.10.Images of all laminates impacted at three different temperatures&energies.

    (1)Maximum displacement of laminate has decreased with increase of laminate thickness as more volume of material is engaged in dissipation of impact energy at higher thickness.Further, maximum displacement has decreased with lowering of temperature due to stiffening of matrix at low temperature.

    (2)Effect of temperature on perforation threshold energy is found to be more significant at higher thickness laminates due to increase of laminate rigidity at low temperature.

    (3)Perforation threshold energy has increased linearly with the increase in laminate thickness.The predicted perforation energies are closely matching with the experimentally measured values.

    (4)Microscopy analysis on impacted laminates showed that matrix cracking,delamination and fibre breakage are the main energy absorption mechanisms.

    (5)Statistical analysis of the results have shown that the laminate thickness has highest influence on peak force due to increase of resistance and stiffness.However,thickness and impact energy have significant effect on displacement.

    Fig.11.(a)Fibre breakage area and(b)Delamination area of all the laminates impacted at different energies at 25°C.

    Table 4Damage areas of all the laminates impacted at three different temperatures.

    Fig.12.Effect of experimental variables on Fmax.

    Fig.13.Effect of experimental variables on Dmax.

    Table 5Analysis of variance for S/N ratios for Fmax and Dmax.

    Acknowledgements

    Authors gratefully acknowledge Dr. Vikas Kumar, Director,Defence Metallurgical Research Laboratory(DMRL),Hyderabad for his encouragement to publish this work.Authors also acknowledge the support rendered by the staff of Armour Design and Development Division(ADDD).Authors specially thank Mr.Ravindranadh Bobbili of ADDD for his help in Taguchi analysis.

    伊人亚洲综合成人网| 免费高清在线观看视频在线观看| 91字幕亚洲| 日本五十路高清| 日本黄色日本黄色录像| 中文字幕另类日韩欧美亚洲嫩草| 又大又爽又粗| 日本wwww免费看| 日韩一卡2卡3卡4卡2021年| 欧美亚洲 丝袜 人妻 在线| 老司机午夜十八禁免费视频| 丰满人妻熟妇乱又伦精品不卡| 窝窝影院91人妻| 一级毛片电影观看| 91大片在线观看| 午夜成年电影在线免费观看| 国产精品成人在线| 日本91视频免费播放| 国产精品麻豆人妻色哟哟久久| 国产日韩欧美在线精品| 久久精品aⅴ一区二区三区四区| 新久久久久国产一级毛片| 亚洲第一av免费看| 久久久欧美国产精品| 日本91视频免费播放| 淫妇啪啪啪对白视频 | 大陆偷拍与自拍| 日韩视频一区二区在线观看| 亚洲九九香蕉| 日韩人妻精品一区2区三区| 成人手机av| 最黄视频免费看| 国产极品粉嫩免费观看在线| tocl精华| 免费看十八禁软件| 大陆偷拍与自拍| 日本精品一区二区三区蜜桃| 蜜桃在线观看..| 日韩电影二区| 狂野欧美激情性bbbbbb| 中文字幕精品免费在线观看视频| 男女国产视频网站| 黄色a级毛片大全视频| 热re99久久国产66热| 曰老女人黄片| 超碰97精品在线观看| 波多野结衣av一区二区av| 欧美在线黄色| 国产精品九九99| 一二三四社区在线视频社区8| 1024香蕉在线观看| 国产精品秋霞免费鲁丝片| 麻豆av在线久日| 亚洲欧美一区二区三区黑人| 亚洲av日韩精品久久久久久密| 亚洲精品中文字幕一二三四区 | 高清视频免费观看一区二区| 久久亚洲国产成人精品v| 精品少妇黑人巨大在线播放| 人人妻人人澡人人爽人人夜夜| 免费女性裸体啪啪无遮挡网站| 男女边摸边吃奶| 操美女的视频在线观看| 精品少妇久久久久久888优播| 一本综合久久免费| 97精品久久久久久久久久精品| 女人被躁到高潮嗷嗷叫费观| 国产亚洲av片在线观看秒播厂| 建设人人有责人人尽责人人享有的| 久久久久久亚洲精品国产蜜桃av| 黑人欧美特级aaaaaa片| 亚洲精品第二区| 国产成人欧美| 久久亚洲精品不卡| 性高湖久久久久久久久免费观看| 在线看a的网站| 久久香蕉激情| 久久久精品94久久精品| 岛国在线观看网站| av天堂在线播放| 亚洲,欧美精品.| 一二三四社区在线视频社区8| www.av在线官网国产| 国产有黄有色有爽视频| 1024视频免费在线观看| 亚洲男人天堂网一区| 99九九在线精品视频| 午夜91福利影院| 黄色毛片三级朝国网站| 亚洲五月色婷婷综合| 亚洲中文字幕日韩| 欧美日韩黄片免| 精品亚洲乱码少妇综合久久| 青春草视频在线免费观看| 国产有黄有色有爽视频| 免费高清在线观看视频在线观看| 日韩大片免费观看网站| 91精品国产国语对白视频| 国产精品一二三区在线看| 美女中出高潮动态图| 国产精品国产av在线观看| 成年人免费黄色播放视频| 亚洲av日韩在线播放| 国产黄频视频在线观看| av一本久久久久| 大片免费播放器 马上看| 国产视频一区二区在线看| 国产精品一二三区在线看| 国产深夜福利视频在线观看| 老熟妇仑乱视频hdxx| 亚洲免费av在线视频| 黄片播放在线免费| 欧美性长视频在线观看| 国产亚洲av高清不卡| 欧美精品高潮呻吟av久久| 亚洲视频免费观看视频| 美女脱内裤让男人舔精品视频| 亚洲精品日韩在线中文字幕| 久久这里只有精品19| 国产亚洲欧美精品永久| 中文字幕av电影在线播放| 热re99久久精品国产66热6| 嫩草影视91久久| 亚洲久久久国产精品| 最近最新免费中文字幕在线| 国产精品免费大片| 50天的宝宝边吃奶边哭怎么回事| a 毛片基地| 国产精品香港三级国产av潘金莲| 亚洲av电影在线进入| 亚洲一码二码三码区别大吗| bbb黄色大片| 国产国语露脸激情在线看| 宅男免费午夜| 国产亚洲欧美在线一区二区| 久久精品亚洲av国产电影网| 女人精品久久久久毛片| 色视频在线一区二区三区| 侵犯人妻中文字幕一二三四区| 在线观看一区二区三区激情| 大香蕉久久网| 亚洲精品日韩在线中文字幕| 两人在一起打扑克的视频| 国产av国产精品国产| 老熟妇乱子伦视频在线观看 | 一级毛片精品| 欧美日韩一级在线毛片| 一本色道久久久久久精品综合| 少妇猛男粗大的猛烈进出视频| 妹子高潮喷水视频| 日本欧美视频一区| 精品免费久久久久久久清纯 | 国产精品二区激情视频| 国产福利在线免费观看视频| 桃花免费在线播放| 亚洲色图综合在线观看| 又紧又爽又黄一区二区| 欧美97在线视频| 最近最新中文字幕大全免费视频| 夜夜夜夜夜久久久久| 亚洲精品国产色婷婷电影| 午夜福利影视在线免费观看| 国产精品一区二区在线观看99| 99re6热这里在线精品视频| 国产精品成人在线| 日本av手机在线免费观看| 久久国产精品影院| 国产精品影院久久| 91精品三级在线观看| 纵有疾风起免费观看全集完整版| a在线观看视频网站| 日韩,欧美,国产一区二区三区| 最新的欧美精品一区二区| 欧美大码av| 欧美成人午夜精品| 欧美老熟妇乱子伦牲交| 亚洲激情五月婷婷啪啪| 91大片在线观看| 欧美精品亚洲一区二区| 在线永久观看黄色视频| 母亲3免费完整高清在线观看| 国产成人欧美在线观看 | av网站免费在线观看视频| 夫妻午夜视频| 亚洲精品第二区| 久久av网站| 日韩大码丰满熟妇| 国产男人的电影天堂91| 不卡av一区二区三区| 美女午夜性视频免费| 国产精品自产拍在线观看55亚洲 | 亚洲国产成人一精品久久久| 亚洲精品粉嫩美女一区| 色婷婷av一区二区三区视频| 亚洲中文日韩欧美视频| 18禁观看日本| 国产欧美日韩一区二区三 | 久久九九热精品免费| 日本av免费视频播放| 欧美黑人精品巨大| 99re6热这里在线精品视频| 国产一区二区三区av在线| 国产亚洲午夜精品一区二区久久| 亚洲欧美一区二区三区久久| 久久精品国产a三级三级三级| 精品少妇黑人巨大在线播放| 国产福利在线免费观看视频| e午夜精品久久久久久久| 黄色怎么调成土黄色| 国产日韩欧美视频二区| 天天躁狠狠躁夜夜躁狠狠躁| 乱人伦中国视频| 亚洲av成人一区二区三| av不卡在线播放| 中文字幕制服av| 欧美老熟妇乱子伦牲交| 又大又爽又粗| 日韩大片免费观看网站| 人人澡人人妻人| 一本大道久久a久久精品| 1024视频免费在线观看| 成人国产av品久久久| 国产精品免费大片| 亚洲精品在线美女| 国产欧美亚洲国产| 一进一出抽搐动态| 久久国产亚洲av麻豆专区| 久久久久久免费高清国产稀缺| 国产在线观看jvid| 日本黄色日本黄色录像| 老鸭窝网址在线观看| 亚洲国产av新网站| 青春草亚洲视频在线观看| 99国产精品一区二区三区| 久久国产精品男人的天堂亚洲| 美女脱内裤让男人舔精品视频| 国产一区二区在线观看av| 大片免费播放器 马上看| 国产精品久久久久久精品古装| 久久毛片免费看一区二区三区| 色精品久久人妻99蜜桃| 自拍欧美九色日韩亚洲蝌蚪91| 亚洲精品国产av成人精品| 黑人巨大精品欧美一区二区蜜桃| 男女床上黄色一级片免费看| 男女边摸边吃奶| 国产精品免费大片| 欧美人与性动交α欧美软件| 嫩草影视91久久| 99精品欧美一区二区三区四区| 在线观看免费日韩欧美大片| xxxhd国产人妻xxx| 黄色 视频免费看| 蜜桃在线观看..| 两性夫妻黄色片| 国产片内射在线| 美女福利国产在线| 亚洲熟女精品中文字幕| 免费av中文字幕在线| 一级黄色大片毛片| 国产亚洲精品第一综合不卡| 亚洲av国产av综合av卡| 亚洲精品av麻豆狂野| 国产成人系列免费观看| 久久天躁狠狠躁夜夜2o2o| 99国产综合亚洲精品| 日本wwww免费看| 夜夜骑夜夜射夜夜干| 精品视频人人做人人爽| 中文欧美无线码| 天天躁日日躁夜夜躁夜夜| 精品一品国产午夜福利视频| 中文欧美无线码| 亚洲国产欧美网| 欧美黑人精品巨大| 后天国语完整版免费观看| 久久午夜综合久久蜜桃| 久久久精品区二区三区| 久久狼人影院| 欧美精品一区二区大全| 免费久久久久久久精品成人欧美视频| 亚洲午夜精品一区,二区,三区| 美女中出高潮动态图| 亚洲精品自拍成人| 人人澡人人妻人| 婷婷成人精品国产| 国产精品.久久久| 性少妇av在线| 色婷婷久久久亚洲欧美| 精品一区二区三卡| 成年美女黄网站色视频大全免费| 各种免费的搞黄视频| 亚洲精品第二区| 人妻一区二区av| 搡老岳熟女国产| 欧美精品高潮呻吟av久久| cao死你这个sao货| 99久久精品国产亚洲精品| av国产精品久久久久影院| 亚洲国产看品久久| 美女主播在线视频| 下体分泌物呈黄色| 亚洲av日韩精品久久久久久密| 国产精品欧美亚洲77777| 天堂俺去俺来也www色官网| 高清视频免费观看一区二区| 亚洲伊人久久精品综合| a级毛片黄视频| 老汉色av国产亚洲站长工具| 日本一区二区免费在线视频| 搡老熟女国产l中国老女人| 巨乳人妻的诱惑在线观看| 欧美日韩视频精品一区| 亚洲国产欧美网| 日韩制服丝袜自拍偷拍| 另类亚洲欧美激情| 亚洲黑人精品在线| 一本色道久久久久久精品综合| 日日摸夜夜添夜夜添小说| 日本五十路高清| 亚洲欧美一区二区三区黑人| 18禁裸乳无遮挡动漫免费视频| 久久九九热精品免费| av一本久久久久| 欧美日韩福利视频一区二区| 日本av手机在线免费观看| 亚洲国产成人一精品久久久| 亚洲九九香蕉| 日韩中文字幕视频在线看片| 国产老妇伦熟女老妇高清| 欧美激情 高清一区二区三区| av福利片在线| 亚洲av片天天在线观看| 搡老岳熟女国产| a在线观看视频网站| 色视频在线一区二区三区| 纯流量卡能插随身wifi吗| www.av在线官网国产| 亚洲国产av影院在线观看| 亚洲欧美清纯卡通| 精品人妻在线不人妻| 日韩有码中文字幕| 两性午夜刺激爽爽歪歪视频在线观看 | av福利片在线| 亚洲色图综合在线观看| 亚洲国产看品久久| 丝袜人妻中文字幕| 黑人欧美特级aaaaaa片| 欧美日韩亚洲高清精品| 男女边摸边吃奶| 老司机深夜福利视频在线观看 | 欧美一级毛片孕妇| 国产精品一二三区在线看| 91av网站免费观看| 亚洲国产欧美在线一区| 热re99久久精品国产66热6| 满18在线观看网站| 久久国产亚洲av麻豆专区| 久久久欧美国产精品| 爱豆传媒免费全集在线观看| 精品国产超薄肉色丝袜足j| 欧美日韩中文字幕国产精品一区二区三区 | xxxhd国产人妻xxx| 少妇精品久久久久久久| 亚洲熟女精品中文字幕| 亚洲精品国产av成人精品| 久久久欧美国产精品| 99香蕉大伊视频| 王馨瑶露胸无遮挡在线观看| 午夜免费观看性视频| 日韩有码中文字幕| 超碰成人久久| 久热这里只有精品99| 人人妻人人澡人人看| 一区二区三区乱码不卡18| 国产真人三级小视频在线观看| 成年人黄色毛片网站| 免费在线观看视频国产中文字幕亚洲 | 亚洲黑人精品在线| 91老司机精品| 国产精品影院久久| 亚洲激情五月婷婷啪啪| 中文字幕高清在线视频| 久久亚洲精品不卡| 欧美日韩一级在线毛片| 欧美日韩av久久| 久久久国产精品麻豆| 一级毛片电影观看| 精品亚洲成国产av| 亚洲熟女精品中文字幕| 9热在线视频观看99| 国产一卡二卡三卡精品| 午夜视频精品福利| 国产一区二区激情短视频 | 国产欧美日韩一区二区精品| xxxhd国产人妻xxx| 国产免费av片在线观看野外av| 最新在线观看一区二区三区| 热re99久久精品国产66热6| 美女脱内裤让男人舔精品视频| 91老司机精品| 国产一卡二卡三卡精品| 成人国语在线视频| 亚洲三区欧美一区| 欧美激情高清一区二区三区| 日本av手机在线免费观看| 精品亚洲成a人片在线观看| 麻豆av在线久日| 日日夜夜操网爽| 免费少妇av软件| 国产黄色免费在线视频| 亚洲欧美一区二区三区久久| 日韩精品免费视频一区二区三区| 免费人妻精品一区二区三区视频| 亚洲色图综合在线观看| 国产又爽黄色视频| 亚洲美女黄色视频免费看| 一本综合久久免费| 国产一区二区激情短视频 | 免费少妇av软件| 精品国产一区二区久久| 久久久精品区二区三区| 亚洲精品中文字幕一二三四区 | 亚洲av片天天在线观看| 欧美黄色片欧美黄色片| 美女高潮喷水抽搐中文字幕| 日本精品一区二区三区蜜桃| 色综合欧美亚洲国产小说| 免费在线观看影片大全网站| 亚洲av日韩在线播放| 午夜福利视频精品| 亚洲精品美女久久久久99蜜臀| 国产精品一区二区在线不卡| 久久国产精品男人的天堂亚洲| 一本色道久久久久久精品综合| 韩国精品一区二区三区| 亚洲美女黄色视频免费看| 美女国产高潮福利片在线看| 国产精品一区二区在线观看99| 亚洲精品久久午夜乱码| 国产av一区二区精品久久| 可以免费在线观看a视频的电影网站| 亚洲国产成人一精品久久久| 亚洲精品日韩在线中文字幕| 不卡av一区二区三区| 国产免费现黄频在线看| 中文精品一卡2卡3卡4更新| 一区二区三区激情视频| 黄色视频,在线免费观看| 国产亚洲午夜精品一区二区久久| 久久久久久免费高清国产稀缺| 99国产综合亚洲精品| 亚洲精品久久午夜乱码| 欧美变态另类bdsm刘玥| 69精品国产乱码久久久| 熟女少妇亚洲综合色aaa.| 日韩大片免费观看网站| 亚洲三区欧美一区| 亚洲欧美一区二区三区黑人| 久久人人97超碰香蕉20202| 国产成人系列免费观看| 日本av免费视频播放| 水蜜桃什么品种好| 久久人妻福利社区极品人妻图片| 久久久久精品国产欧美久久久 | 欧美黑人欧美精品刺激| 久久久久精品国产欧美久久久 | 人成视频在线观看免费观看| 日日摸夜夜添夜夜添小说| 欧美亚洲日本最大视频资源| 国产一级毛片在线| 最新的欧美精品一区二区| 老司机在亚洲福利影院| 男女之事视频高清在线观看| 9191精品国产免费久久| 欧美日本中文国产一区发布| 亚洲精品久久午夜乱码| 亚洲精品美女久久久久99蜜臀| 搡老乐熟女国产| 久久狼人影院| 大码成人一级视频| 精品人妻一区二区三区麻豆| 日本wwww免费看| 免费在线观看影片大全网站| 久久久久国内视频| 女性被躁到高潮视频| 精品国产乱码久久久久久男人| 精品少妇久久久久久888优播| 国产精品国产av在线观看| 首页视频小说图片口味搜索| 动漫黄色视频在线观看| 免费女性裸体啪啪无遮挡网站| 咕卡用的链子| 亚洲人成77777在线视频| 真人做人爱边吃奶动态| 亚洲精品粉嫩美女一区| 亚洲色图综合在线观看| 大香蕉久久网| 久久 成人 亚洲| 国产三级黄色录像| 少妇猛男粗大的猛烈进出视频| 国产三级黄色录像| 美女福利国产在线| 久久久国产精品麻豆| 大片免费播放器 马上看| 国产成人精品在线电影| 亚洲 欧美一区二区三区| 国产在线免费精品| 精品卡一卡二卡四卡免费| 亚洲性夜色夜夜综合| 精品国产国语对白av| 久久女婷五月综合色啪小说| 大片免费播放器 马上看| 久久人妻福利社区极品人妻图片| 精品久久久精品久久久| 天堂中文最新版在线下载| 色老头精品视频在线观看| av超薄肉色丝袜交足视频| 老司机在亚洲福利影院| 视频在线观看一区二区三区| 国产精品一区二区免费欧美 | 狠狠精品人妻久久久久久综合| 午夜激情久久久久久久| 老熟妇仑乱视频hdxx| 亚洲精华国产精华精| 欧美日韩国产mv在线观看视频| 久久中文字幕一级| a 毛片基地| 桃红色精品国产亚洲av| 国产一级毛片在线| 日韩一卡2卡3卡4卡2021年| 久久国产精品男人的天堂亚洲| 日本猛色少妇xxxxx猛交久久| a级片在线免费高清观看视频| 淫妇啪啪啪对白视频 | 日本vs欧美在线观看视频| 精品亚洲成a人片在线观看| 菩萨蛮人人尽说江南好唐韦庄| 亚洲国产毛片av蜜桃av| www.精华液| 宅男免费午夜| 免费一级毛片在线播放高清视频 | 中文字幕制服av| 视频区图区小说| 91成人精品电影| 日韩中文字幕视频在线看片| 亚洲三区欧美一区| 男女床上黄色一级片免费看| 人人妻人人添人人爽欧美一区卜| 国产亚洲欧美在线一区二区| 咕卡用的链子| 狠狠狠狠99中文字幕| 曰老女人黄片| 欧美精品一区二区免费开放| 国产欧美日韩一区二区三区在线| 极品人妻少妇av视频| 午夜影院在线不卡| svipshipincom国产片| 国产伦理片在线播放av一区| 精品少妇久久久久久888优播| 日韩熟女老妇一区二区性免费视频| 中文字幕高清在线视频| 少妇裸体淫交视频免费看高清 | 最新在线观看一区二区三区| 日韩欧美一区视频在线观看| 黑人欧美特级aaaaaa片| 国产一区二区激情短视频 | 大型av网站在线播放| 韩国高清视频一区二区三区| 亚洲欧美成人综合另类久久久| 午夜福利视频在线观看免费| 久久久国产一区二区| 亚洲,欧美精品.| 日日爽夜夜爽网站| 欧美激情高清一区二区三区| 九色亚洲精品在线播放| 成人手机av| 成年av动漫网址| 在线av久久热| 热99久久久久精品小说推荐| xxxhd国产人妻xxx| 99国产综合亚洲精品| 岛国在线观看网站| 中国美女看黄片| 午夜视频精品福利| 久久久久久亚洲精品国产蜜桃av| 日韩制服丝袜自拍偷拍| 777米奇影视久久| 国产又色又爽无遮挡免| 国产av国产精品国产| 狠狠婷婷综合久久久久久88av| 亚洲熟女毛片儿| 性少妇av在线| kizo精华| 亚洲av电影在线观看一区二区三区| videosex国产| www日本在线高清视频| 亚洲精品久久久久久婷婷小说| 久久久久久久国产电影| 十分钟在线观看高清视频www| 日韩欧美一区二区三区在线观看 | 国产精品久久久av美女十八| 欧美精品av麻豆av| 久久精品人人爽人人爽视色| 下体分泌物呈黄色| 99精品久久久久人妻精品| 黄网站色视频无遮挡免费观看| 男女无遮挡免费网站观看| 国产成人啪精品午夜网站| 亚洲视频免费观看视频| 亚洲色图综合在线观看| 久久人妻福利社区极品人妻图片| 久久久久国产精品人妻一区二区| 亚洲人成电影免费在线| 国产精品麻豆人妻色哟哟久久|