    Tribological behaviour of AZ31 magnesium alloy reinforced by bimodal size B4C after precipitation hardening

    2022-12-30 03:41:22SeyeKiomarsMoheimaniAzaehKeshtarSaeeKhaemzaehMortezaTayebiAliRajaeeAbollahSaboori
    Journal of Magnesium and Alloys 2022年11期

    Seye Kiomars Moheimani,Azaeh Keshtar,Saee Khaemzaeh,Morteza Tayebi,Ali Rajaee,Abollah Saboori

    a Advanced Materials Research Center,Department of Materials Engineering,Najafabad Branch,Islamic Azad University,Najafabad,Iran

    b Department of Research and Development,Nejat Darya Company,Boushehr,Iran

    cCenter for Risk and Reliability,University of Maryland,College Park,MD 20742,United States

    dDepartment of Industrial Engineering,University of Padova,35131 Padova,Italy

    e Young Researchers and Elites Club,Science and Research Branch,Islamic Azad University,Tehran,Iran

    fDepartment of Materials and Polymer Engineering,Hakim Sabzevari University,Sabzevar,Iran

    g Integrated Additive Manufacturing Center (IAM),Department of Management and Production Engineering (DIGEP),Politecnico di Torino,Corso Duca Degli Abruzzi,24,10129,Torino,Italy

    Abstract This study investigated dry sliding wear properties of AZ31 magnesium alloy and B4C-reinforced AZ31 composites containing 5,10,and 20 wt.% B4C with bimodal sizes under different loadings (10–80 N) at various sliding speeds (0.1–1 m/s) via the pin-on-disc configuration Microhardness evaluations showed that when the distribution of B4C particles was uniform the hardness of the composites increased by enhancing the reinforcement content.The unreinforced alloy and the composite samples were examined to determine the wear mechanism maps and identify the dominant wear mechanisms in each wear condition and reinforcement content.For this purpose,wear rates and friction coefficient were recorded during the wear tests and worn surfaces were characterized by scanning electron microscopy and energy dispersive X-ray spectrometry analyses.The determined wear mechanisms were abrasion,oxidation,delamination,adhesion,and plastic deformation as a result of thermal softening and melting.The wear evaluations revealed that the composites containing 5 and 10 wt.% B4C had a significantl higher wear resistance in all the conditions.However,20 wt.% B4C/AZ31 composite had a lower resistance at high sliding speeds (0.5–1 m/s) and high loadings (40–80 N) in comparison with the unreinforced alloy.The highest wear resistance was obtained at high sliding speeds and low loadings with the domination of oxidative wear.

    Keywords: B4C;AZ31 alloy;Metal matrix composite;Wear mechanism;Bimodal.

    1.Introduction

    Currently,to meet lightweight standards,the development of high strength-to-weight ratio materials is inevitable,which plays a significan role in energy saving for structural applications.Mg alloys can be an alternative to the conventional alloys used for gears,bearings,cylinder bores,and pistons due to their unique properties,namely high specifi ductility,low density,and great shock absorption [1–3].Nevertheless,low mechanical properties of Mg alloys,especially low wear resistance,can be a restriction for being used in industrial applications [4],which is critical in automotive and aircraft engine components [5,6].Compositing is an efficien method to develop the mechanical and wear properties of Mg alloys.In the meantime,their reinforcement selection is the most important factor in the composite preparation process along with the evolution of the microstructure and reinforcement distribution in the matrix[7,8].However,tribological properties of the composites are also highly dependant on the matrix and reinforcement materials (size,shape,content,and distributions),experimental conditions (loading,environment,sliding speed,and sliding distance) and surficia conditions (e.g.roughness and hardness) [5,9].The description of the aforementioned parameters is brought in details in a previous study [5].

    Particle-reinforced metal-matrix composites (MMCs) display great mechanical and wear properties compared to unreinforced metals due to the existence of hard reinforcement particles in them,protecting the material from continuous abrasion during tribo-contacts [9–11].Results of an earlier investigation have shown that although the addition of the SiC microparticles to Mg matrixes leads to improved mechanical properties,homogenous distribution is not attained in the matrix.Different factors affect the wear resistance of MMCs,amongst which some are well-known.For instance,particle size has been stated to have conflictin results.A few studies have claimed that fine-size particles enhance wear resistance by increasing the composite strength.Such reports concern mechanisms such as dislocation strengthening,Orowan strengthening,and grain refinemen strengthening.An improvement in the friction can also be seen as a result of more particle/counterface contacts.Other studies have proposed that large reinforcement sizes can increase the wear resistance through deep embedment in the matrix and improve load-bearing capacity [12].Based on the mentioned findings it can be concluded that both fin and coarse particles can have positive effects on the improvement of the friction and wear resistance of MMCs.Thus,composites reinforced by bimodal size particles are expected to have a combination of both particle types.Fine (submicron-scale) and coarse particles (micron-scale) in the matrixes assist grain refinemen by stimulating dynamic recrystallization and nucleation,and grain boundary pinning during the mechanical processes,respectively.Thus significan strengthening has been achieved[13].

    An increase in the particle content results in the development of the wear resistance of MMCs by inter-particle spacing on the tribological properties of the composites [1].Micro/nano-scaled particles of SiC [7,8,14,15],B4C [16–18],Al2O3[5,10],and CNT [19] are typically employed as the reinforcement particles which improve the hardness,strength and elastic modulus of the composites [1,2].Amongst them,B4C is a more suitable alternative for the improvement of MMCs properties such as high melting point,high thermal stability,excellent abrasion resistance,high hardness,great neutron absorption,and low density [16,17].

    In addition,B4C density is 2.52 g/cm3,whereas Mg density is 1.74 g/cm3.Hence,B4C/Mg composites are considered as lightweight materials with density values of around 2 g/cm3even if 50 vol.% B4C particles are introduced [20].It is worth noting that B4C/Mg composites containing a high volume fraction of ceramic particles show excellent wear resistance that can have a great potential for aerospace applications.

    Several methods have been employed for the preparation of Mg-matrix composites,including powder metallurgy [21,22],pressureless infiltratio [23],stir casting,and squeeze casting [1,2].Powder metallurgy can offer homogeneous distribution of particles in the matrix,resulting in a low reaction of the matrix and reinforcement [16].Recently,researchers have tried many other techniques for uniform distribution of particles,including high energy ball milling,friction stir processing,squeeze casting,spread dispersion method,and spray deposition.Amongst these techniques,stir casting has attracted great attention due to its simplicity,uniform distribution of reinforcement,and ability to prepare complex-shaped products.Only few investigations were carried out on the preparation of B4C/Mg composites using stir casting [24,25].But,several studies have been carried out on the preparation of B4C/Mg composites via other techniques [20,26–29].For instance,Ghasali et al.[30] fabricated 5 wt.% B4C/Mg composites by spark plasma sintering process and investigated the hardness and bending strength of the composites.They stated that although the strength and hardness of the prepared composites were improved compared with those fabricated via conventional methods,brittle phases of MgB2and Mg2C3were formed in the microstructure.Additionally,Jiang et al.[28] prepared B4C/Mg composites by powder metallurgy and evaluated their wear behaviour.They reported that the wear properties of the reinforced samples were improved,respecting the unreinforced samples.However,they did not examine extensive conditions to obtain detailed information on the wear mechanisms.

    There are numerous investigations in the literature on the sliding wear behaviour of the dendritic Mg alloys and their composites.For instance,Somekawa et al.[31] evaluated the wear behaviour and the microstructural evolution of commercially pure Mg and Mg–Y alloys during the wear tests.Their finding revealed that the wear rate of Mg alloys was superior to that of pure one,which was related to the formation of {102} twinning.

    Surface treatment techniques such as physical vapour deposition and plasma electrolytic oxidation have been frequently used to enhance the wear properties of Mg alloys and composites [32].The effect of the addition of oxide and carbidebased reinforcements on the wear behaviour of Mg materials was also investigated [33].Chen et al.[34] reported two wear regimes for the as-cast AZ91 Mg alloy;the severe wear,in which severe plastic deformation and melt wear were the dominant mechanisms,and the mild wear regime,which was dominated by oxidation and delamination wear mechanisms.By studying the temperature of the contact surface of each material,they found that the equilibrium temperature could determine the transition between the regimes.On the contrary,Wang et al.[35]demonstrated that the mild wear regime occurred during low loadings,irrespective of the test temperature.This can be attributed to the formation of a thick layer consisting of Mg and MgAl2O4,known as the mechanical mixing layer (MML).Taltavull et al.[36] constructed a wear map for AM60B Mg alloy at different loads (10–250 N)and various sliding speeds of 0–1 m/s.Results showed that at lower loadings,the dominant wear mechanisms were oxidation,delamination,and adhesion,whereas,at higher loadings,the dominant wear mechanism was altered by severe plastic deformation.Moreover,the wear properties of AZ91 alloy were evaluated by Zafari et al.[37].They determined the severe plastic deformation wear regimes for AZ91 alloy at different loadings.Furthermore,their study demonstrated that the sample temperature was effective in the determination of the wear mechanism.In a similar vein,Lim et al.[33] investigated the wear behaviour of SiC-reinforced AZ91 alloy during the dry sliding wear test.It was reported that the addition of the reinforcement particles was only effective at low loadings.Habibnejad et al.[38] also compared the tribological behaviours of commercially pure Mg and AZ31 composites reinforced by Al2O3nanoparticles.It was shown that the wear rate declined with increasing the reinforcement content.The improved wear behaviour was related to the composite strengthening mechanisms such as mismatch hardening mechanism and the load-bearing ability of the hard ceramic particles.

    To the best of the authors’ knowledge,before the publication date of the present paper,no comprehensive study in the literature has been conducted concerning the effect of microstructure on the wear properties of B4C/Mg composites prepared by stir casting in details.However,the fiel of wear behaviour of B4C/Mg composites still requires detailed investigation.For this reason,the current study focused on the wear properties of B4C/Mg composite samples prepared by stir casting.In addition,the dominant wear mechanisms were also comparatively evaluated for both the unreinforced Mg and B4C-reinforced Mg composites.

    2.Materials and method

    2.1.Materials

    AZ31 magnesium alloy (Shandong Hongtai Science and Technology Co.,Ltd.,China) was selected as the B4C/AZ31 composites matrix,and its chemical composition is shown in Table 1.A mixture of bimodal B4C particles (Merck Co.,Germany) with average diameters of 1 and 50 μm and the ratio of 1:5 was added as the reinforcement.

    Table 1 Chemical composition of the AZ31 Mg alloy.

    2.2.Sample preparation

    Fig.1.Schematic of the stir casting method employed for preparation of B4C/AZ31 composite samples.

    The stir casting method was employed for the B4C/AZ31 composites preparation,as demonstrated in Fig.1.To obtain a uniform heat distribution,the furnace temperature was increased gradually from 100 to 780 °C.A gaseous mixture of carbon dioxide (CO2) and sulfur fluorid (SF6) was inserted into the furnace at 300 °C to avoid burning,while argon gas was injected at 600 °C to prevent oxidation.After stabilization at 780 °C for 20 min,the B4C particles were preheated at 200 °C and added to the melt via vortex method.For gaining a uniform distribution of B4C particles in the matrix,the melt was stirred at 350 rpm for 8 min.Finally,the melt was poured into a steel mould.Four types of composites with 0,5,10,and 20 wt.% B4C contents were prepared.The samples were heated at 400 °C in an atmosphere-controlled furnace for 10 h to homogenize the chemical composition;then,they were quenched in water and aged artificiall at 175 °C for 10 h.

    2.3.Density

    The practical density was measured via the Archimedes principle.The theoretical density of the composite samples was determined by dividing the sample mass by its volume.The average theoretical density of each sample was calculated as a result.The porosity of the samples was measured using Eq.(1) [8].

    whereρa(bǔ)andρtare the skeletal and apparent density values of the samples,respectively.Four samples of each composite were tested,and the average value was reported as the fina result.

    2.4.Hardness

    The microhardness of the samples was measured using a Vickers microhardness testing machine (Leitz,England)equipped with a diamond indenter.A 300-N load was applied with a dwell time of 20 s.Five replicate measurements were carried out,and the average value was reported as the microhardness.

    2.5.Wear test

    Fig.2.Schematic of pin-on-disk configuratio used for the sliding wear tests.

    Dry sliding wear tests were carried out using an AISI 52,100 steel pin with a hardness of 45 HRC and pinon-disk configuratio at ambient temperature,as shown in Fig.2.Samples with dimensions of 35 mm?× 5 mm were utilized for the tests,and the steel pin had a 5 mm effective diameter.All tests were performed at the loadings of 10,20,40,and 80 N,the sliding speeds of 0.1,0.3,0.7,and 1 m/s,and the sliding distance of 1000 m.This sliding distance was prolonged to 1000 m to ensure that the steady-state regime was reached.The surface of the samples was cleaned and degreased by acetone in an ultrasonic bath for 5 min.The weight loss was determined by measuring the sample weight before and after each test using a photoelectric weight balance.The volume loss was also calculated by dividing the weight loss by the density of each sample.The wear rates of the samples were assessed by Archard’s law which can be expressed as Eq.(2) [39].

    whereLis the sliding distance,Vis the wear volume loss,Fis the applied load,kis the specifi wear rate,His the hardness,andKis the Archard’s constant.The average friction coefficien was also calculated for the wear distance.The applied tangential force on the holder was determined,and the coefficien of friction (COF) was calculated based on a function of the applied load.The perpendicular position of the holder was monitored to observe the displacement caused by the material removal during the wear test.Three replicates of each sample were tested,and the average COF value was reported as the fina result.

    2.6.Characterizations

    Samples were grounded using 200,400,800,1000,and 2500-grit sandpapers,and then they were polished by alumina suspension to obtain a mirror-like surface.The samples were etched by a solution of 10 mL nitric acid,10 mL deionized water,and 75 mL ethanol for 20 s.The microstructure of the samples was studied using scanning electron microscopy(SEM) Philips (model PW1800,Netherlands) equipped with energy-dispersive X-ray spectroscopy (EDS).The grain size was calculated by the linear intercept method based on three metallography images with different magnification to improve the precision of the data.

    Fig.3.Density and porosity of the samples containing different B4C contents.

    3.Results and discussion

    3.1.Density

    Fig.3 demonstrates variations of density and porosity for the samples.An increase was evident in the bulk density by increasing B4C content,which implied the strong bonding between ceramic particles and the alloy matrix.This increase was also attributed to the higher density of B4C compared to that of the matrix.The porosity of composite samples remained almost constant by increasing B4C content up to 10 wt.%.This trend could be related to the uniform distribution of the B4C particles in the matrix caused by the shearing of the melt during the stirring process [40].It can be concluded that the formation of an efficien bonding between the particles and the matrix,proper wettability of the particles by the melt,and suitable reinforcement distribution led to a reduction in the porosity.According to Fig.4,the microstructural characterizations confirme that a proper adhesion between the ceramic particles and the matrix was achieved due to the good wettability between them.It was also observed that sample 20 wt.% B4C/AZ31 had a higher porosity.Uniform dispersion of B4C in the matrix is a major benefi in the manufacturing of MMCs.A recent investigation in this fiel has reported that the agglomeration phenomenon can become dominant and exacerbate the porosity for composites containing ceramic particle higher than 10 wt.% [41].Although all pores cannot be eliminated,they can be efficientl controlled by adjusting the casting parameters,namely stirring conditions,pouring method,and casting atmosphere neutralization[40].

    3.2.Microhardness measurement

    Fig.4.SEM micrographs of the as-cast samples with different B4C contents: (a) unreinforced alloy,(b) 5% B4C/AZ31,(c) 10% B4C/AZ31,and (d) 20%B4C/AZ31.

    Fig.5.Microhardness variation of the samples containing different B4C concentrations before and after the ageing treatment.

    The microhardness of the samples with various weight percentages of B4C is shown in Fig.5.As can be seen,the microhardness of the samples was increased by elevating the B4C content.The increase in the hardness was attributed to the presence of B4C particles due to three possible strengthening mechanisms.First,an increase in the strength was due to the effective load transfer from the matrix to the reinforcement,in which the effect of microparticles is more noticeable to that of submicron particles.Second,an increase in the strength according to the Hall-Patch effect,which can be achieved through the grain refinement resulted from the presence of particles.Moreover,by increasing the number of particles,the inter-particle spacing is reduced.Accordingly,the elasticallydeformed regions around the ceramic particles are overlapped,providing the required activation energy for the grain refine ment.During this mechanism,the presence of submicron particles is more effective in attaining a uniform distribution and reduction of the inter-particle spacing (Fig.4).This aim can be achieved by the bimodal distribution of the B4C particles.The bimodal distribution prevents the localized deformation of the matrix surface during the test and refine matrix grain size [42].Localized deformation of composites and showed that deformation in the composites with high volume fraction of reinforcement was highly localized,which is due to clustering and agglomeration.They reported that the slip lines initiated in regions containing many clusters of SiC particles.Then,the slip lines spread from one cluster region to another,while the deformation remains almost zero in other samples.Moreover,in general,it should be said that by increasing the volume fraction of reinforcement,the strength of the material increased,and it is less prone to plastic deformation.To clarify the reason for the initiation of the plastic deformation in the clustered regions,deformation compatibility of inhomogeneous (clustering) distribution of reinforcement particles should be considered.The reason can be related to the higher stiffness of the clusters,which bear higher loading than the rest of the matrix to satisfy the deformation compatibility.On the other hand,the local volume fraction is higher in the clusters;thus for the same extent of deformation,more slip systems must be activated in the matrix.When the effective plastic strain diverges at various locations of the matrix,the total applied strain reaches zero,indicating the existence of a large gradient of plastic deformation in the matrix,which is due to primary residual thermal stresses [43].Third,an increase in the hardness can be related to the presence of hard B4C particles in the soft Mg matrix.The difference in the thermal expansion coefficient of the reinforcement particles and the matrix can lead to the formation of mismatch dislocations that improve the strength of the matrix up to the plastic level and increase the hardness [16,44].In this mechanism,the presence of both particle types can also be effective due to the increase in the dislocation density in the matrix[13].Here,the density increase contributed to the increase in the hardness.By increasing the reinforcement content up to 20 wt.%,the hardness value was increased up to 68.50 HV.Although the hardness was improved by rising the B4C content for all the samples,the increasing rate of the hardness was lowered when the reinforcement content increased from 10 to 20 wt.%.The reduction in the hardness rate was credited to the agglomeration of B4C particles,which led to a decrease in densificatio and hardness deterioration [14].In this study,the reduction in the hardness rate due to the agglomeration was low,indicating the successful compensation of the mechanisms of grain refinement mismatch dislocations,and load transfer for hardness.It was revealed that the microhardness of the aged composite samples was slightly higher than those of as-cast ones,which might be related to two factors;first activation of the Orowan mechanism due to the presence of precipitations acting as barriers to the dislocation movement,and second dynamic recrystallization and grain refinin phenomena during the ageing process [45].It has been reported that the existence of the reinforcement in the matrix assists the precipitation nucleation at the early stages of dynamic recrystallization and declines the average grain size of the matrix[46].Overall,the most common recrystallization mechanism in Mg alloys is continuous dynamic recrystallization,which declines the grain size during ageing treatment[47].This phenomenon also results in increase in the precipitation content,which are dissolved during solid solution,re-dispersed along the grain boundaries,and prevent the grain coarsening,leading to improvement of the mechanical properties via dynamic Hall-Petch effect [48].

    3.3.Microstructure evaluation

    Fig.6.SEM micrograph of aged unreinforced alloy indicating the presence of the precipitations with dendritic morphology.

    Fig.4a demonstrates the microstructure of the unreinforced AZ31 alloy.Dark and bright regions in the figur represent primaryα-phase grains andβ-phases,respectively.As described in earlier studies,theβ-phase locating at the grain boundaries consists of Mg17Al12compound [49,50].Moreover,η-phase particles with Al8Mn5composition are present in both inter-dendritic regions andα-phase grains,which is due to the presence of 0.2 wt.% Mn.Since mechanical stirring has been utilized,this phase formed a continuous network through the microstructure [49,51].As demonstrated in Fig.4b-d,a bimodal distribution of B4C particles is evident in the samples,which are mostly distributed in theα-phase.Figs 4c and d display the effect of B4C content on the average grain size of the B4C/AZ31 composites.It is noticeable that the addition of B4C causes a decline in the grain size to 5 μm.In fact,the grain size was reduced by enhancing the B4C content.The grain refinemen is ascribed to the distribution of B4C particles in the microstructure,pinning the grain boundaries and resulting in heterogeneous nucleation of precipitations.Moreover,it is evident that the grains around the B4C microparticles are fine than those around the submicron B4C particles.It can be deduced that B4C microparticles were more efficien in grain refinemen in comparison to the submicron B4C particles.In addition,it was observed that B4C microparticles were mainly distributed in the grain boundaries,while B4C nanoparticles were both distributed in the grain boundaries and inside the grains.

    Fig.6 and 7 show the SEM micrographs of the unreinforced alloy and 10 wt.% B4C/AZ31 composite samples after ageing treatment,respectively.According to Fig.6,the microstructure of the unreinforced AZ31 alloy mostly consists of MgZn (spot A in Fig.6),Mg2Al3(B in Fig.6),Mg17Al12(C in Fig.6),and Al4Mn (D in Fig.6) compounds,which was approved by EDS analysis.In the present research,the compounds were uniformly distributed in the samples.Theη-phase precipitations were formed continuously and discontinuously at the grain boundaries.The precipitations marked in Fig.6 had a dendritic morphology.The buildup of the solute phases and high temperature of the interface could cause conditions in which the melt was super-cooled in the solidificatio front.During these conditions,the interface became unstable that resulted in dendritic solidification Because of interface instability,the dendrites tended to branch.The precipitations were concentrated by the addition of B4C particles at the grain boundaries.For the as-cast 20 wt.% B4C/AZ31 composite sample,the Mg17Al12compound was diffused or dissolved in the matrix,which left behind shallow pores at the grain boundaries.These pores were also noticeable in sample 20 wt.% B4C/AZ31 approving the results discussed in the porosity section.

    Fig.7.SEM micrographs of the aged sample 10% B4C/AZ31 with different magnifications

    By comparing Figs.4 and 7,it can be said that ageing affects the diffusion and phase-generation processes in the matrix.It is evident that theβ-Mg17Al12phase was entirely dissolved,and instead,a granular intermetallic phase was formed close to the grains and at grain boundaries.The improvement in the mechanical strength was generally caused by the formation of thermodynamically stable phases,grain refinement and diffusion ofβ-Mg17Al12.EDS elemental analysis of A and B regions supported the presence of Mg2Al3and Al4Mn3compounds.

    3.4.Wear rate

    Contour plots of volumetric wear rate were developed for aged samples to facilitate the determination of sliding speed and applied load parameters (Fig.8).The data uncertainty was represented by the error bars,which was lower than 3%.Besides,by plotting the contour maps,the zones where B4C particles improved the wear behaviour of the composites were easily determined.B4C particles could pin the grain boundaries and prevent the grain boundary sliding.The reinforcement particles acted as a bonding agent in the matrix and improved the wear resistance.The wear behaviour of materials resulted from different parameters,including grain refinement porosity,strength,and hardness.The reduction in weight loss was related to the addition of B4C particles,which enhanced the strength and hardness of the composite samples.At all sliding speeds,a similar trend was detected (Fig.8a-c).With increasing the load for both unreinforced and composite samples,the volumetric wear rate increased that could be predictable by Archard’s law;however,decreases in the wear rate were detected under certain conditions.According to Archard’s law,the weight and volumetric loss for all samples declined with increasing the hardness (Figs.4 and 2).The wear rate of the composite containing 20 wt.% B4C differed slightly with respect to other samples.The composite samples showed lower hardness through the initial stage of sliding wear compared with the subsequent stages because after a certain sliding distance,the composites were subjected to strain hardening under the applied load during the continuous sliding [52].As can be seen,no rapid change in the wear behaviour is observed in the graph.The graphs of volumetric wear rate after the dry sliding test as a function of B4C content are shown in Fig.8b-d.Their trends were similar to that of dry sliding tests showing the reduction of wear rate during the tests.This phenomenon was related to surface plastic deformation.Furthermore,it was observed that regardless of the test speed,the wear rate of the sample 20 wt.% B4C/AZ31 was higher than that of the unreinforced sample under elevated loadings.Arrows on the contour maps of the wear rates show the zones where the reinforcement particles deteriorate the wear resistance (Fig.8b and c).The most signifi cant dissimilarity was seen over the speed range of 0.6–1 m/s(Fig.8d).Hence,the presence of B4C particles deteriorated the wear resistance of AZ31 alloy at elevated loadings.However,under low loadings (10–40 N),B4C reinforcement enhanced the wear resistance in comparison to the unreinforced AZ31 alloy at nearly all speeds (Fig.8a and d).Over the speed range of 0.1–0.5 m/s,the increase in the B4C content of the composite samples appeared to be beneficia to the wear resistance.For example,the wear rates of samples 10 wt.%B4C/AZ31 and 5 wt.%B4C/AZ31 reduced by ?30%and ?10%compared to unreinforced alloy,respectively.Nonetheless,under lower loadings,the dissimilarity of the wear rates was not significant

    The maximum wear rate was attained under high loadings for all sliding speeds,but it decreased when the sliding speed was decreased for composite samples.It was deduced that the dependence of the wear rate on the sliding speed was more notable under lower loadings.

    3.5.Friction coefficien

    Fig.8.Contour plots of volumetric wear rates (mm3/Nm) of the samples with different B4C contents: (a) unreinforced alloy,(b) 5% B4C/AZ31,(c) 10%B4C/AZ31,and (d) 20% B4C/AZ31.

    Graphs of friction coefficien as a function of sliding speed are shown in Fig.9.It was found that the friction coefficien of the unreinforced alloy was much lower than that of the composite samples.Additionally,sample 20 wt.% B4C/AZ31 had the highest friction coefficient All the friction coefficient were lower than 0.75,and in most cases,they were below 0.5.The friction coefficien was unsteady under low loadings up to 40 and 20 N for the unreinforced and the composite samples,respectively.On the other side,in the mentioned loading ranges,by elevating the applied load,the coefficien was slightly decreased,stabilized,and almost independent of the sliding speed.Similarly,the composite samples with higher reinforcement contents showed higher friction coefficients It can be concluded that different wear mechanisms were dominant for different test conditions and various reinforcement contents.The composites containing high reinforcement contents showed a more stable friction coefficient which was attributed to the wear behaviour of B4C particles.However,the decrease in the friction coefficien of aged composite samples was due to the formation of the Mg12Al17phase that ameliorates the wear resistance.Indeed less ploughing grooves cased impede the wear process,which decreases in friction coeffi cient [53].Regarding Ramezani and Ripin’s friction model[54],the coefficien of friction can be determined via calculating Ff/Fn.The friction force was directly associated with the friction coefficien under similar loading conditions.Consequently,it could be concluded that wear resistance was related to the friction coefficient

    3.6.Worn surface

    Fig.10a and b reveal the worn surfaces of the unreinforced and 10 wt.% B4C/AZ31 samples at a speed of 0.1 m/s,and loading of 10 N.In both images,grooves parallel to the sliding direction are evident,which is a characteristic of the abrasive wear.This mechanism was detected at low loadings and all sliding distances for all samples.These grooves were normally caused by the hard counterface that has ploughed the soft surface of the samples.The material surface was removed during this mechanism,and the mentioned grooves were formed at the surface.A similar case can be observed for samples containing 5 and 20 wt.% B4C.The abrasion mechanism was more evident in the unreinforced sample so that the formed grooves were more severe than those of the composite samples (Fig.10b).In fact,by increasing the B4C content,the abrasion mechanism was delayed.

    Fig.10c and d show the worn surfaces of the unreinforced and 10 wt.% B4C/AZ31 samples at the speed of 1 m/s,and load of 10 N.As can be seen,a thin layer of oxide is formed almost everywhere on the surface of the unreinforced sample.The presence of the compact oxide layer on the surface leads to the improvement of the wear-resistant.The oxygen concentration of the abraded surfaces confirm the domination of the oxidative wear (Fig.10I).In addition,SEM and EDS analyses of the worn surface approved the occurrence of severe oxidization.This phenomenon comes back to the generated heat during the sliding that led to the surface oxidation.Thereafter,the wear occurred due to the elimination of the oxidized fragments (Fig.10e).In some conditions,the detached oxide particles fille the voids,mixed with the surface composition,and formed a protective oxide layer during the wear test,known as MML [55,56].The formation of this oxide layer during the wear test prevented the contact of the pin and sample,and as a consequence,the wear rates decrease.The MML reduced the friction coefficient which is evident in Fig.9d.In previous works,it is reported that Mg alloys are susceptible to oxidation,and this tendency affects their wear rates[40].In this research,during continuous sliding,the brittle layer composing of MgO and/or Mg2Al2O4was fractured and formed fragments and a protective oxide layer on the surface of the alloy,which prevented the sliding surfaces from metal-to-metal contact during sliding.By comparing the wear rates of the unreinforced alloy and composite samples at the sliding speed of 1 m/s and loading of 60 and 80 N,it was revealed that the composite samples had a lower value.For composite samples under these conditions,oxidative wear was the dominant mechanism,and the formed oxide layer lowered the wear rate.Besides,this phenomenon occurred for the unreinforced alloy,which had a low wear rate.This could be related to two factors;(i) removal of the formed oxide layer of the unreinforced alloy due to low strength,(ii) exposure of a new surface to the wear and oxidation.In fact,oxidation of the new surface increases the wear rate.Moreover,the difference in the oxide layer types in the composite and unreinforced samples resulted in a higher wear resistance in the composite samples.Since the wear rate was low during the oxidative wear,this mechanism was considered as mild wear that could be dependant on the thickness of the oxide layer.The SEM micrographs showed bright regions on the surface,which were fully covered by an oxide layer.The EDS results in Fig.10 II demonstrate the strong peaks of oxygen and magnesium.Mild wear conditions resulted from the protection of the sliding surface by a thick oxide layer that caused low wear rates [57].Lim and Ashbay [58] suggested that a threshold velocity must be maintained until the surface heat generated a proper protective oxide film Moreover,they stated that to maintain the protective film the exposed sample must provide adequate physical support and oxidative wear was the dominant mechanism for narrow ranges of load and speed,where the oxidation layer was removed under severe conditions.Unlike the stated results of Lim and Ashby[58],the oxide layers were wider in the present investigation.

    Fig.9.Friction coefficien variations vs.loading for samples with different B4C contents at: (a) 0.1 m/s,(b) 0.3 m/s,(c) 0.7 m/s,and (d) 1 m/s.

    Fig.10.SEM micrographs and EDS analyses of the worn surfaces of samples with different B4C contents at various wear conditions: (a) unreinforced alloy at 0.1 m/s under 10 N,(b) 10% B4C/AZ31 at 0.1 m/s under 10 N,(c) unreinforced alloy at 1 m/s under 10 N,(d) and (e) 10% B4C/AZ31 at 1 m/s under 10 N,(f) unreinforced alloy at 0.1 m/s under 80 N,(g) 10% B4C/AZ31 at 0.1 m/s under 80 N,(h) unreinforced alloy at 1 m/s under 80 N,(i) 5% B4C/AZ31 at 1 m/s under 80 N,and (j) 10% B4C/AZ31 at 1 m/s under 80 N.

    Fig.10f demonstrates the worn surface of the unreinforced sample under the load of 80 N and speed of 0.1 m/s,which represents the delamination mechanism.When delamination is the dominant mechanism,the worn surface is detached in the form of layers.This is caused by the nucleation of cracks perpendicular to the sliding direction and growth of subsurface cracks during the wear process that leads to the delamination.The propagation of the subsurface cracks shears the surface,which results in the removal of fla es and laminates by coalescence of the cavities and formation of tunnels underneath the worn surface [49].It was observed that the detachment of fla es formed cracks perpendicular to the sliding direction.The dimensions of the laminates varied from 50 to 300 nm.Severe deformation of the fla y wear debris left shallow cavities on the surface (Fig.10f).As it was apparent,the width of the formed grooves varied from 20 up to 200 μm.

    For sample 10 wt.%B4C/AZ31,numerous fla es and chips were observed on the surface (Fig.10g).The induced fatigue during the sliding resulted in the deformation of the subsurface,nucleation of cracks,and crack propagation.In fact,the elevation of the applied load promoted the process and led to delamination wear.For all composite samples,it was determined that under high loadings (40–80 N) and low speeds(0.1–0.3 m/s),the delamination occurred simultaneously with an abrasion mechanism.However,this loading range was narrower for sample 20 wt.% B4C/AZ31 (at the speeds of 0.1 and 0.5 m/s and loadings of 60–80 N).The ceramic/matrix interface contributed to void nucleation by providing preferential paths for crack propagation [59].In addition,it was found that in comparison with the unreinforced alloy,the wear rate of the composite samples at the sliding speed of 0.1 m/s and loading of 80 N was higher.This discrepancy indicated that in the composites,the dominant wear mechanism changed from abrasion to delamination wear.This findin was consistent with earlier previous studies [18,31],which reported the destructive effect of particulate reinforcement on strength in the delamination mechanism.Fig.10g demonstrates the delamination of composite samples,which represents mild wear conditions.Under constant loading conditions,a transition from abrasion to delamination mechanism was detected in the wear behaviour.The most important factor,which determined the wear mechanism was the temperature elevation of the contact surfaces.Indeed,the increase in temperature led to softening and adhesion of the surface roughness.On the other hand,no adhesion was observed on the counterface.For this reason,the abrasive debris accumulated on the contact surface during the continuous sliding,which resulted in crack nucleation beneath the surface and separation of the laminates [40,49].After the delamination,the surface was oxidized due to the exposure of the fresh surface to the atmosphere.

    Fig.10h shows that the dominant wear mechanism at high speeds and loadings is plastic deformation for the unreinforced sample.This findin was in agreement with previous reports on other Mg alloys [49].In these circumstances,local melting of low-melting-temperature phases of the matrix and/or severe plastic deformation induced by thermal softening could occur.According to this figure the oxides and grooves caused by the abrasion mechanism could not be observed because of the severe surface deformation.Another evidence to confir the dominant mechanism (plastic deformation)was the small amount of detached debris.In fact,during the plastic deformation,high loadings and sliding speeds enhance the temperature of the sample and the pin,which leads to the melting of the Mg alloy matrix [33].

    On the other hand,as shown in Fig.10i,the deformation extensively damages the surface under the loading conditions for 5 wt.%B4C/AZ31 sample.This damage demonstrates that the transition from the delamination to the plastic deformation wear mechanism occurred by increasing the sliding speed under high loadings.This transition (mild to severe wear)took place mainly owing to the increase in surface roughness,while the reason for the plastic deformation was temperature elevation at the steel counterface/sample interface [60].With the temperature elevation,the strength of the samples was declined,and consequently,the surface was more susceptible to plastic deformation [33].

    The wear rate of the 10 wt.%B4C/AZ31composite showed that the B4C particles in the Mg alloys were beneficia to wear resistance.The presence of particles with bimodal distribution in the Mg matrix prevented the thermal softening of the composite.In fact,the presence of B4C particles and precipitations caused the formation of geometrically necessary dislocations in the matrix during the cooling stage of the casting and ageing process.Consequently,it improved the strength,which resulted in the reduction of the plastic deformation during the wear test (Fig.10j).Furthermore,it can be said that the presence of ceramic particles hindered the effect of the temperature elevation on the wear mechanism during the test.Additionally,no crack,which could be nucleated due to the loading force,was evident.It can be concluded that the composites strengthened by B4C particles exhibit higher delamination resistance.

    Fig.11 indicates that at high speeds and loadings,the dominant wear mechanism is abrasion for the 20 wt.% B4C/AZ31 composite.Hence,the wear rate of 20 wt.% B4C/AZ31 composite was higher than that of the unreinforced alloy under the most severe conditions.In these conditions,the wear resistance of this composite sample was not improved.This could be described by the high ductility of the unreinforced AZ31 alloys.Since a broad area of the surface was worn without cracks,the plastic deformation was considered as a severe wear mechanism.Achieving a homogeneous distribution of the particles during the preparation was desirable for obtaining high wear resistance.Nevertheless,a few reinforcement particles agglomerated in the matrix,which was attributed to the abrasive wear mechanism.In this mechanism,due to wedging and ploughing of the steel pin,fin particles were formed,or the debris were removed from the surface,and the particles adhered to the contact surface [40,61].Wider grooves and scratches could be intensifie by abrading using low hardness materials.The grooves were evident at the centre of the abrasive wear area (Fig.11b).Generally,when a hard material slides over a soft surface,the surface roughness acts as an abrader,and the process is called two-body abrasion.But,when particles,which are sufficientl hard to abrade one or both surfaces,are trapped between the contact surfaces,the phenomenon is called three-body abrasion.This wear mechanism can be active at wear loading conditions and can occur simultaneously with other mechanisms[62,63].This behaviour can be attributed to the entrapment of the separated and fractured ceramic particles at the sliding interface,which contributes to the abrasive wear.This is consistent with the reports of Kwok and Lim [64] for Al/SiC composites.The presence of debris particles with elongated form in Fig.10c,confirme the domination of the abrasion wear mechanism.

    Fig.11.SEM micrographs of the worn surfaces of 20% B4C/AZ31 sample with different magnifications

    By evaluating the parameters of wear rate,friction coeffi cient and observing the SEM micrographs of the worn surfaces,the wear mechanism maps were constructed for each sample (Fig.12).As can be seen in the figure the dominant mechanism in each region is defined and the boundaries represent the transitions.Thus,regardless of the low sliding speed and low loadings,abrasive wear was the dominant mechanism for all the samples.Nevertheless,an increase in the applied load resulted in the domination of oxidative wear.At low-speed regimes,by increasing the loading,fatigue-induced surficia cracks and separated or delaminated the material;therefore,the wear rate increased and caused a transition from abrasive wear to delamination mechanism.For the unreinforced alloy,this transition occurred at loadings higher than 80 N.But in the composites,higher speeds and loadings were required for shifting the mechanism to the delamination wear.For the 5 wt.% B4C/AZ31 composite,it was revealed that at low sliding speeds,the transition occurred at loadings higher than 150 N.As a matter of fact,when the B4C content was increased to 10 wt.% in the composite,an increase in both sliding speed and the loading was necessary for the transition.It should be noted that,under high loadings;(i) the oxide layer was formed on the surface of the composites,acting as a protecting layer and hindering the transition from the oxidative and abrasive wear to delamination mechanism,and (ii) the B4C particles successfully improved the mechanical properties of the Mg alloy matrix.

    Additionally,high B4C contents in the composite(10 wt.%B4C/AZ31) led to the formation of a more compact oxide layer,protecting the surface from metallic wear up to 80 N at low speeds.Thus,higher speeds were required to change the wear mechanism,where delamination was the dominant wear mechanism for the composites and the unreinforced alloy (Fig.12c).The wear rates of the composite samples were generally lower than that of the unreinforced alloy.The elevated wear rates were observed in Fig.2c and Fig.2d for the composites when the loading was more than 80 N at the sliding speeds of 0.5 m/s and 1 m/s,respectively.A gradual transition from delamination to plastic deformation occurred for the composite samples under these intense conditions.

    To evaluate the effect of the microstructure on the wear behaviour of the unreinforced alloy,the obtained wear mechanism map was compared with the results of Chen et al.[34] for a dendritic AZ91 Mg alloy under similar loading and speed ranges.They also described two different wear behaviours for the samples;mild wear behaviour,characterized by oxidative and delamination mechanisms,and severe wear behaviour,which was identifie by plastic deformation.They constructed a wear transition map,which was consistent with the attained results of this study on AZ91 alloy.This confirme that the wear parameters had a stronger influenc on the wear behaviour in comparison with the microstructure that might be owing to the role of the B4C/matrix interface that could facilitate the nucleation and propagation of cracks.

    4.Conclusions

    In this investigation,unreinforced AZ31 Mg alloy and AZ31 matrix composites reinforced by bimodal size B4C particles were prepared using a stir casting technique followed by precipitation hardening treatment.Thereafter,the effect of B4C content on the microhardness,dry sliding wear behaviour,and microstructure of the samples was studied.Based on the results,the following conclusions can be drawn:

    1.Uniform dispersion of bimodal size B4C particles in the AZ31 matrix can be successfully obtained via the stir casting method.The porosity of the B4C/AZ31 composites was slightly increased by enhancing the B4C content.

    2.The microhardness of the composites was increased by enhancing the B4C content for all the samples.After 10 h of age hardening,the hardness of all composites was increased as a consequence of the homogeneous distribution of the reinforcement particles.

    Fig.12.Wear mechanism maps for samples with different B4C contents: (a) unreinforced alloy,(b) 5% B4C/AZ31,(c) 10% B4C/AZ31,and (d) 20%B4C/AZ31.

    3.The addition of B4C particles to the AZ31 matrix caused a considerable decrease in the wear rate.

    4.The oxidative wear mechanism was dominant at low loadings (10–40 N) and high speeds.Oxidative wear was observed more frequently for the composite samples,which had a protective oxide layer and a minimum wear rate of 0.013 mm3/Nm for sample 10 wt.% B4C.

    5.The lowest coefficien of friction (0.3) was observed for the composite samples for 10 wt.% B4C at the speed of 1 m/s.

    6.By increasing the load,the plastic deformation was dominant due to the elevation of the frictional heating that resulted in the surface melting.

    7.At low speeds and under low loadings,the abrasive wear was dominant,while by increasing the load,delamination was dominant.This behaviour was similar to that of AZ31 alloys and implied the insignifican effect of microstructure on the wear conditions.

    8.A delay was detected for the transition to delamination wear mechanism when the B4C content was increased(sample 10 wt.% B4C/AZ31).

    9.Under the most intense conditions (sliding speed of 0.5–1 m/s and loadings of 60–80 N),the dominant mechanism was abrasive wear for the sample containing 20 wt.% B4C.

    All in all,it can be concluded that under these circumstances,the presence of B4C particles did not improve the wear resistance of composite samples.

    Declaration of Competing Interest

    The authors declare that they have no known competing financia interests or personal relationships that could have appeared to influenc the work reported in this paper.

    九九在线视频观看精品| 各种免费的搞黄视频| 久久鲁丝午夜福利片| 午夜视频国产福利| 韩国高清视频一区二区三区| 能在线免费看毛片的网站| 中文字幕最新亚洲高清| 看免费成人av毛片| 美女中出高潮动态图| 国产精品熟女久久久久浪| 亚洲欧洲日产国产| av免费观看日本| 亚洲国产精品一区二区三区在线| 国产成人午夜福利电影在线观看| 少妇人妻 视频| 新久久久久国产一级毛片| 下体分泌物呈黄色| 久久午夜福利片| 国产精品国产av在线观看| 蜜桃久久精品国产亚洲av| videosex国产| 少妇被粗大的猛进出69影院 | 精品久久久噜噜| 日韩一区二区三区影片| 久久国内精品自在自线图片| 精品一区在线观看国产| 久久久久久久久大av| 亚洲激情五月婷婷啪啪| 黑丝袜美女国产一区| 尾随美女入室| 国产精品麻豆人妻色哟哟久久| 亚洲精品久久午夜乱码| 国产男女内射视频| 日韩精品有码人妻一区| 久久免费观看电影| 插逼视频在线观看| 欧美激情极品国产一区二区三区 | 麻豆精品久久久久久蜜桃| 亚洲综合精品二区| 一区二区三区四区激情视频| 久久ye,这里只有精品| 又大又黄又爽视频免费| 国产精品 国内视频| 99视频精品全部免费 在线| 五月开心婷婷网| 80岁老熟妇乱子伦牲交| 国产高清三级在线| 自线自在国产av| 国产精品国产三级国产专区5o| 亚洲精品国产av成人精品| 天堂8中文在线网| 久久人人爽人人爽人人片va| 国产成人91sexporn| 成人国产麻豆网| 精品久久久久久久久亚洲| 国产精品成人在线| 高清黄色对白视频在线免费看| 久久久国产精品麻豆| 久久久久久久久久成人| 日韩在线高清观看一区二区三区| 日韩精品免费视频一区二区三区 | 大码成人一级视频| 亚洲欧洲国产日韩| 欧美日韩视频精品一区| 国产精品 国内视频| av网站免费在线观看视频| 永久网站在线| 性高湖久久久久久久久免费观看| 日韩成人伦理影院| 免费黄频网站在线观看国产| 欧美成人午夜免费资源| 免费看av在线观看网站| 中文字幕精品免费在线观看视频 | 国产男人的电影天堂91| 最黄视频免费看| 只有这里有精品99| 制服丝袜香蕉在线| 久久久久久久久久人人人人人人| 夜夜爽夜夜爽视频| 亚洲精品一区蜜桃| 欧美亚洲日本最大视频资源| 亚洲国产精品成人久久小说| 丰满少妇做爰视频| 最后的刺客免费高清国语| 久久久久久久亚洲中文字幕| 日本黄色日本黄色录像| 美女大奶头黄色视频| 九九久久精品国产亚洲av麻豆| 日韩熟女老妇一区二区性免费视频| 性色av一级| 九色亚洲精品在线播放| 日韩 亚洲 欧美在线| 亚洲精品第二区| 在线 av 中文字幕| 亚洲四区av| 国产黄片视频在线免费观看| 日韩强制内射视频| 2018国产大陆天天弄谢| 少妇人妻久久综合中文| 久久久久久久久久人人人人人人| 日韩视频在线欧美| 女的被弄到高潮叫床怎么办| 香蕉精品网在线| 免费看av在线观看网站| 国产黄色视频一区二区在线观看| 亚洲欧美日韩另类电影网站| 亚洲国产精品一区三区| 一级,二级,三级黄色视频| 男的添女的下面高潮视频| 亚洲国产精品一区二区三区在线| 亚洲成色77777| 99精国产麻豆久久婷婷| 久久人妻熟女aⅴ| 亚洲av欧美aⅴ国产| 亚洲av欧美aⅴ国产| av福利片在线| 久久免费观看电影| 又粗又硬又长又爽又黄的视频| av免费观看日本| 2018国产大陆天天弄谢| 成人漫画全彩无遮挡| 啦啦啦中文免费视频观看日本| 久久韩国三级中文字幕| 久久午夜福利片| 亚洲国产最新在线播放| 老司机影院成人| 国产精品99久久99久久久不卡 | 一级黄片播放器| 18禁动态无遮挡网站| 十八禁高潮呻吟视频| 成人综合一区亚洲| 另类亚洲欧美激情| 亚洲,欧美,日韩| 伦理电影大哥的女人| 国产高清不卡午夜福利| 免费观看av网站的网址| 久久久亚洲精品成人影院| 亚洲精品亚洲一区二区| 国产精品无大码| 少妇丰满av| 99热网站在线观看| 亚洲av福利一区| 中文字幕最新亚洲高清| av国产精品久久久久影院| 91在线精品国自产拍蜜月| av国产久精品久网站免费入址| 我要看黄色一级片免费的| 在现免费观看毛片| 国产老妇伦熟女老妇高清| 欧美精品亚洲一区二区| 99热这里只有是精品在线观看| 亚洲av不卡在线观看| 亚洲精品一区蜜桃| 大又大粗又爽又黄少妇毛片口| 久久婷婷青草| 91精品一卡2卡3卡4卡| 国产一区二区三区综合在线观看 | 久久毛片免费看一区二区三区| 色5月婷婷丁香| 日韩熟女老妇一区二区性免费视频| 熟女电影av网| 久久久亚洲精品成人影院| 中文欧美无线码| 99热国产这里只有精品6| 久久久久久久久久久免费av| 国产午夜精品久久久久久一区二区三区| 免费不卡的大黄色大毛片视频在线观看| 大片电影免费在线观看免费| 简卡轻食公司| 91精品一卡2卡3卡4卡| 亚洲av综合色区一区| 亚洲人与动物交配视频| 天堂俺去俺来也www色官网| 精品视频人人做人人爽| 满18在线观看网站| 十分钟在线观看高清视频www| 精品国产国语对白av| 成年av动漫网址| 日韩熟女老妇一区二区性免费视频| 免费观看a级毛片全部| 黄片播放在线免费| 另类精品久久| 久久精品国产亚洲网站| 亚洲精品国产av成人精品| 曰老女人黄片| 狂野欧美激情性bbbbbb| 日日啪夜夜爽| 80岁老熟妇乱子伦牲交| 亚洲,欧美,日韩| 边亲边吃奶的免费视频| 午夜日本视频在线| 免费不卡的大黄色大毛片视频在线观看| 午夜久久久在线观看| 亚洲精品乱久久久久久| 欧美少妇被猛烈插入视频| 在线观看国产h片| 免费观看性生交大片5| 99九九在线精品视频| 老司机亚洲免费影院| 亚洲精品成人av观看孕妇| 妹子高潮喷水视频| 欧美成人午夜免费资源| 一个人看视频在线观看www免费| 日日摸夜夜添夜夜添av毛片| 欧美日韩视频高清一区二区三区二| 午夜免费鲁丝| 丰满少妇做爰视频| 亚洲精品日本国产第一区| 狂野欧美激情性bbbbbb| 久久久久久久大尺度免费视频| av线在线观看网站| 日韩视频在线欧美| 日韩一本色道免费dvd| 成人手机av| 日本午夜av视频| 一本—道久久a久久精品蜜桃钙片| 18禁在线无遮挡免费观看视频| 午夜福利影视在线免费观看| 日韩 亚洲 欧美在线| 欧美丝袜亚洲另类| 乱人伦中国视频| 免费人成在线观看视频色| 在线精品无人区一区二区三| 欧美激情极品国产一区二区三区 | av在线app专区| 久久狼人影院| 我的老师免费观看完整版| 在线观看免费日韩欧美大片 | 少妇人妻精品综合一区二区| 欧美成人精品欧美一级黄| 在线观看人妻少妇| 少妇的逼水好多| 成人免费观看视频高清| 国产女主播在线喷水免费视频网站| 免费人妻精品一区二区三区视频| 91国产中文字幕| 国产伦精品一区二区三区视频9| 国产欧美另类精品又又久久亚洲欧美| 国产视频首页在线观看| 毛片一级片免费看久久久久| a级毛片黄视频| 欧美日韩亚洲高清精品| 国产亚洲精品第一综合不卡 | 天天影视国产精品| 蜜桃在线观看..| 老司机影院毛片| 一级,二级,三级黄色视频| 26uuu在线亚洲综合色| 精品久久久久久久久av| 91精品国产国语对白视频| 在现免费观看毛片| 蜜桃国产av成人99| 在线观看一区二区三区激情| 亚洲无线观看免费| 你懂的网址亚洲精品在线观看| 免费高清在线观看视频在线观看| 久久久久久伊人网av| 天堂中文最新版在线下载| 高清黄色对白视频在线免费看| 国产 一区精品| 亚洲av福利一区| 亚洲,一卡二卡三卡| 国产老妇伦熟女老妇高清| 欧美日韩亚洲高清精品| 成年女人在线观看亚洲视频| 性高湖久久久久久久久免费观看| 亚洲av欧美aⅴ国产| 日本wwww免费看| 成人漫画全彩无遮挡| 一本久久精品| 少妇猛男粗大的猛烈进出视频| 黄色视频在线播放观看不卡| 自线自在国产av| 蜜桃在线观看..| 寂寞人妻少妇视频99o| 成人黄色视频免费在线看| 日本猛色少妇xxxxx猛交久久| 成人无遮挡网站| 在线观看www视频免费| 久久99热6这里只有精品| 蜜桃国产av成人99| 久久久久久人妻| 欧美一级a爱片免费观看看| 大香蕉久久网| 中文欧美无线码| 国产国拍精品亚洲av在线观看| 好男人视频免费观看在线| 天堂俺去俺来也www色官网| 欧美97在线视频| 亚洲成色77777| 一区二区三区精品91| 亚洲av福利一区| 嫩草影院入口| 国产亚洲一区二区精品| 久久狼人影院| 国产有黄有色有爽视频| 日本av免费视频播放| 2018国产大陆天天弄谢| 久久午夜福利片| 黄色视频在线播放观看不卡| 精品亚洲乱码少妇综合久久| 99re6热这里在线精品视频| 国产女主播在线喷水免费视频网站| 久久久久精品久久久久真实原创| 久久ye,这里只有精品| 免费观看的影片在线观看| 国产欧美日韩一区二区三区在线 | 搡女人真爽免费视频火全软件| 亚洲国产精品一区三区| 曰老女人黄片| av在线老鸭窝| 人体艺术视频欧美日本| 免费观看a级毛片全部| 18禁在线播放成人免费| 国产精品一区www在线观看| 涩涩av久久男人的天堂| av有码第一页| 午夜免费鲁丝| 亚洲av免费高清在线观看| 久久久久久久国产电影| 人妻一区二区av| 亚洲av中文av极速乱| 大片电影免费在线观看免费| 夜夜骑夜夜射夜夜干| 中文字幕免费在线视频6| 国产毛片在线视频| 亚洲av中文av极速乱| 高清av免费在线| 国语对白做爰xxxⅹ性视频网站| 午夜精品国产一区二区电影| 人妻一区二区av| 亚洲av中文av极速乱| a级毛片免费高清观看在线播放| 国内精品宾馆在线| 精品亚洲成a人片在线观看| 看十八女毛片水多多多| 婷婷色综合大香蕉| 日日爽夜夜爽网站| 蜜桃国产av成人99| 国产毛片在线视频| av在线观看视频网站免费| av一本久久久久| 亚洲欧美日韩另类电影网站| av专区在线播放| 午夜福利网站1000一区二区三区| 18禁裸乳无遮挡动漫免费视频| 丝袜美足系列| 久久精品国产亚洲av天美| 看免费成人av毛片| 国产精品一国产av| 人人妻人人添人人爽欧美一区卜| 国产视频内射| 18+在线观看网站| freevideosex欧美| 成人影院久久| 一级黄片播放器| kizo精华| 婷婷色麻豆天堂久久| 高清不卡的av网站| tube8黄色片| 日韩av不卡免费在线播放| 99久久中文字幕三级久久日本| 色视频在线一区二区三区| 丝袜在线中文字幕| 国产一区二区三区综合在线观看 | 久久99一区二区三区| 精品午夜福利在线看| 亚洲av免费高清在线观看| 成人午夜精彩视频在线观看| 日本与韩国留学比较| 日日爽夜夜爽网站| 精品亚洲乱码少妇综合久久| 美女脱内裤让男人舔精品视频| 亚洲伊人久久精品综合| 免费黄色在线免费观看| 欧美激情国产日韩精品一区| 少妇被粗大猛烈的视频| 日韩欧美精品免费久久| 国产亚洲av片在线观看秒播厂| 一级毛片黄色毛片免费观看视频| 精品午夜福利在线看| 久久99热6这里只有精品| 欧美日本中文国产一区发布| 日韩伦理黄色片| 人妻人人澡人人爽人人| 免费人成在线观看视频色| 亚洲激情五月婷婷啪啪| 久久午夜综合久久蜜桃| 久久久久久久大尺度免费视频| 久久久久久久久久人人人人人人| 亚洲综合色惰| 女性被躁到高潮视频| 80岁老熟妇乱子伦牲交| 国产精品偷伦视频观看了| 日日爽夜夜爽网站| 一个人免费看片子| 成人毛片a级毛片在线播放| 国产日韩一区二区三区精品不卡 | 久久久国产欧美日韩av| 成人毛片a级毛片在线播放| 国产精品女同一区二区软件| 亚洲精品456在线播放app| 人人妻人人澡人人爽人人夜夜| 一本色道久久久久久精品综合| 国内精品宾馆在线| 久久毛片免费看一区二区三区| 成人手机av| 黄色毛片三级朝国网站| 亚洲欧美色中文字幕在线| 91午夜精品亚洲一区二区三区| 丰满迷人的少妇在线观看| 国产精品久久久久久久久免| 久久精品人人爽人人爽视色| 五月玫瑰六月丁香| 色婷婷久久久亚洲欧美| 蜜桃在线观看..| 看非洲黑人一级黄片| 插阴视频在线观看视频| 久久婷婷青草| 日本午夜av视频| 国产亚洲精品久久久com| 蜜桃在线观看..| 五月伊人婷婷丁香| 欧美日韩国产mv在线观看视频| 国产免费又黄又爽又色| 日韩av在线免费看完整版不卡| 日本爱情动作片www.在线观看| 一个人免费看片子| 久久久午夜欧美精品| 少妇猛男粗大的猛烈进出视频| 亚洲第一av免费看| 精品人妻偷拍中文字幕| 人人妻人人添人人爽欧美一区卜| 精品少妇久久久久久888优播| 国产精品久久久久久精品古装| 夫妻性生交免费视频一级片| 亚洲高清免费不卡视频| av黄色大香蕉| 人成视频在线观看免费观看| 制服人妻中文乱码| 高清在线视频一区二区三区| 亚洲av欧美aⅴ国产| 午夜免费鲁丝| 亚洲少妇的诱惑av| 日韩av在线免费看完整版不卡| xxxhd国产人妻xxx| 亚洲第一av免费看| 最新的欧美精品一区二区| 国产av国产精品国产| 在线观看一区二区三区激情| 久久99蜜桃精品久久| 一本大道久久a久久精品| 赤兔流量卡办理| 国产极品粉嫩免费观看在线 | 精品人妻熟女av久视频| 国产精品一区二区三区四区免费观看| 亚洲一级一片aⅴ在线观看| 飞空精品影院首页| tube8黄色片| 国产精品偷伦视频观看了| 能在线免费看毛片的网站| 赤兔流量卡办理| 亚洲欧洲国产日韩| 亚洲av免费高清在线观看| 老女人水多毛片| 欧美日韩一区二区视频在线观看视频在线| 2018国产大陆天天弄谢| 久久久精品区二区三区| 亚洲成人av在线免费| 久久久精品94久久精品| 内地一区二区视频在线| 久久免费观看电影| 91精品国产国语对白视频| 精品视频人人做人人爽| 美女主播在线视频| 精品人妻熟女av久视频| 亚洲中文av在线| 多毛熟女@视频| 欧美成人午夜免费资源| 免费人妻精品一区二区三区视频| 大片免费播放器 马上看| 日韩视频在线欧美| 人成视频在线观看免费观看| 中文字幕最新亚洲高清| 蜜桃久久精品国产亚洲av| 天天操日日干夜夜撸| 久久国产亚洲av麻豆专区| av视频免费观看在线观看| 国产国语露脸激情在线看| 人妻系列 视频| 熟女电影av网| 黄色怎么调成土黄色| 精品久久久噜噜| 国产极品粉嫩免费观看在线 | 精品亚洲乱码少妇综合久久| 成年人免费黄色播放视频| 草草在线视频免费看| 久久精品夜色国产| 成人亚洲欧美一区二区av| 午夜免费鲁丝| 热99久久久久精品小说推荐| 十分钟在线观看高清视频www| 丝袜在线中文字幕| 边亲边吃奶的免费视频| 99九九在线精品视频| 在线播放无遮挡| 大码成人一级视频| 黑人巨大精品欧美一区二区蜜桃 | 欧美三级亚洲精品| 黑人欧美特级aaaaaa片| 精品亚洲成a人片在线观看| 91国产中文字幕| 亚洲精品日本国产第一区| 波野结衣二区三区在线| 久久久久人妻精品一区果冻| 国产日韩欧美在线精品| 少妇人妻 视频| 一区二区三区乱码不卡18| 日韩在线高清观看一区二区三区| 亚洲av福利一区| 精品人妻一区二区三区麻豆| 国产精品一国产av| 精品人妻熟女av久视频| 你懂的网址亚洲精品在线观看| 91久久精品国产一区二区成人| 国产不卡av网站在线观看| 777米奇影视久久| 国产乱人偷精品视频| 日本午夜av视频| 一级黄片播放器| 亚洲国产精品一区二区三区在线| 一二三四中文在线观看免费高清| 国产毛片在线视频| 国产高清国产精品国产三级| 久热这里只有精品99| av又黄又爽大尺度在线免费看| 伊人久久国产一区二区| 69精品国产乱码久久久| 久久久精品区二区三区| 亚洲一区二区三区欧美精品| 免费日韩欧美在线观看| 夜夜看夜夜爽夜夜摸| 午夜老司机福利剧场| 性高湖久久久久久久久免费观看| 啦啦啦中文免费视频观看日本| 色5月婷婷丁香| 在线观看国产h片| 国产午夜精品一二区理论片| 亚洲av福利一区| 老女人水多毛片| 日韩制服骚丝袜av| 欧美成人午夜免费资源| 欧美bdsm另类| 中文字幕制服av| 国产一区二区在线观看av| 亚洲精品乱码久久久v下载方式| 视频区图区小说| 国产亚洲精品第一综合不卡 | 黄片无遮挡物在线观看| 欧美xxxx性猛交bbbb| 一级,二级,三级黄色视频| av女优亚洲男人天堂| 亚洲一区二区三区欧美精品| 麻豆精品久久久久久蜜桃| 亚洲熟女精品中文字幕| 天堂俺去俺来也www色官网| 亚洲av中文av极速乱| 狂野欧美白嫩少妇大欣赏| 中文天堂在线官网| 丝袜脚勾引网站| 亚洲激情五月婷婷啪啪| 青春草国产在线视频| 精品人妻偷拍中文字幕| av不卡在线播放| 久久人妻熟女aⅴ| av不卡在线播放| 国产熟女欧美一区二区| 国语对白做爰xxxⅹ性视频网站| 亚洲人成77777在线视频| 国产精品久久久久久av不卡| 少妇高潮的动态图| 国产成人免费无遮挡视频| 黄色一级大片看看| xxxhd国产人妻xxx| 日本黄色日本黄色录像| 国产成人av激情在线播放 | 日本免费在线观看一区| 春色校园在线视频观看| 全区人妻精品视频| av电影中文网址| 高清午夜精品一区二区三区| 人妻人人澡人人爽人人| 国产熟女欧美一区二区| 国产精品熟女久久久久浪| 亚洲第一区二区三区不卡| av不卡在线播放| 人妻夜夜爽99麻豆av| 国产精品久久久久久精品电影小说| 永久网站在线| 国产精品久久久久久精品电影小说| 亚洲av欧美aⅴ国产| 最近2019中文字幕mv第一页| 超色免费av| 久久精品国产亚洲网站| 久久99精品国语久久久| 啦啦啦啦在线视频资源| 哪个播放器可以免费观看大片| 欧美 日韩 精品 国产| 久久精品久久久久久噜噜老黄| 亚洲不卡免费看| av免费在线看不卡| 天天影视国产精品| 有码 亚洲区| 蜜桃在线观看..| 欧美日韩视频高清一区二区三区二|