    Tool Wear in Turning of Titanium Alloy after Thermohydrogen Treatment

    2012-01-20 04:45:58WEIWeihuaXUJiuhuaFUYucanandYANGShubao

    WEI Weihua,XU Jiuhua*,FU Yucan,and YANG Shubao

    College of Mechanical and Electrical Engineering,Nanjing University of Aeronautics and Astronautics,Nanjing 210016,China

    1 Introduction

    Titanium alloys have been widely used in the aerospace,biomedical,automotive and petroleum industries because of their good strength-to-weight ratio and superior corrosion resistance.However,it is very difficult to machine them due to their poor machinability[1-2].Due to their low thermal conductivity,high chemical reactivity and low modulus of elasticity,together with the effect of abrasive,adhesion,diffusion and oxidation,which gives rise to the crater wear of rake face and the wear land of flank face[3-5].If the tool wear is too quickly,the tool cost will be high,and it will affect the machining quality of workpiece and decrease the productivity.How to reduce the tool wear and the cost has become one of the primary problems in machining titanium alloys.

    In order to research the tool wear regularity in machining titanium alloys,some scholars have done some cutting tests by means of hydrogenation before machining.KOLACHEV,et al[6],investigated the effect of hydrogen on the machinability of titanium alloys of VT5-1 by cutting.The experimental results demonstrate that hydrogenation is one of the promising methods for the improvement of the machining efficiency.Alloying of VT5-1 with hydrogen decreases cutting forces and increases the tool life within a certain range of concentration of hydrogen.EGOROVA,et al[7],investigated the effect of hydrogen on the microstructure and the cutability of various classed titanium alloys VT1-0,VT8 and VT25.Experimental data showed that hydrogenation could improve the cutability of titanium alloy.EZUGWU,et al[8],studied the machinability of hydrogenation titnaium alloy such as BT1-0,BT5-1 and BT8.They found that the cutting temperature could reduced by 100-150 ℃ and cutting force reduced by 100N,meanwhile,tool life would improve 3 times when machining BT1-0 alloy with 0.3%-0.6% hydrogen at cutting speed of 40-60 m/min.Many researchers had investigated the effect of hydrogen on the machinability of titanium alloy by cutting,and they had obtained the tool life in the process of cutting the titaium alloys with various hydrogen contents,but they only researched the flank wear of the common cutting tools made of VK60M alloy,and the influence of hydrogen contents on the tool wear have been less investigated comprehensively[9-11].The present investigation is an attempt to research the influence hydrogen contents on tool wear regularity in turning hydrogenated Ti-6Al-4V alloy with analysis and discussion.

    2 Experimental Methods and Condition

    2.1 Workpiece materials

    The material used in this investigation is a forging Ti-6Al-4V alloy (TC4),its chemical compositions in mass fraction are summarized in Table 1.The unhydrogenated specimens have a diameter of 60 mm and a length of 300 mm.The hydrogenated specimens had a diameter of 60 mm and a length of 100 mm,and their hydrogenation technology is as follows:the Ti-6Al-4V alloy bars are hydrogenated in molecular hydrogen at 800℃ for 10 h in hydrogen furnace followed by furnace cooling to room temperature.The specimens with various hydrogen contents (mass fraction,w(H),%) in the range of 0%-0.5%are obtained by controlling the hydrogen pressure in the system.The actual hydrogen contents of the specimens which were determined by weighing the specimens before and after hydrogenation applying rigorous analysis scale are 0.09%,0.16%,0.26%,0.37%,and 0.48%,respectively.

    Table 1.Chemical composition of TC4 wt.%

    2.2 Cutting tools

    The uncoated cemented carbide tools are made by Kennametal Co.in American,and the type is ISO K313 SNMG 120408MS and its basal body consisted of uncoated WC/Co fine granular material.Its geometrical parameter:rake angle 5°,relief angle 8°,inclination angle 4°,major declination angle 45°,minor declination angle 45°,corner radius 0.8 mm.

    2.3 Experimental methods

    The experiments are fulfilled by dry turning on the lathe CA6140 with a maximum spindle speed 1 400 r/min which realizes stepless speed regulation by combining converter.The cutting temperature is determined by natural thermocouple method which can measure the mean temperature of contacting zone between rake face and chip,the schematic diagram of the cutting temperature test is shown in Fig.1.

    Fig.1.Schematic diagram of the cutting temperature test

    The cutting temperature measurement system includes NI USB-621X signal analyzer and temperature calibration equipment.The tool wear is measured by using three-dimensional video microscope which is made by Hirox Co.in Japan (model:KH7700),and the average flank wear width (VB) is tracking measured at regular intervals.It is very difficult to accurately measure crater wear depth (KT) owing to complexity of crater wear on the rake face in turning titanium alloys[12-14].However,the crater wear depthKTcan be accurately measured by the three-dimensional video microscope,and it can easily find the place of the maximumKTby moving section perpendicular to main cutting edge.We can measure theKTby the intersection of the section and crater.The schematic diagram of the measurement is shown in Fig.2.

    The cutting speeds are 90 m/min and 130 m/min since it has been shown that the parameter has principal effect on tool wear[16].The cutting depth and feed are kept constant,and they are 1 mm/r and 0.1 mm/r,respectively.

    Fig.2.Schematic diagram of the measurement

    3 Results and Discussion

    Fig.3 shows the change curve of average flank wearVBwith machining time.With the increase of time,theVBboth accordingly increase,and the difference ofVBis more when time is longer.Moreover,the flank wearVBincrement of unhydrogenated specimen comparison to pre-machining is more than hydrogenated specimens,theVBincrement of the specimen with 0.26% H is minimum.So theVBis minimum only for the specimen with optimum hydrogen content.

    Fig.3.Average flank wear vs.cutting time

    The average flank wearVBwith hydrogen content are presented in Fig.4.It is apparently found thatVBmonotonously decreases when w(H) is less than 0.16%,and the change ofVBis very small ranging from 0.16% to 0.26%,and then increases with the increase of w(H).In addition,theVBis minimum when hydrogen content is 0.26%,and the most decrease amplitude ofVBis more at lower speed.

    The depth of crater wear after the same machining time at different speeds versus hydrogen contents is shown in Fig.5.From the figure it can be seen thatKTare both minimum when hydrogen content is 0.26%,and the most decrease amplitude ofKTis more at lower speed.Besides,the change law ofKTwith w(H) is the same asVB,but the increase amplitude ofVBis more than that ofKTafter hydrogen content is more than 0.26%,which is attributed to reduction of elastic modulus value after hydrogenation[17].The reduction of elastic modulus after hydrogenation causes more serious rebound deformation in machining,which gives rise to increase ofVBowing to aggravation of friction between tool and machined surface,while has a slight effect onKT.

    Fig.4.Average flank wear vs.hydrogen content

    Fig.5.Crater wear vs.hydrogen content

    Fig.6 shows the change curve of crater wear widthKBwith w(H).KBof unhydrogenated specimen is more comparison to hydrogenated specimens,and then the change ofKBcan be neglected between hydrogenated specimens.So hydrogenation have nearly no effect on width of crater.

    Fig.6.Crater wear width vs.hydrogen content

    Fig.7 shows the change curve of craterKM(distance between the cutting edge and the position of maximalKT)with w(H).From the graph,theKMfirstly monotonously rises to maximum,and then monotonously reduces with the increase of hydrogen content ranging from 0% to 0.48%.KMreaches maximum when the hydrogen content is 0.26%,so the cutting edge strength is correspondingly at the most and is advantage to machining.Besides,KMof unhydrogenated specimen is least.The crater areaKAis presented in Fig.8.It is apparently found thatKAof unhydrogenated specimen is more than other hydrogenated specimens,and the change ofKAof hydrogenated specimens is very small at the speed of 90 m/min.KAwill directly influences tool nose stress,and further effects tool wear and life.

    Fig.7.Distance between the cutting edge and the position of maximal KTvs.hydrogen content

    Fig.8.Crater wear area vs.hydrogen content

    Fig.9 shows the change curve of cutting temperature (θ)with hydrogen contents whenVBis 0.1 mm.With the increase of hydrogen content ranging from 0% to 0.48%,θfirstly monotonously reduce to minimum,and then monotonously rise.θreach minimum when the hydrogen content is 0.26% (the optimum hydrogen content).It can be found from the numerical value in the Fig.9 that the correspondingly maximal reduction ofθis 80℃ and 47℃when cutting speed is 90 m/min and 130 m/min.Moreover,the reduction amplitude ofθcorresponding to the speeds are about 13.1%,6.6%,respectively.Therefore,the cutting speed has a distinct effect on decreasingθ,and the reduction amplitude ofθis more distinct at lower speed in machining Ti-6Al-4V alloy.Besides,the reduction amplitude ofθhas a close relationship with hydrogen content,the reduction amplitude is just maximum only for optimum hydrogen content.

    Fig.9.Cutting temperature vs.hydrogen content

    According to the result analyzed above,the most decrease amplitude ofKTandVBis obvious at lower speed,which is attributed to following reasons.On the one hand,the cutting zone temperature increases with the increase of cutting speed,which gives rise to aggravation of tool diffusion wear.On the other hand,the mechanical properties of Ti-6Al-4V alloy changed after the cutting temperature reaches 700 ℃-800℃,and hydyogen has no positive effect on improving tool wear when cutting temperature reaches 1 000 ℃-1 100 ℃.

    As for reasons of hydrogen effect on the wear regularity,combining with the previous studies[17-20],they are chiefly attributed to comprehensive effect of hydrogen contents on microstructure,physical properties.With the decreasing of flow stress and friction coefficient after thermohydrogen treatment,the deformation and friction in chip formation reduce.Moreover,Low cutting force and cutting temperature reduce tool wear.

    4 Conclusions

    (1) The average flank wearVBand crater wearKTfirstly decrease and then increase with the rise of hydrogen content,and hydrogenation has no effect on the width of crater wear.

    (2) The tool wear is closely related to cutting speed in machining hydrogenated Ti-6Al-4V alloy,and the reduction amplitude of crater wearKTand flank wearVBare more distinct at lower speed.

    (3) The tool wear has a close relationship with hydrogen content of the Ti-6Al-4V alloy,and the reduction amplitude of crater wearKTand flank wearVBis just maximum only for optimum hydrogen content.

    (4) The reduction of cutting temperature is an important factor for improving tool wear after the Ti-6Al-4V alloy is properly hydrogenated.

    (5) The reasons of hydrogen effect on the wear are chiefly attributed to comprehensive effect of hydrogen contents on microstructure,physical properties and dynamic mechanical properties of the Ti-6Al-4V alloy.

    [1]Jiuhua,REN Kaiqiang,GENG Guosheng.Cutting forces in high-speed milling of a close alpha titanium alloy[J].Key Engineering Materials,2004,259-260:451-455.

    [2]LI Liang,HE Ning,XU Jiuhua.Experimental study on high speed milling of Ti alloys[J].Materials Science Forum,2004,471-472:414-417.

    [3]RIBEIRO M V,FERREIRA J R.Optimization of titanium alloy(6Al-4V) machining[J].Journal of Materials Processing Technology,2003,143-144:458-463.

    [4]RAHMAN M V,WONG Y S,RAHMATH Z A.Machinability of titanium alloys[J].Machine Elements and Manufacturing,2003,46(1):107-115.

    [5]VENUGOPAL K A,PAULB S,CHATTOPADHYAY A B.Growth of tool wear in turning of Ti-6Al-4V alloy under cryogenic cooling[J].Wear,2007,262(9-10) :1 071-1 078.

    [6]KOLACHEV B A,TALALAEV V D.Effect of hydrogen on the machinability of VT5-1 alloy by cutting[J].Materials Science,1996,32(6):753.

    [7]EGOROVA Y B,KOLACHEV B A.Structure effect on cutting machinability of Ti alloys[J].Metal Science and Heat Treatment,2003(4):16-21.

    [8]EZUGWU E O,BONNEY J,YAMANE Y.An overview of the machinability of aeroengine alloys[J].Journal of Materials Processing Technology,2003,134:233-253.

    [9]SENKOV O N,FROES F H.Thermohydrogen processing of titanium alloys[J].International Journal of Hydrogen Energy,1999,24(6):565-576.

    [10]FROES F H,SENKOV O N.Hydrogen as a temporary alloying element in titanium alloys:Thermohydrogen processing[J].International Materials Reviews,2004,49(3-4):227-245.

    [11]FROES F H,ELIEZER D,SENKOV O N,et al.Beneficial effects of hydrogen as a temporary alloying element in titanium alloys:An overview[J].The Minerals Metals and Materials Society,2003:301-313.

    [12]DEVILLEZ A,LESKO S,MOZER W.Cutting tool crater wear measurement with white light interferometry[J].Wear,2004,256(1-2):56-65.

    [13]WANG W H,WONG Y S,HONG G S.3D measurement of crater wear by phase shifting method[J].Wear,2006,261(2):164-171.

    [14]DAWSON T G,KURFESS T R.Quantification of tool wear using white light interferometry and three-dimensional computational metrology[J].International Journal of Machine Tools &Manufacture,2005,45:591-596.

    [15]VENUGOPAL K A,PAUL S,CHATTOPADHYAY A B.Growth of tool wear in turning of Ti-6Al-4V alloy under cryogenic cooling[J].Wear,2007,262(9-10):1 071-1 078.

    [16]LI Hong,HOU Hongliang.Relationship between effect of hydrogen on physical and mechanical properties and Its machinability for TC4 titanium alloy[J].Aeronautical Manufacturing Technology,2008(20):80-83.(in Chinese)

    [17]HOU Hongliang,LI Zhiqiang,WANG Yaoqi.Technology of hydrogen treatment for titanium alloy and its application prospect[J].The Chinese Journal of Nonferrous Metals,2003,13(3):533-549.(in Chinese)

    [18]WEI Weihua,XU Jiuhua,FU Yucan,et al.Machinability of hydrogenating titanium alloy[J].Journal of Nanjing University of Aeronatics &Astronautics,2009,41(5):633-638.(in Chinese)

    [19]WEI Weihua,XU Jiuhua,FU Yucan,et al.Optimization of hydrogenation process and hydrogenation concentration in improving titanium alloy machinability[J].China Mechanical Engineering,2010,21(2):196-201.(in Chinese)

    [20]WEI Weihua,XU Jiuhua,FU Yucan,et al.Influence of hydrogen contents of Ti-6Al-4V alloy on cutting force and temperature[J].Key Engineering Materials,2010,419-420:789-792.

    Biographical notes

    WEI Weihua,born in 1977,is currently a PhD candidate atCollege of Mechanical and Electrical Engineering,Nanjing University of Aeronautics and Astronautics,China.His research interests include high performance cutting technology.

    E-mail:weiweihua2005@163.com

    XU Jiuhua,born in 1964,is currently a professor atNanjing University of Aeronautics &Astronautics,China.He received his PhD degree fromNanjing University of Aeronautics and Astronautics,China,in 1992.His research interests include high performance cutting/grinding technology,high efficiency combined machining technology,super-hard abrasive tool technology.

    Tel:+86-25-84 896511;E-mail:jhxu@nuaa.edu.cn

    FU Yucan,born in 1972,is currently a professor atNanjing University of Aeronautics and Astronautics,China.He received his PhD degree fromNanjing University of Aeronautics and Astronautics,China,in 1999.His research interests include high performance combined machining technology,modeling and simulation of machining process.

    Tel:+86-25-84 895857;E-mail:yucanfu@nuaa.edu.cn

    YANG Shubao,born in 1978,is currently a PhD candidate atCollege of Mechanical and Electrical Engineering,Nanjing University of Aeronautics and Astronautics,China.His research interests include high performance cutting technology.

    E-mail:sbyang2007@nuaa.edu.cn

    国产成年人精品一区二区| 精品无人区乱码1区二区| 成人亚洲精品av一区二区| 赤兔流量卡办理| 亚洲第一区二区三区不卡| 看非洲黑人一级黄片| 国产成人福利小说| 国产淫片久久久久久久久| 免费黄网站久久成人精品| 精品久久久久久久人妻蜜臀av| 夜夜看夜夜爽夜夜摸| 一a级毛片在线观看| 欧美性猛交╳xxx乱大交人| 日韩亚洲欧美综合| 国产在线精品亚洲第一网站| 亚洲一区二区三区色噜噜| 久久亚洲精品不卡| 男女之事视频高清在线观看| 国产亚洲欧美98| 亚洲丝袜综合中文字幕| 国内精品美女久久久久久| 男女下面进入的视频免费午夜| 国产一区二区三区在线臀色熟女| 少妇人妻精品综合一区二区 | 国产一区亚洲一区在线观看| 免费黄网站久久成人精品| 人妻丰满熟妇av一区二区三区| 亚洲人成网站高清观看| 欧美日本视频| 国产精品国产高清国产av| 成年女人看的毛片在线观看| 亚洲中文字幕日韩| 日本与韩国留学比较| 亚洲精品在线观看二区| 国产成人91sexporn| a级毛片免费高清观看在线播放| 亚洲婷婷狠狠爱综合网| 免费在线观看成人毛片| 日本一本二区三区精品| 日日摸夜夜添夜夜添av毛片| 欧美三级亚洲精品| 免费看a级黄色片| 国内揄拍国产精品人妻在线| 黑人高潮一二区| 国产高清视频在线观看网站| 欧美一区二区亚洲| 午夜福利视频1000在线观看| 成人性生交大片免费视频hd| 51国产日韩欧美| 99热这里只有是精品在线观看| 夜夜夜夜夜久久久久| 男插女下体视频免费在线播放| 亚洲国产色片| 欧美色欧美亚洲另类二区| 天堂影院成人在线观看| 亚洲最大成人中文| 欧美绝顶高潮抽搐喷水| 少妇的逼水好多| 少妇的逼水好多| 国产伦精品一区二区三区四那| 亚洲欧美日韩高清在线视频| 真实男女啪啪啪动态图| 国产高清三级在线| 免费人成在线观看视频色| 久久久久国产网址| 蜜臀久久99精品久久宅男| 国产亚洲91精品色在线| 亚洲av第一区精品v没综合| 欧美成人a在线观看| 亚洲成a人片在线一区二区| 欧洲精品卡2卡3卡4卡5卡区| 日日摸夜夜添夜夜添小说| 又黄又爽又免费观看的视频| 亚洲一区二区三区色噜噜| 久久久午夜欧美精品| 男人舔女人下体高潮全视频| 久久精品国产清高在天天线| 99久久中文字幕三级久久日本| a级毛片免费高清观看在线播放| 国产亚洲精品久久久com| 久久久久性生活片| 九九爱精品视频在线观看| 在线播放国产精品三级| 国产激情偷乱视频一区二区| 大香蕉久久网| 97碰自拍视频| 日韩制服骚丝袜av| 国产一区二区三区在线臀色熟女| 99riav亚洲国产免费| 最近的中文字幕免费完整| 亚洲国产精品久久男人天堂| 日韩一区二区视频免费看| 99久久九九国产精品国产免费| 国产白丝娇喘喷水9色精品| 人妻夜夜爽99麻豆av| 亚洲欧美日韩无卡精品| av免费在线看不卡| 精品久久国产蜜桃| 中文字幕熟女人妻在线| 男女之事视频高清在线观看| 高清毛片免费观看视频网站| 99久国产av精品国产电影| 久久久国产成人精品二区| 久久久a久久爽久久v久久| 久久人妻av系列| 国产高清三级在线| 亚洲在线自拍视频| 久久精品91蜜桃| 午夜久久久久精精品| 99热这里只有精品一区| 老司机午夜福利在线观看视频| 又爽又黄无遮挡网站| 中文在线观看免费www的网站| 国产精品久久电影中文字幕| av黄色大香蕉| 免费黄网站久久成人精品| 国产探花在线观看一区二区| 日韩欧美国产在线观看| 内地一区二区视频在线| 免费看av在线观看网站| 久久人人爽人人片av| 91狼人影院| 免费搜索国产男女视频| 欧美激情在线99| 亚洲内射少妇av| 观看美女的网站| 精品久久久久久久久av| 91久久精品国产一区二区三区| 日本与韩国留学比较| 久久亚洲精品不卡| 欧美日韩精品成人综合77777| 亚洲欧美日韩无卡精品| 亚州av有码| 99国产极品粉嫩在线观看| 亚洲成人久久性| 99视频精品全部免费 在线| 国产三级中文精品| 亚洲欧美日韩无卡精品| 欧美日本亚洲视频在线播放| 色综合亚洲欧美另类图片| 91麻豆精品激情在线观看国产| 我要看日韩黄色一级片| 国产精品精品国产色婷婷| 俺也久久电影网| 99久久成人亚洲精品观看| 国产在线男女| 国产成人a区在线观看| 又黄又爽又免费观看的视频| 欧美不卡视频在线免费观看| 99久久久亚洲精品蜜臀av| 热99在线观看视频| 精品一区二区免费观看| 亚洲18禁久久av| 99在线人妻在线中文字幕| 69人妻影院| 插阴视频在线观看视频| 一级黄片播放器| 国产欧美日韩精品一区二区| 伦理电影大哥的女人| 全区人妻精品视频| 久久精品夜夜夜夜夜久久蜜豆| 国产高清视频在线观看网站| 亚洲18禁久久av| 69人妻影院| 久久午夜福利片| 欧美xxxx性猛交bbbb| 国产综合懂色| 大又大粗又爽又黄少妇毛片口| 天堂影院成人在线观看| 国产探花在线观看一区二区| 插逼视频在线观看| 永久网站在线| 变态另类成人亚洲欧美熟女| 亚洲av中文av极速乱| 国产一区二区在线观看日韩| 免费电影在线观看免费观看| 两个人视频免费观看高清| 欧美zozozo另类| 最近在线观看免费完整版| 欧美成人精品欧美一级黄| 午夜日韩欧美国产| 国产毛片a区久久久久| 夜夜看夜夜爽夜夜摸| 国产午夜福利久久久久久| 日韩成人伦理影院| 午夜日韩欧美国产| 一个人看的www免费观看视频| 欧美一区二区精品小视频在线| 国产精品,欧美在线| 黄色视频,在线免费观看| 午夜老司机福利剧场| 极品教师在线视频| 国产高清三级在线| 大香蕉久久网| 国产伦一二天堂av在线观看| 久久久久久九九精品二区国产| 国产爱豆传媒在线观看| 蜜臀久久99精品久久宅男| 精品人妻视频免费看| 亚洲美女视频黄频| 99久久无色码亚洲精品果冻| 三级毛片av免费| 晚上一个人看的免费电影| 可以在线观看毛片的网站| 国产探花极品一区二区| 九九在线视频观看精品| 在线观看av片永久免费下载| 五月玫瑰六月丁香| 天堂网av新在线| 尾随美女入室| 欧美又色又爽又黄视频| 最新中文字幕久久久久| 国产国拍精品亚洲av在线观看| 俺也久久电影网| 国产淫片久久久久久久久| 成人鲁丝片一二三区免费| 深爱激情五月婷婷| 亚洲婷婷狠狠爱综合网| 精品人妻一区二区三区麻豆 | 少妇的逼水好多| 熟妇人妻久久中文字幕3abv| 久久欧美精品欧美久久欧美| 日韩欧美三级三区| 床上黄色一级片| 18禁裸乳无遮挡免费网站照片| 精品人妻熟女av久视频| 国产乱人偷精品视频| 精品不卡国产一区二区三区| av在线观看视频网站免费| 国产精品国产三级国产av玫瑰| 夜夜爽天天搞| 好男人在线观看高清免费视频| 国产单亲对白刺激| 又黄又爽又免费观看的视频| 又粗又爽又猛毛片免费看| 99久久精品热视频| 欧美成人a在线观看| 麻豆乱淫一区二区| 精品国内亚洲2022精品成人| 人妻夜夜爽99麻豆av| 热99在线观看视频| 综合色av麻豆| 成年免费大片在线观看| 乱码一卡2卡4卡精品| 伦理电影大哥的女人| 欧美一区二区精品小视频在线| 免费av毛片视频| 午夜免费激情av| 精品午夜福利视频在线观看一区| 亚洲av成人精品一区久久| 日本黄大片高清| 国产不卡一卡二| 嫩草影院新地址| 麻豆国产av国片精品| 蜜桃久久精品国产亚洲av| 亚洲av二区三区四区| av在线观看视频网站免费| 国国产精品蜜臀av免费| 三级毛片av免费| 国产色爽女视频免费观看| 91狼人影院| 午夜福利在线观看免费完整高清在 | 国产亚洲欧美98| 亚洲在线观看片| 国产免费男女视频| 日本色播在线视频| 变态另类丝袜制服| 日韩av在线大香蕉| 精品日产1卡2卡| 美女高潮的动态| 国产成人福利小说| 国产精华一区二区三区| 内地一区二区视频在线| 又黄又爽又免费观看的视频| 神马国产精品三级电影在线观看| 亚洲一级一片aⅴ在线观看| 超碰av人人做人人爽久久| 亚洲精品456在线播放app| 国内精品久久久久精免费| 熟妇人妻久久中文字幕3abv| 少妇被粗大猛烈的视频| 激情 狠狠 欧美| 国产精品久久久久久av不卡| 老师上课跳d突然被开到最大视频| 国产精品乱码一区二三区的特点| 18禁黄网站禁片免费观看直播| 男女下面进入的视频免费午夜| 日本免费a在线| 嫩草影院入口| 中文字幕人妻熟人妻熟丝袜美| 亚洲最大成人中文| 日产精品乱码卡一卡2卡三| 亚洲aⅴ乱码一区二区在线播放| 亚洲av免费高清在线观看| 精品午夜福利视频在线观看一区| 变态另类成人亚洲欧美熟女| 3wmmmm亚洲av在线观看| 精品午夜福利在线看| 麻豆成人午夜福利视频| 亚洲av电影不卡..在线观看| 国产在线男女| 国产精品无大码| 国产黄a三级三级三级人| 日本免费a在线| 人妻久久中文字幕网| 搞女人的毛片| 国产一级毛片七仙女欲春2| 长腿黑丝高跟| 1024手机看黄色片| 尤物成人国产欧美一区二区三区| 寂寞人妻少妇视频99o| 国产男人的电影天堂91| 亚洲四区av| 精品人妻一区二区三区麻豆 | 男人和女人高潮做爰伦理| 又黄又爽又刺激的免费视频.| 亚洲经典国产精华液单| 九九久久精品国产亚洲av麻豆| 久99久视频精品免费| 夜夜夜夜夜久久久久| 老师上课跳d突然被开到最大视频| 国产又黄又爽又无遮挡在线| 国产精品亚洲一级av第二区| 日本五十路高清| 国国产精品蜜臀av免费| 色播亚洲综合网| 国产aⅴ精品一区二区三区波| 亚洲性久久影院| 22中文网久久字幕| 久久久精品94久久精品| 麻豆精品久久久久久蜜桃| 中文字幕av在线有码专区| 亚洲成人av在线免费| 亚洲av美国av| 天天躁日日操中文字幕| 女人被狂操c到高潮| 三级经典国产精品| 99国产极品粉嫩在线观看| 在线观看一区二区三区| 日韩欧美一区二区三区在线观看| 日日干狠狠操夜夜爽| 中文字幕精品亚洲无线码一区| 高清毛片免费看| 亚洲图色成人| 亚洲精华国产精华液的使用体验 | 男女之事视频高清在线观看| 人妻少妇偷人精品九色| 日韩大尺度精品在线看网址| 色综合色国产| 色综合亚洲欧美另类图片| а√天堂www在线а√下载| 毛片一级片免费看久久久久| 精品人妻熟女av久视频| 伦精品一区二区三区| 国产精品一及| 欧美一区二区国产精品久久精品| 国产美女午夜福利| 国产亚洲精品av在线| 3wmmmm亚洲av在线观看| 久久精品国产清高在天天线| 最后的刺客免费高清国语| 中文字幕人妻熟人妻熟丝袜美| 麻豆一二三区av精品| 欧美三级亚洲精品| 五月玫瑰六月丁香| 六月丁香七月| 国产乱人偷精品视频| 亚洲性久久影院| 精品一区二区免费观看| 国产成人a∨麻豆精品| 久久草成人影院| 伦精品一区二区三区| 欧美+亚洲+日韩+国产| 亚洲精品粉嫩美女一区| 国产人妻一区二区三区在| 国产av一区在线观看免费| 国产成人一区二区在线| 午夜福利高清视频| 亚洲精品国产成人久久av| 麻豆成人午夜福利视频| 久久精品国产亚洲av天美| 国产成人一区二区在线| 深夜a级毛片| 久久久精品94久久精品| 成人无遮挡网站| 国产亚洲欧美98| 免费看光身美女| 嫩草影视91久久| 高清日韩中文字幕在线| 久久久久九九精品影院| 99热这里只有是精品50| 女同久久另类99精品国产91| 在线免费观看的www视频| 午夜亚洲福利在线播放| av黄色大香蕉| 日本-黄色视频高清免费观看| 日本与韩国留学比较| 男女做爰动态图高潮gif福利片| 国产一区二区在线av高清观看| 国产成人a∨麻豆精品| aaaaa片日本免费| 精品99又大又爽又粗少妇毛片| 三级经典国产精品| 亚洲美女黄片视频| 男女边吃奶边做爰视频| 国产中年淑女户外野战色| 波野结衣二区三区在线| 五月伊人婷婷丁香| 色综合站精品国产| 国产v大片淫在线免费观看| 欧美最新免费一区二区三区| 我要看日韩黄色一级片| 日本在线视频免费播放| 在线观看66精品国产| 九九热线精品视视频播放| 亚洲精品456在线播放app| 成人特级黄色片久久久久久久| 色吧在线观看| 欧美在线一区亚洲| 最近最新中文字幕大全电影3| 国产白丝娇喘喷水9色精品| 一区二区三区高清视频在线| 国产黄a三级三级三级人| 久久人人爽人人片av| 国产色婷婷99| 黄色配什么色好看| 亚洲专区国产一区二区| 3wmmmm亚洲av在线观看| 亚洲高清免费不卡视频| 国产欧美日韩精品一区二区| 黄色配什么色好看| 搡老岳熟女国产| 男人的好看免费观看在线视频| 热99re8久久精品国产| 99久久精品一区二区三区| 最好的美女福利视频网| 亚洲无线在线观看| 精品无人区乱码1区二区| 国产精品一区二区三区四区免费观看 | 在线播放无遮挡| 麻豆久久精品国产亚洲av| 亚洲av成人av| 一本一本综合久久| 亚洲在线自拍视频| 不卡一级毛片| 精品久久国产蜜桃| 精品日产1卡2卡| 欧美日本视频| 欧美丝袜亚洲另类| 日韩在线高清观看一区二区三区| 91午夜精品亚洲一区二区三区| 综合色丁香网| 小蜜桃在线观看免费完整版高清| 黄片wwwwww| 欧美激情在线99| 午夜久久久久精精品| 亚洲一区二区三区色噜噜| 国产成人福利小说| aaaaa片日本免费| 国产午夜精品论理片| 欧美一区二区精品小视频在线| 舔av片在线| 精品无人区乱码1区二区| 午夜日韩欧美国产| 天堂动漫精品| 综合色丁香网| 最近2019中文字幕mv第一页| 精品久久久久久久久久久久久| 成人综合一区亚洲| 长腿黑丝高跟| 男女之事视频高清在线观看| 日本在线视频免费播放| 国产精品亚洲一级av第二区| 久久久久久久久大av| 一本一本综合久久| 波多野结衣巨乳人妻| av中文乱码字幕在线| 久久天躁狠狠躁夜夜2o2o| 99热这里只有精品一区| .国产精品久久| 女人十人毛片免费观看3o分钟| 国产高清三级在线| 国产三级在线视频| 久久午夜福利片| 在线播放国产精品三级| 日本黄色视频三级网站网址| 亚洲一级一片aⅴ在线观看| 午夜激情欧美在线| 1000部很黄的大片| 国产欧美日韩精品亚洲av| 亚洲人与动物交配视频| 色5月婷婷丁香| 亚洲美女黄片视频| 嫩草影院精品99| 十八禁国产超污无遮挡网站| 日本-黄色视频高清免费观看| 舔av片在线| 女人被狂操c到高潮| 婷婷精品国产亚洲av| 校园人妻丝袜中文字幕| 免费看av在线观看网站| 三级男女做爰猛烈吃奶摸视频| 91久久精品国产一区二区三区| 99热6这里只有精品| 国产亚洲精品av在线| 色吧在线观看| 国产黄色视频一区二区在线观看 | 人妻少妇偷人精品九色| 色综合色国产| 久久久成人免费电影| 18禁裸乳无遮挡免费网站照片| 91狼人影院| 久久久久久久久久黄片| 亚洲成a人片在线一区二区| 免费观看在线日韩| 十八禁网站免费在线| 国产美女午夜福利| 国产精品国产高清国产av| 国产精品国产三级国产av玫瑰| 97超级碰碰碰精品色视频在线观看| 亚洲中文字幕一区二区三区有码在线看| 淫秽高清视频在线观看| 国产91av在线免费观看| 老熟妇仑乱视频hdxx| 亚洲精品国产成人久久av| 中出人妻视频一区二区| 1000部很黄的大片| 偷拍熟女少妇极品色| 免费看av在线观看网站| 久久人人精品亚洲av| 日韩欧美精品免费久久| 亚洲无线观看免费| 久久精品夜夜夜夜夜久久蜜豆| 最近手机中文字幕大全| 99热精品在线国产| 久久中文看片网| 久久人人爽人人片av| 国产男靠女视频免费网站| 国产成人影院久久av| av专区在线播放| 丰满人妻一区二区三区视频av| 久99久视频精品免费| 一个人看视频在线观看www免费| 床上黄色一级片| 亚洲欧美精品综合久久99| 悠悠久久av| 一区二区三区免费毛片| 国产激情偷乱视频一区二区| 久久婷婷人人爽人人干人人爱| 国产精品一区www在线观看| 成年版毛片免费区| 精品久久久久久久末码| 国产激情偷乱视频一区二区| 男人舔女人下体高潮全视频| 欧洲精品卡2卡3卡4卡5卡区| 我的老师免费观看完整版| 18禁在线无遮挡免费观看视频 | 久久久久国产精品人妻aⅴ院| 18禁黄网站禁片免费观看直播| 一卡2卡三卡四卡精品乱码亚洲| 色哟哟哟哟哟哟| 插阴视频在线观看视频| 日韩在线高清观看一区二区三区| 男女下面进入的视频免费午夜| 亚洲不卡免费看| 2021天堂中文幕一二区在线观| 欧美3d第一页| 一区二区三区高清视频在线| av在线天堂中文字幕| 乱码一卡2卡4卡精品| 2021天堂中文幕一二区在线观| 欧美色欧美亚洲另类二区| 在线观看66精品国产| 成人无遮挡网站| 国产精品亚洲美女久久久| 在线观看美女被高潮喷水网站| 丝袜喷水一区| 亚洲精品成人久久久久久| 国产亚洲欧美98| 久久热精品热| 热99re8久久精品国产| 中文亚洲av片在线观看爽| 久久久久国内视频| 伦精品一区二区三区| 亚洲熟妇熟女久久| 久久久精品94久久精品| 桃色一区二区三区在线观看| 永久网站在线| 亚洲成人精品中文字幕电影| 成年免费大片在线观看| 精品一区二区三区视频在线观看免费| 亚洲国产精品成人综合色| a级一级毛片免费在线观看| 欧美bdsm另类| 亚洲不卡免费看| 91av网一区二区| 国产精品伦人一区二区| 国产乱人视频| 日韩欧美免费精品| 亚洲欧美日韩高清在线视频| 少妇人妻一区二区三区视频| 桃色一区二区三区在线观看| 三级国产精品欧美在线观看| 亚洲欧美日韩高清专用| 国产精品一区二区三区四区免费观看 | 最好的美女福利视频网| 成人鲁丝片一二三区免费| 欧美一区二区精品小视频在线| 非洲黑人性xxxx精品又粗又长| 色哟哟哟哟哟哟| 亚洲av熟女| 国产白丝娇喘喷水9色精品| 国产黄a三级三级三级人| 99久久精品一区二区三区| 国产精品一及|