    C/SiOC Composites by a Modified PIP Using Solid Polysiloxane:Fabrication,Microstructure and Mechanical Properties

    2019-12-28 01:28:16WUQingQingWANGZhenDINGQiNIDeWeiKANYanMeiDONGShaoMing
    無機材料學報 2019年12期

    WU Qing-Qing,WANG Zhen,DING Qi,4,NI De-Wei,KAN Yan-Mei,DONG Shao-Ming

    (1.The State Key Lab of High Performance Ceramics and Superfine Microstructures,Shanghai Institute of Ceramics,Chinese Academy of Sciences,Shanghai 200050,China;2.University of Chinese Academy of Sciences,Beijing 100049,China;3.Structural Ceramics and Composites Engineering Research Center,Shanghai Institute of Ceramics,Chinese Academy of Sciences,Shanghai 200050,China;4.ShanghaiTech University,Shanghai 201210,China;5.Center of Materials Science and Optoelectronics Engineering,University of Chinese Academy of Sciences,Beijing 100049,China)

    Abstract:A modified polymer infiltration and pyrolysis method (PIP) was developed to enhance the densification of C/SiOC composites,using molten MK resin (polymethylsilsesquioxane) as precursor.Organic sulfonic acid was added as cross-linking agent to lower the curing temperature.The cross-linking mechanism and ceramization behavior of MK resin was studied.A high ceramic yield of about 85wt% and low free carbon content below 3wt% are achieved,with excellent high-temperature stability of the derived SiOC.The modified PIP approach presents a high densification efficiency.After only 8 PIP cycles,the final C/SiOC composites possess a density of about 1.81 g/cm3.Compared with those composites fabricated by conventional PIP process,the C/SiOC composites prepared by modified PIP process show a much denser microstructure with much more improved densification efficiency.Bending strength of the as-fabricated C/SiOC composites is of (312±25) MPa,showing obvious non-brittle fracture behavior.

    Key words:C/SiOC composite;high-efficient PIP;microstructure;cross-linking mechanism

    Continuous fiber reinforced ceramic matrix composites (CFRCMCs) have been considered as excellent structure materials for the applications requiring low specific weight,high strength and toughness at elevated temperature[1-2].Generally,several approaches can be used for the fabrication of CFRCMCs,such as chemical vapor infiltration (CVI),slurry infiltration (SI),and precursor infiltration and pyrolysis (PIP),etc.[3-4].Among these methods,the PIP route is getting increasing attention in recent years,due to its advantages in low processing temperature,controllable ceramic compositions,suitable for large-scale components fabrication with complicated shapes and low cost[5-6].

    As a type of amorphous ceramic,SiOC can be considered as an anionic modification of silica glass in which Si-O bonds are partially replaced by Si-C bonds,and the other carbon atoms,free carbon,form graphene-like layers[7],which are expected to improve the thermal and mechanical properties for the applications at high temperatures[8-9].Owing to the advantages such as excellent high temperature stability,oxidization resistance and low cost,polymer-derived silicon oxycarbides (SiOC) ceramics attract lots of attention being of CRFCMCs.As reported,C/SiOC composites showed excellent mechanical performance,which was fabricated by using polysiloxane(PSO) as SiOC precursor[10].In recent years,liquid hydrogen-containing PSO or polymethyl(phenyl)siloxane flake was used as precursor for SiOC.Their pyrolysates at 1000 ℃ have relatively high content of free carbon(about 26wt% or even 29wt%)[11-12],which can easily react with SiO2phase at high temperature,leading to high-temperature instability of composites.Among the common polysiloxanes,MK resin is a carbon-poor precursor for SiOC ceramic with carbon content of about 14wt% and only about 8wt% free carbon[13-14],which makes MK resin a promising precursor for C/SiOC composites.

    In the present study,a modified PIP process with high efficiency was developed to fabricate C/SiOC composites based on MK resin.The cross-linking and pyrolysis behavior of MK resin was optimized and the crosslinking mechanism was studied.The microstructures and mechanical properties of C/SiOC composites fabricated through the modified PIP process were investigated.

    1 Experimental

    A commercially available polysiloxane (MK resin,Wacker GmbH,Burghausen,Germany) was used as the precursor for SiOC matrix.As reported in literature[15-17],MK resin in state of white powders,possessesca.2mol%of cross-linkable hydroxy and ethoxy groups with[CH3SiO1.5]nbasic structure referred as polymethylsilsesquioxane.Its possible structure is depicted in Fig.1[15].To lower the curing temperature and shorten the curing period,organic sulfonic acid was chosen as crosslinking agent (henceforth referred as CLA).

    MK resin was firstly compacted into a cylindroid tablet with a diameter of 10 mm,to investigate its softening behavior.The photograph and the size of the tablet were recordedin situas a function of temperature by a high temperature real-time observation and test system (TOMAC,FRAUNHOFER- GESELLSCHAFT,Germany) at a heating rate of 1 ℃/min in vacuum.The viscosity of MK resin at different temperatures and the dynamic modulus at 160 ℃ were measured by a rheometer (MCR301,Anton Paar GmbH,Austria).In order to investigate the curing mechanism,the functional groups of PSO before and after cross-linking process were analyzed by a FT-IR spectroscopy (NICOLET ls10,Thermo Scientific,America).To investigate ceramization behavior of MK resin,the thermogravimetric (TG) and differential thermal analysis (DTA) were performed with MK resin on a STA 449/F3 simultaneous thermal analyzer (Netzsch,Germany).The heating rate for DTA measurement was 10 ℃/min in flowing Ar.Content of oxygen and carbon atoms were analyzed by oxygen/ nitrogen detertminator (TC600C,LECO,America) and carbon/ sulfur detertminator(CS2000,ELTRA,Germany),respectively.

    Three-dimensional needle-punched carbon fiber preforms fabricated with T700SC carbon fiber (12 K) were used as the reinforcement in this study.MK resin with different contents of CLA was cross-linked at 160 ℃ in vacuum and then pyrolyzed at 1000 ℃ in Ar atmosphere.A modified PIP process illustrated in Fig.2 was performed to fabricate the C/SiOC composites.Following this process,the composites with dense matrix can be achieved.In the modified PIP process,MK resin with CLA was firstly heated to melt,and then was infiltrated into the fiber preform placed in a flexible container with aids of pressure difference between inside and outside of the flexible container.Secondly,the infiltrated preform was cured at 160 ℃ for 6 h.Thirdly,the cured specimens were pyrolyzed at 1000 ℃ for 30 min at a heating rate of 5 ℃/min in Ar atmosphere,and then cooled down to room temperature.PIP process was repeated for 8 times to get C/SiOC composites with high densities.As a contrast,a conventional PIP process with ethanol solution of MK resin being used as precursor was utlized to fabricate C/SiOC composites.To clearly distinguish between the two kinds of C/SiOC composites,the C/SiOC composites fabricated by the modified PIP process is henceforth referred as M-C/SiOC composites,and the C/SiOC composites fabricated by the conventional PIP process is referred as C-C/SiOC composites.

    The densities as well as open porosities of the C/SiC composites were measured by Archimedes method with deionized water as the immersion medium.The bending strength of the final composites was characterized by three-point bending test (DDL20,Changchun Research Institute for Mechanical Science Co.Ltd,Changchun,China) with a span length of 50 mm and a crosshead speed of 0.5 mm/min.The dimensions of the specimens for three-point bending test were 60 mm×6 mm ×4 mm.Microstructures of composites were observed on both the fracture surfaces and polished cross-sections using a field-emission scanning electron microscope (Hitachi SU8220,Japan).

    Fig.1 Scheme of the possible structure of MK resin[15]

    Fig.2 Schematic diagram of the modified PIP process

    2 Results and discussion

    2.1 Viscosity-temperature characteristics of MK resin

    The viscosity of precursor is a key parameter for control of the PIP process.The high viscosity of precursor would lead to a poor fluidity during the impregnation process,while the excessively low viscosity would make the precursor easily flow out of the preforms during the crosslinking process[18].Therefore,the viscosity of MK resin was investigated firstly as a function of temperature.Softening point was determined by the change of geometric size of the MK resin as shown in Fig.3(a).It can be observed that there is no obvious deformation of MK resin at temperature below 55 ℃,while the right angle turned into round ones when the temperature was rising above 60 ℃.It reveals that the softening point of MK resin is in the range of 55-60 ℃.As shown in Fig.3(b),it is clear that the viscosity of MK resin drops sharply at temperature higher than 110 ℃.The viscosities of MK resin are about 100 mPa?s at 150 ℃,144 mPa?s at 160 ℃ and 87 mPa?s at 170 ℃,respectively.

    Fig.3 (a) Change of geometric size of MK resin as a function of temperature;(b) Temperature dependence of the viscosity of MK resin

    2.2 Curing and ceramization behavior of MK resin

    As a kind of thermoplastic polymer,MK resin begins to cross-link above 250 ℃,while the low viscosity can lead to waste of precursor during the pyrolysis.To lower the curing temperature,CLA was applied as crosslinking agent considering the cross-linkable hydroxy and ethoxy groups.

    CLA of various contents (1wt%,0.5wt%,0.1wt%,0.05wt%,and 0.01wt%) were added into MK resin to pick out the most suitable ratio.The optical photographs of MK resin with different contents of CLA heated at 160 ℃ are shown in Fig.4,and the weight losses are also labeled.It can be observed that when no CLA was added,MK resin kept in the liquid state even after being heated at 160 ℃ for 12 h and the weight loss is only 0.67wt%.With the addition of CLA,MK resin can convert into solid state and the weight loss increased,which meant CLA could effectively promote the cross-linking of MK resin.When the content of CLA was higher than 0.1wt%,MK resin can get cross-linked within 30 min.When 1wt% CLA was added,the cross-linking time was as short as 5 min and the weight loss increased to 3.32wt%.When the content of CLA decreased to 0.05wt% and 0.01wt%,the cross-linking time increased to about 1 and 3 h,respectively.It can also be observed that when more than 0.05wt% CLA was added,the crosslinked precursor presented a porous structure,which may be caused by escaping of generated gases during the cross-linking.

    Rheological parameters such as storage modulus (G')and loss modulus (G") were employed to further evaluate the curing behavior of MK resin.For the sake of convenience,MK resin with 0.05wt% CLA was selected for rheological test.As shown in Fig.5,storage moduli and loss moduli kept constant at the beginning of the test and then increased slowly until 1000 s.Two moduli increased sharply after 1000 s,and there was an intersection point ofG'andG"at about 1970 s.After the intersection point,theG'exceededG",which indicated that the elastic deformation of MK resin was dominant rather than viscous deformation of materials.Furthermore,the polymer began to transform into elastomer.The gel point of MK resin,on which the polymer begins to crosslink,can be determined by the intersection point ofG'andG"[19].It can be concluded that MK resin with 0.05wt% CLA began to crosslink after being treated at 160 ℃ for 0.5 h,which is in consistent with the phenomenon referred above.

    To investigate the curing mechanism,FT-IR spectroscopy of the as-received MK resin (without cross-linking)and MK resin with 0.01wt% CLA cured at 160 ℃ were tested (Fig.6).The spectrum of MK resin shows absorption bands atv=765,1275 cm-1(Si-CH3),v=2913,2975 cm-1(C-H),v=1618,3437 cm-1(Si-OH),v=1023 cm-1(Si-O-C) andv=1111 cm-1(Si-O-Si),as previously reported[16,20-23].As the curing time increases,the intensity of absorption bands assigned to Si-O-C and Si-O-Si slightly increases.What's more,the intensities of Si-O-Si and Si-O-C increases with curing time,indicating that the network of Si-O-Si was gradually formed.It can be concluded that condensation reactions of Si-OH with Si-OH,Si-OEt as well as with RSO2-OH groups with the aids of CLA are main reactions involved during cross-linking.

    Fig.4 Optical photographs of MK resin with different contents of CLA after heat treatment at 160 ℃

    Fig.5 Storage moduli and loss moduli versus curing time for MK resin with 0.05wt% CLA at 160 ℃

    Fig.6 (a) Cross-linking reactions during the curing process;(b) FT-IR spectra of as-obtained MK resin without curing and MK resin with 0.01wt% CLA after curing at 160 ℃ for different time;(c) details in enlarged view of wavenumber in the range from 1250 cm-1 to 500 cm-1

    FT-IR spectroscopy of the cured MK resins with different contents of CLA were also tested as shown in Fig.7.There is no obvious difference in their IR spectra except for the absorption bands for Si-O (at 1023 and 1111 cm-1) and -OH (at 1618 and 3437 cm-1).As the CLA content increases,the intensity ratio of Si-O-Si and Si-O-C absorption increases,which reveals that CLA affects curing rate and cross-linking degree of MK resin.Excessively rapid cross-linking rate results in generation of a mass of small molecules such as ethanol and H2O which fails to volatilize before Si-O-Si network is formed,and is then absorbed in porous structure of the cured MK resin.Consequently,the intensity of -OH bands show a remarkable increase.

    Fig.7 FT-IR spectra of MK resin with various contents of CLA after being treated at 160 ℃ for 8 h

    Fig.8 TGA-DTA curves of the decomposition behavior for MK resin

    TG-DTA curves of MK resin without CLA from 100 ℃ to 1000 ℃ were shown in Fig.8.The ceramic yield is as high as 88wt% after pyrolyzation at 1000 ℃.The weight loss mainly occurred in two temperature ranges.A weight loss of about 4.91wt% occurred at temperatures ranging from 170 ℃ to 350 ℃,which may be ascribed to the vaporization of H2O,n-propanol,ethanol and POSS during the cross-linking process[16,23-26].A further weight loss of about ~6.09wt% occurs between 350 and 900 ℃,which may be resulted from breakage/rearrangement of molecular chains and release of a large number of small molecular gas,such as H2,H2O and propane,etc.[15,22].Table 1 shows the ceramic yields of MK resin with different CLA contents pyrolized at 1000 ℃ in Ar atmosphere and the chemical compositions of the pyrolysates in the formation ofxSiO2·ySiC·zC.The ceramic yields of MK resin with different contents of CLA ranges from 82.9wt% to 85.6wt%,which means that the effect of CLA on the ceramic yield is negligible.It is indicated that free carbon is less than 3wt% in pyrolysates.

    2.3 Microstructures and mechanical properties of C/SiOC composites

    Based on the above-mentioned cross-linking and pyrolysis behavior of MK resin with different CLA contents,it is found that the MK resin with 0.01wt% of CLA is a suitable matrix precursor for the fabrication of C/SiOC composites,which can guarantee enough time for the molten precursor to be infiltrated into the fiber preform.During the PIP process,the precursor was first cross-linked at 160 ℃ for 4 h before pyrolysis.

    Fig.9 shows the density and the open porosity of C/SiOC composites as a function of PIP cycles.It is obvious that the density increases with the increase of PIP cycles,and the open porosity decreases.As a result of high ceramic yield of precursor as well as eliminating effect of solvent,the high efficiency in modified PIP was realized in comparation with the conventional ones.Remarkably,the open porosity of M-C/SiOC composites(6.2%) is much lower than that of C-C/SiOC composites(17.4%) after 8 cycles.After the first cycle,the density of M-C/SiOC composites increased from 0.6 g/cm3to 1.14 g/cm3.Compared with the C-C/SiOC composites,the final M-C/SiOC composite possessed relatively high density of about 1.81 g/cm3after the eighth cycle.Similarly,the density of C/SiOC composites fabricatedviathe modified PIP process in this work is increased by about 10% in comparation with the results of 1.64 g/cm3in the reported literature[27].

    Fig.10 shows the cross-sectional microstructures of the final C/SiOC composites fabricated by two different PIP processes.Compared with the C-C/SiOC composites(Fig.10(a)),the inter-bundle pores in M-C/SiOC composites is obviously much less (Fig.10(b)).Although some pores can still be found in the matrices,the final M-C/SiOC composites are highly dense in general.When the preforms were infiltratedviathe modified PIP process,the precursors with moderate viscosity can fill in almost all pores and turn into solid state during the cross-link process.The existence of sevaral micro-pores and microcracks in matrices (Fig.10(b-d)) can be attributed to generation of close pores resulted from porous precursor pyrolysates during the precious PIP cycles.Therefore,the precursor can't reach anymore in the latter infiltration process.

    Table 1 The ceramic yield and the element composition for MK resin with different CLA contents pyrolized at 1000 ℃

    Fig.9 Density and open porosity variation of C/SiOC composites during the PIP process

    Fig.10 SEM images of the polished cross sections of (a)C-C/SiOC composites;(b-d) M-C/SiOC composites

    Fig.11 Typical bending stress vs.strain curve for the C/SiOC composites

    Fig.12 SEM micrographs of the fracture surfaces of M-C/SiOC composites

    The three-point-bending test shows that the M-C/SiOC composites possess a relatively higher bending strength of (312±25) MPa than the C-C/SiOC composites with a bending strength of (211±7) MPa.The M-C/SiOC composites also show superiority in mechanical properties as compared to the C/SiOC composites prepared by conventional PIP process with other polysiloxane precursors reported (217[28],247[29]and 265[1]).The M-C/SiOC composites show a typical non-brittle fracture behavior,which can be concluded from the bending stress-strain curves of three-point bending test as shown in Fig.11.The stress-strain curve of the M-C/SiOC composites can be divided into three regions,namely,linear region,non-linear region and fracture region.In the non-linear region,micro-cracks generation and propagation as well as the interfacial debonding are responsible for the pseudo-plastic deformation behavior[30].Once the stress reaching to the maximum as observed in the fracture region,the stress drops abruptly.Then the stress show a step-like decrease,which may be ascribed to the layer-fiber-distribution characteristics of the preforms.At the beginning of three-point-bending test,fibers on the underside layer have the largest deformation.When fibers at this layer was destroyed,the second layer of fibers momentarily bear the load,therefore the imposed load dropped abruptly,then slightly increased again.Meanwhile,the C-C/ SiOC composites show a narrower non-linear region,leading to the worse bending strength.

    Fig.12 shows the microstructure of fracture surfaces of the M-C/SiOC composites.Pulled-out fibers can be observed in the SiOC matrix.As the deposited PyC interphase ensures the weak bonding between matrix and fiber,cracks can propagate either along the matrix-PyC interface or along PyC-fiber interphase.Therefore,the de-bonding phenomenon can be observed on the surface of the pulled-out fibers.

    3 Conclusion

    Based on a modified highly-efficient PIP process using molten MK resin,C/SiOC composites with a density of 1.81 g/cm3was fabricated by only 8 cycles of PIP.When MK resin with 0.01wt% CLA was firstly crosslinked at 160 ℃ for 4 h,precursor can tranform into solid state and fill in both inter-bundle pores and intrabundle pores,therefore only very small amount of micropores can be found in the composites.The as-fabricated C/SiOC composites possess a relatively high bending strength of (312±25) MPa and show an obvious nonbrittle fracture behavior.

    大片电影免费在线观看免费| 国产老妇伦熟女老妇高清| 少妇粗大呻吟视频| 十八禁网站网址无遮挡| 丝袜人妻中文字幕| 一级片免费观看大全| 国产有黄有色有爽视频| 交换朋友夫妻互换小说| 亚洲美女黄色视频免费看| 18禁黄网站禁片午夜丰满| 夜夜夜夜夜久久久久| 亚洲国产av影院在线观看| 久久久久国产一级毛片高清牌| 法律面前人人平等表现在哪些方面 | 免费在线观看视频国产中文字幕亚洲 | 色婷婷久久久亚洲欧美| 久久久国产欧美日韩av| 国产亚洲精品久久久久5区| 国产麻豆69| 中文字幕av电影在线播放| 黄网站色视频无遮挡免费观看| 日韩欧美一区视频在线观看| 伊人亚洲综合成人网| 精品久久蜜臀av无| 9热在线视频观看99| 无遮挡黄片免费观看| 久久女婷五月综合色啪小说| 国产欧美日韩综合在线一区二区| 久久国产精品人妻蜜桃| 亚洲成人免费电影在线观看| 欧美激情 高清一区二区三区| 亚洲一区二区三区欧美精品| 中国国产av一级| 又紧又爽又黄一区二区| 人妻 亚洲 视频| 欧美在线一区亚洲| 成人18禁高潮啪啪吃奶动态图| 亚洲专区国产一区二区| 免费在线观看完整版高清| 欧美精品一区二区大全| 日韩有码中文字幕| 十八禁人妻一区二区| 天天操日日干夜夜撸| 国产色视频综合| 最黄视频免费看| 一级毛片电影观看| 啦啦啦啦在线视频资源| av有码第一页| av片东京热男人的天堂| 色老头精品视频在线观看| 久久国产精品男人的天堂亚洲| 91av网站免费观看| 老司机福利观看| 女性被躁到高潮视频| 日本欧美视频一区| 纵有疾风起免费观看全集完整版| 性色av乱码一区二区三区2| 免费高清在线观看日韩| 五月开心婷婷网| 国产一区二区三区在线臀色熟女 | 国产精品 国内视频| 最新的欧美精品一区二区| 免费人妻精品一区二区三区视频| 麻豆国产av国片精品| 别揉我奶头~嗯~啊~动态视频 | 国产精品影院久久| 国产成人系列免费观看| 久久av网站| 电影成人av| 亚洲avbb在线观看| 欧美精品啪啪一区二区三区 | 久久99一区二区三区| 一级片'在线观看视频| 久久久久网色| 亚洲,欧美精品.| 国产黄色免费在线视频| 亚洲国产精品一区三区| 18禁观看日本| 久久99一区二区三区| 欧美中文综合在线视频| 蜜桃国产av成人99| 国产av精品麻豆| av片东京热男人的天堂| 欧美国产精品va在线观看不卡| 男人添女人高潮全过程视频| 纵有疾风起免费观看全集完整版| 亚洲国产精品一区三区| 欧美亚洲日本最大视频资源| 女人久久www免费人成看片| 一区二区av电影网| 女性被躁到高潮视频| 久久久精品免费免费高清| 亚洲精品自拍成人| 一区二区三区四区激情视频| 欧美+亚洲+日韩+国产| 黑丝袜美女国产一区| 国产97色在线日韩免费| 97精品久久久久久久久久精品| 久久久欧美国产精品| 大香蕉久久成人网| 精品久久久精品久久久| avwww免费| 午夜福利在线观看吧| 亚洲av电影在线观看一区二区三区| 性色av一级| 老汉色av国产亚洲站长工具| 夜夜夜夜夜久久久久| 色婷婷久久久亚洲欧美| 人妻一区二区av| 久久香蕉激情| 高清欧美精品videossex| 搡老岳熟女国产| 国产精品 国内视频| 久久热在线av| 自线自在国产av| 少妇裸体淫交视频免费看高清 | 女人高潮潮喷娇喘18禁视频| 老鸭窝网址在线观看| 国产激情久久老熟女| 99热全是精品| 亚洲精品国产精品久久久不卡| 日本vs欧美在线观看视频| 中文字幕精品免费在线观看视频| 久久天堂一区二区三区四区| 久久久精品国产亚洲av高清涩受| 黄色视频在线播放观看不卡| 亚洲国产日韩一区二区| 777米奇影视久久| 久久久久久久精品精品| 韩国精品一区二区三区| 国产有黄有色有爽视频| 欧美少妇被猛烈插入视频| 婷婷色av中文字幕| 亚洲av日韩精品久久久久久密| 操美女的视频在线观看| a级毛片黄视频| 久久久欧美国产精品| 免费观看a级毛片全部| 亚洲av成人一区二区三| 国产主播在线观看一区二区| 国产福利在线免费观看视频| 各种免费的搞黄视频| 少妇的丰满在线观看| 母亲3免费完整高清在线观看| 视频区图区小说| 黑人欧美特级aaaaaa片| 婷婷色av中文字幕| 亚洲精品一二三| 成在线人永久免费视频| 91国产中文字幕| 日韩视频一区二区在线观看| 热99re8久久精品国产| 中文字幕精品免费在线观看视频| av天堂在线播放| 亚洲性夜色夜夜综合| 菩萨蛮人人尽说江南好唐韦庄| 国产高清videossex| 水蜜桃什么品种好| 一区福利在线观看| 亚洲欧美精品自产自拍| 夜夜夜夜夜久久久久| 久久 成人 亚洲| 国产成人欧美| 美女高潮到喷水免费观看| 波多野结衣一区麻豆| 精品一区二区三区av网在线观看 | 纵有疾风起免费观看全集完整版| 99精品久久久久人妻精品| 亚洲精品乱久久久久久| 精品少妇久久久久久888优播| 高清欧美精品videossex| 每晚都被弄得嗷嗷叫到高潮| 国产精品久久久av美女十八| 国产一区二区三区综合在线观看| 在线看a的网站| 精品熟女少妇八av免费久了| av网站在线播放免费| 一级毛片精品| 亚洲精品国产区一区二| 在线观看免费视频网站a站| 成年美女黄网站色视频大全免费| 久久精品久久久久久噜噜老黄| 成人三级做爰电影| 欧美激情高清一区二区三区| 一区二区三区精品91| 大片电影免费在线观看免费| 久久99热这里只频精品6学生| 国产精品免费视频内射| 日本欧美视频一区| 成人免费观看视频高清| 亚洲五月婷婷丁香| 国产激情久久老熟女| 亚洲专区字幕在线| 丝瓜视频免费看黄片| 免费在线观看完整版高清| 狠狠狠狠99中文字幕| 三级毛片av免费| 淫妇啪啪啪对白视频 | 亚洲,欧美精品.| 亚洲av男天堂| 12—13女人毛片做爰片一| 日本a在线网址| 亚洲情色 制服丝袜| 丁香六月天网| 操出白浆在线播放| 狂野欧美激情性bbbbbb| 亚洲九九香蕉| 两个人看的免费小视频| 日本91视频免费播放| 在线观看免费日韩欧美大片| 我要看黄色一级片免费的| 亚洲久久久国产精品| 国产成人欧美在线观看 | 91九色精品人成在线观看| 午夜激情av网站| 啦啦啦视频在线资源免费观看| 亚洲五月色婷婷综合| 一区二区日韩欧美中文字幕| a级毛片在线看网站| 欧美大码av| 老司机靠b影院| 欧美黑人欧美精品刺激| 制服诱惑二区| 97精品久久久久久久久久精品| 黑丝袜美女国产一区| 亚洲国产精品一区三区| 天天影视国产精品| 亚洲国产av影院在线观看| 国产视频一区二区在线看| 欧美激情高清一区二区三区| 久久久久久久精品精品| 亚洲精品一二三| 国产97色在线日韩免费| 999久久久精品免费观看国产| 亚洲欧美精品自产自拍| 99九九在线精品视频| 欧美黄色片欧美黄色片| 国产成人啪精品午夜网站| 好男人电影高清在线观看| 午夜福利在线观看吧| 午夜福利影视在线免费观看| 视频区欧美日本亚洲| 成人影院久久| 97在线人人人人妻| 后天国语完整版免费观看| 在线 av 中文字幕| videosex国产| 亚洲情色 制服丝袜| 巨乳人妻的诱惑在线观看| 午夜精品久久久久久毛片777| 老司机在亚洲福利影院| 肉色欧美久久久久久久蜜桃| 大片免费播放器 马上看| 久久中文看片网| 老司机午夜福利在线观看视频 | 飞空精品影院首页| 汤姆久久久久久久影院中文字幕| 亚洲国产精品成人久久小说| 欧美xxⅹ黑人| 亚洲欧美清纯卡通| 久久久国产精品麻豆| 国产高清国产精品国产三级| av免费在线观看网站| 国产一区二区三区综合在线观看| 99热网站在线观看| 亚洲精品国产区一区二| 午夜福利在线观看吧| 亚洲情色 制服丝袜| 精品亚洲成a人片在线观看| 欧美成狂野欧美在线观看| 在线 av 中文字幕| 国产免费福利视频在线观看| 国产亚洲精品一区二区www | 国产在线视频一区二区| www.熟女人妻精品国产| 久热这里只有精品99| 十分钟在线观看高清视频www| 在线亚洲精品国产二区图片欧美| 两性夫妻黄色片| 精品福利观看| 国产精品久久久久久人妻精品电影 | 中文字幕av电影在线播放| 久久中文看片网| 欧美另类亚洲清纯唯美| 精品国产一区二区三区四区第35| 亚洲第一欧美日韩一区二区三区 | 午夜福利一区二区在线看| 18禁裸乳无遮挡动漫免费视频| 亚洲全国av大片| 久久精品亚洲av国产电影网| 日韩中文字幕欧美一区二区| 亚洲精品久久久久久婷婷小说| 色老头精品视频在线观看| 成在线人永久免费视频| 黑人操中国人逼视频| www.av在线官网国产| 青春草亚洲视频在线观看| 在线观看免费视频网站a站| 国产区一区二久久| 悠悠久久av| 汤姆久久久久久久影院中文字幕| 亚洲精品成人av观看孕妇| 亚洲欧美一区二区三区黑人| 热99国产精品久久久久久7| 久久久国产精品麻豆| 久久99热这里只频精品6学生| 宅男免费午夜| av天堂久久9| 日韩 欧美 亚洲 中文字幕| 亚洲免费av在线视频| 午夜视频精品福利| 日韩有码中文字幕| 自线自在国产av| 午夜精品久久久久久毛片777| 丰满饥渴人妻一区二区三| av超薄肉色丝袜交足视频| 超碰成人久久| 在线看a的网站| 又黄又粗又硬又大视频| 香蕉丝袜av| 99久久综合免费| 国产在线免费精品| 久久久国产一区二区| 一二三四在线观看免费中文在| h视频一区二区三区| 久热这里只有精品99| 亚洲激情五月婷婷啪啪| 日日夜夜操网爽| 国产亚洲精品第一综合不卡| 免费在线观看完整版高清| 久久久国产成人免费| 美女国产高潮福利片在线看| 日韩欧美一区二区三区在线观看 | 青草久久国产| 日本av手机在线免费观看| 伊人久久大香线蕉亚洲五| 51午夜福利影视在线观看| 法律面前人人平等表现在哪些方面 | 无遮挡黄片免费观看| 免费高清在线观看视频在线观看| 国产成人精品久久二区二区免费| avwww免费| 精品国产乱码久久久久久小说| 老熟妇乱子伦视频在线观看 | av片东京热男人的天堂| 97精品久久久久久久久久精品| 国产精品九九99| 国产成人啪精品午夜网站| 中文字幕制服av| av超薄肉色丝袜交足视频| 99国产精品99久久久久| 两个人免费观看高清视频| 性少妇av在线| 丰满饥渴人妻一区二区三| 亚洲欧美一区二区三区黑人| 日日夜夜操网爽| 在线永久观看黄色视频| 欧美日韩视频精品一区| 12—13女人毛片做爰片一| 波多野结衣一区麻豆| 婷婷成人精品国产| 在线观看免费午夜福利视频| 久久精品国产a三级三级三级| 亚洲欧美成人综合另类久久久| 久久久久久久大尺度免费视频| 中文字幕人妻熟女乱码| 久久精品国产a三级三级三级| 亚洲国产av新网站| 18禁观看日本| 中国美女看黄片| www.熟女人妻精品国产| 亚洲综合色网址| 岛国在线观看网站| 考比视频在线观看| 国产极品粉嫩免费观看在线| 国产精品99久久99久久久不卡| 五月开心婷婷网| 精品一区在线观看国产| 亚洲少妇的诱惑av| 亚洲人成电影观看| 一本大道久久a久久精品| 日本精品一区二区三区蜜桃| 婷婷丁香在线五月| 18禁观看日本| 汤姆久久久久久久影院中文字幕| 午夜福利影视在线免费观看| 亚洲精品美女久久久久99蜜臀| 熟女少妇亚洲综合色aaa.| 国产精品影院久久| 后天国语完整版免费观看| a 毛片基地| 国产精品av久久久久免费| 欧美久久黑人一区二区| 亚洲视频免费观看视频| 久久热在线av| 亚洲中文av在线| 美女福利国产在线| 久久中文字幕一级| 下体分泌物呈黄色| 久久精品亚洲av国产电影网| 18禁观看日本| 国产成人欧美在线观看 | 精品福利观看| 国产精品成人在线| 三上悠亚av全集在线观看| 黄色片一级片一级黄色片| 午夜免费成人在线视频| 老司机福利观看| 午夜福利一区二区在线看| 91大片在线观看| 国产精品二区激情视频| 99久久综合免费| 欧美激情高清一区二区三区| 欧美日韩精品网址| 制服诱惑二区| av天堂在线播放| 精品久久蜜臀av无| 欧美午夜高清在线| 亚洲 欧美一区二区三区| 日韩熟女老妇一区二区性免费视频| netflix在线观看网站| 男女之事视频高清在线观看| 日韩 亚洲 欧美在线| 国产成人影院久久av| 老汉色∧v一级毛片| 亚洲少妇的诱惑av| 少妇的丰满在线观看| 久久亚洲精品不卡| 亚洲精品国产色婷婷电影| 18禁国产床啪视频网站| 丁香六月欧美| 国产伦人伦偷精品视频| 亚洲欧美日韩另类电影网站| 麻豆国产av国片精品| av线在线观看网站| 成人三级做爰电影| 欧美黄色片欧美黄色片| 国产成人精品久久二区二区免费| 久久精品国产亚洲av高清一级| 九色亚洲精品在线播放| 亚洲美女黄色视频免费看| 91字幕亚洲| 各种免费的搞黄视频| 午夜免费观看性视频| 黄片播放在线免费| 国产精品自产拍在线观看55亚洲 | 黑人操中国人逼视频| 美女脱内裤让男人舔精品视频| 国产精品久久久久成人av| 久久久久久久久久久久大奶| 国产成人欧美| 成人国产av品久久久| 久久av网站| 国产免费视频播放在线视频| 51午夜福利影视在线观看| 又紧又爽又黄一区二区| 女警被强在线播放| 男人添女人高潮全过程视频| 91老司机精品| 最近中文字幕2019免费版| 亚洲国产精品成人久久小说| 如日韩欧美国产精品一区二区三区| 日韩欧美国产一区二区入口| 成人三级做爰电影| 天堂中文最新版在线下载| 美女国产高潮福利片在线看| 两性夫妻黄色片| 老熟女久久久| 午夜久久久在线观看| 高清视频免费观看一区二区| 午夜日韩欧美国产| 欧美精品一区二区大全| 悠悠久久av| 一本—道久久a久久精品蜜桃钙片| 在线观看免费视频网站a站| 我的亚洲天堂| 中文字幕另类日韩欧美亚洲嫩草| 久久人人爽人人片av| 午夜精品久久久久久毛片777| 久久久国产欧美日韩av| 国产精品一区二区在线不卡| 国产精品一区二区在线观看99| 岛国在线观看网站| 男人操女人黄网站| 天天躁狠狠躁夜夜躁狠狠躁| 精品第一国产精品| 老司机影院毛片| 岛国在线观看网站| 国产一区二区三区av在线| 新久久久久国产一级毛片| 欧美少妇被猛烈插入视频| 岛国毛片在线播放| 欧美精品啪啪一区二区三区 | www日本在线高清视频| 嫁个100分男人电影在线观看| av线在线观看网站| 免费久久久久久久精品成人欧美视频| 亚洲精品美女久久久久99蜜臀| 国产在视频线精品| a在线观看视频网站| 久久精品国产a三级三级三级| 国产亚洲午夜精品一区二区久久| 深夜精品福利| 久久精品国产综合久久久| 啪啪无遮挡十八禁网站| 三上悠亚av全集在线观看| 老司机福利观看| 一二三四社区在线视频社区8| 亚洲欧美清纯卡通| 久久九九热精品免费| 女人高潮潮喷娇喘18禁视频| 久久ye,这里只有精品| 久久久国产精品麻豆| a 毛片基地| 国产欧美日韩综合在线一区二区| avwww免费| 一级毛片精品| 母亲3免费完整高清在线观看| 在线亚洲精品国产二区图片欧美| 熟女少妇亚洲综合色aaa.| 成年人免费黄色播放视频| 欧美精品啪啪一区二区三区 | 日韩一区二区三区影片| av片东京热男人的天堂| 亚洲,欧美精品.| 亚洲精品国产av成人精品| 桃红色精品国产亚洲av| 日本91视频免费播放| svipshipincom国产片| 亚洲精品粉嫩美女一区| 男人爽女人下面视频在线观看| 别揉我奶头~嗯~啊~动态视频 | 久久国产精品人妻蜜桃| 国产在线免费精品| 国产精品1区2区在线观看. | 肉色欧美久久久久久久蜜桃| 激情视频va一区二区三区| 两人在一起打扑克的视频| 国产一卡二卡三卡精品| 一本久久精品| 国产色视频综合| 在线观看一区二区三区激情| 脱女人内裤的视频| 亚洲av欧美aⅴ国产| 老熟妇仑乱视频hdxx| www.精华液| 91成年电影在线观看| 少妇 在线观看| 99热网站在线观看| 美女高潮喷水抽搐中文字幕| 两性午夜刺激爽爽歪歪视频在线观看 | 考比视频在线观看| 亚洲精品国产色婷婷电影| 久久亚洲国产成人精品v| 日本av手机在线免费观看| 黄色视频不卡| 精品卡一卡二卡四卡免费| 中文字幕另类日韩欧美亚洲嫩草| 岛国在线观看网站| 亚洲一区二区三区欧美精品| 国产亚洲一区二区精品| 99香蕉大伊视频| 日韩制服丝袜自拍偷拍| 十分钟在线观看高清视频www| 精品一区二区三卡| 男女国产视频网站| 十八禁网站网址无遮挡| 亚洲成人手机| 欧美xxⅹ黑人| 黑人巨大精品欧美一区二区mp4| 久久精品亚洲av国产电影网| 中文字幕制服av| 成人国产av品久久久| 亚洲欧美色中文字幕在线| 男女国产视频网站| 国产在线视频一区二区| 搡老熟女国产l中国老女人| 日本a在线网址| 国产视频一区二区在线看| 国产熟女午夜一区二区三区| 国产日韩欧美亚洲二区| 午夜久久久在线观看| 99国产精品免费福利视频| 美女国产高潮福利片在线看| 精品一区二区三区四区五区乱码| 免费在线观看完整版高清| 五月天丁香电影| 国产国语露脸激情在线看| 国产精品国产av在线观看| 亚洲专区字幕在线| 亚洲人成电影免费在线| 国产不卡av网站在线观看| 两性午夜刺激爽爽歪歪视频在线观看 | 午夜两性在线视频| 精品欧美一区二区三区在线| 亚洲av日韩精品久久久久久密| 日韩中文字幕欧美一区二区| av网站在线播放免费| 国产一区二区三区在线臀色熟女 | 成年女人毛片免费观看观看9 | 91字幕亚洲| 欧美国产精品一级二级三级| 亚洲精品美女久久av网站| 亚洲精品国产av成人精品| 侵犯人妻中文字幕一二三四区| 满18在线观看网站| 美国免费a级毛片| 亚洲精华国产精华精| 欧美日韩黄片免| 日韩有码中文字幕| 国产亚洲av片在线观看秒播厂| 美女扒开内裤让男人捅视频| 两个人免费观看高清视频| 啦啦啦中文免费视频观看日本| 亚洲性夜色夜夜综合|