    Role of bimodal-grained structure with random texture on mechanical and corrosion properties of a Mg-Zn-Nd alloy

    2022-10-25 09:28:26MingGaoKeYangLiliTanZhengMa
    Journal of Magnesium and Alloys 2022年8期

    Ming Gao ,Ke Yang ,Lili Tan,? ,Zheng Ma,?

    aSchool of Materials Science and Engineering,University of Science and Technology of China,Shenyang,110016,China

    b Shi-changxu Innovation Center for advanced Materials,Institute of Metal Research,Chinese Academy of Sciences,Shenyang,110016,China

    Abstract Fine grained ZN20 alloy was obtained by combining equal-channel angular pressing (ECAP) with extrusion.Microstructural observation showed an obvious grain refinement with an average grain size of 10μm after ECAP.The original bimodal-grained structure composed of coarse grains with strong basal texture and fine grains with random texture was substituted by a new kind of bimodal-grained structure with finer grains and more random texture after 4 passes ECAP at 300 °C.The combination of grain refinement and texture weakening caused the ductility can be increased by 40% compared with the as-extruded alloy.Immersion test in simulated intestinal fluid revealed an improvement of corrosion resistance after ECAP.Grain refinement can stable the corrosion product layer and basal texture is more beneficial for the corrosion resistance than the non-basal texture.

    Keywords: Magnesium;ECAP;Bimodal-grained structure;Corrosion resistance;Mechanical property.

    1.Introduction

    Magnesium and its alloys with excellent specific properties are regarded as the most promising candidate as a kind of biodegradable materials [1-4].It can degrade totally after implanted in human body and reduce patients’ pain without second surgery to remove the implant.Moreover,magnesium is an essential nutrient element in human body [5,6].However,the relatively poor formability and corrosion resistance are the bottlenecks that restrict the widespread applications of magnesium and its alloys as biomedical materials.This situation makes it pretty urgent to improve the formability and corrosion resistance of magnesium alloys for future applications [7-11].

    Grain refinement and homogeneous distribution of second phase in matrix are effective ways to improve the mechanical property and promote uniform corrosion behavior of magnesium alloys [12-15].The ultra-fine grain (UFG) structure can be achieved by severe plastic deformation (SPD)techniques.As a kind of this method,equal channel angular pressing (ECAP) is an effective way to improve the mechanical property and corrosion resistance of magnesium alloys by grain refinement and texture weakening.The effects of different processing parameters on the mechanical property and the corrosion resistance have already been explained clearly in the past few years.Magnesium alloy with different microstructure can be obtained by altering the processing temperature and the number of passes of ECAP.The effect of grain refinement is obvious when the temperature is low enough,and the increase of passes is beneficial for the uniform dispersion of the grain size [16-21].

    The bimodal-grained structure,which is common in magnesium alloys,could be obtained by ECAP at low temperature and with specific parameter [22,23].Many studies have been clearly explained the influence of bimodal-grained structure on mechanical properties of magnesium alloys [24-27].This typical structure is mainly composed of coarse un-dynamic recrystallized (unDRXed) grains with relative strong textures and fine dynamic recrystallized (DRXed) grains with very random texture.The strength of magnesium alloy can be improved effectively by the texture strengthening in unDRXed grains and the grain boundary strengthening in DRXed grains.The stronger texture in unDRXed grains will promote the formation of tension twinning,which can act as the crack source and finally has a negative influence on the ductility of magnesium alloys.Therefore,such a kind of microstructure will cause a characteristic of high strength and low ductility.It is important for magnesium alloy,which slip system at room temperature is limited,to improve the ductility for subsequent processing.Besides,few studies focused on the influence of bimodal-grained structure on corrosion resistance of magnesium alloy,which is also essential to biomedical material.

    As a nutrient element,Zn can improve the mechanical property and corrosion resistance by solid solution strengthening and increasing the corrosion potential.The addition of Nd has a positive influence on the ductility of magnesium alloy by texture weakening.And the biological safety has also been proved when the content of Nd is low enough [28,29].Therefore,a Mg-2Zn-0.5Nd (ZN20) alloy was extruded with a high extrusion ratio at low temperature to obtain a bimodal grained structure in this study.But the strong texture in un-DRXed grains will lead to the formation of twinning,and it had a negative influence on the ductility of ZN20 alloy.Therefore,4 passes ECAP at different processing temperature was carried out to modify this original bimodal-grained structure and the texture characteristic.ECAP combined with extrusion was expected to obtain a bimodal grained structure with random texture and improve the ductility of ZN20 alloy by inhibiting the premature appearance of twinning during deformation.Such a bimodal grained structure with random texture should improve the strength,ductility and corrosion resistance of ZN20 alloy comprehensively.Therefore,microstructure evolution,mechanical property and corrosion resistance of ZN20 alloy processed by extrusion and ECAP were studied to explore the influence of bimodal-grained structure on the mechanical property and corrosion resistance.

    2.Materials and methods

    2.1.Materials and ECAP processing

    In this study,ECAP was performed on an extruded ZN20 alloy with a chemical composition of 1.84% Zn,0.52% Nd and remaining Mg.As-cast ZN20 alloy was prepared by melting pure Mg (99.99%),pure Zn (99.99%) and Mg-20%Nd master alloy in a resistance furnace under a protective atmosphere of mixed SF6and CO2.Then it was homogenized at 325 °C for 10h and machined into billets with diameter of 80mm and height of 100mm.Then they were preheated at 390 °C for 2h and extruded into 10mm cylindrical rods with an extrusion rate of 10mm s-1and an extrusion ratio of 64.The ECAPed rods were cut into billets with length of 100mm.The die for ECAP was heated in an electrical resistance furnace,which was placed on the outside of the die,and the temperature was monitored by a thermocouple inserted in the bottom of the die.The sample was pressed into the die with a speed of 30mm min-1,lubricated by molybdenum disulphide (MoS2) and then rotated along extrusion direction(ED) by 90° in the same direction before each new pass.It has been reported in some researches that increasing the processing temperature was beneficial for improving the formability and reducing the defects in the sample,and increasing the passes of ECAP was beneficial for the grain refinement[16-21].Therefore,two different temperatures,300 °C and 350 °C,and 4 passes were chosen to obtain the bimodalgrained structure with random texture.The ZN20 alloy samples after extrusion,4 passes ECAP at 300 °C and 4 passes ECAP at 350 °C were marked as E,E1 and E2,respectively.

    2.2.Microstructure characterization

    The specimens for electron back-scattering diffraction(EBSD) were prepared by electro-polishing with a solution of 10mL perchloric acid and 90mL alcohol,and three specimens of each kinds of samples were used to ensure the reliability of the results.The microstructure evolution of ZN20 alloy processed by ECAP was observed by EBSD.The data were analyzed by Oxford Channel 5 software to obtain the orientation maps,pole figures (PF),inverse pole figures (IPF),recrystallized maps,recrystallized fractions and Schmid factor distributions.Second phases in the alloys were detected by transmission electron microscopy (TEM,TECNAI G20).The specimens for TEM were prepared by ion thinning.

    2.3.Tensile test

    Tensile samples with gage section 15mm in length,6mm in width and 2mm in thickness were tested by using a universal testing machine(ZwickZ050)with a tensile speed of 1mm min-1.Three samples were used to ensure the reliability of the experimental results,and the fracture surface morphology was observed by a scanning electron microscope (SEM Zeiss Supra 55).

    2.4.Immersion test

    Simulated intestinal fluid was chose as the corrosion medium to test corrosion resistance of ZN20 alloy due to the potential application for surgical staples in further study.The immersion test was performed in the simulated intestinal fluid for 14 days at 37 °C with an immersion ratio of 20mL cm-2.The simulated intestinal fluid was prepared according to the United States pharmacopeia,using 0.68g KH2PO4,25mL distill water and 19mL NaOH with concentration of 0.2mol L-1,then pH of the fluid was adjusted to 6.8 by NaOH,and finally distill water was added to make sure the volume of the solution was 100mL.The samples for immersion test were ground by SiC papers to 2000 grids,and three samples were used at each timepoint to ensure the reliability of the results.The simulated intestinal fluid was refreshed every day to simulate the environment in human body.After 3,7 and 14 days,the corrosion product was removed by ultrasonic clean in chromic acid solution (20%Cr2O3+1%AgNO3+2%Ba(NO3)2) for 1min,washed by ethanol and then dried.Corrosion rate was calculated by the following equation:

    whereKis 87,600,Wis the weight loss after the immersion test (g),Ais the superficial area of the sample (cm2),tis the immersion time (h),andDis the density of magnesium alloy(g cm-3).The corrosion morphology was observed by SEM.

    2.5.Electrochemical test

    The samples for electrochemical test were embedded in epoxy resin with a surface in contact with simulated intestinal fluid and then polished with SiC papers to 2000 grid.Potential-dynamic polarization (PD) and Electrochemical Impedance Spectroscopy (EIS) were conducted in simulated intestinal fluid at 37 °C by an electrochemical workstation (Gamry Reference 610,USA) with a classical three electrodes cell which comprised of platinum as auxiliary electrode,saturated calomel electrode as reference electrode and sample as working electrode.PD test was carried out with a scan rate of 0.5mV/s and the scanning potential ranged from-2.1V to -1.2V vs Eref (potential of reference electrode)after the samples were immersed in simulated intestinal fluid for 30min.And EIS test was conducted with a scan frequency ranged from 100kHz to 10 mHz and 10mV root-mean-square perturbation.The corrosion potential (Ecorr) and corrosion current density (Icorr) were calculated according to the Tafel extrapolation method,and EIS spectra were fitted by Gamry Echem Analyst software.

    3.Results

    3.1.Microstructure

    Fig.1 shows EBSD maps and grain size distributions of ZN20 alloy taken on the longitudinal section after extrusion and ECAP.The microstructure of sample E featured a rather heterogeneous microstructure composed of a large number of fine grains smaller than 10μm and some coarse grains of 10-40μm.After 4 passes ECAP at 300 °C,sample E1 featured a completely recrystallized microstructure with an average grain size of 10μm.While after 4 passes ECAP at 350 °C,grain coarsening can be observed on sample E2 due to the recrystallization and a rapid grain growth caused by relatively high temperature and the inter-pass time at this processing temperature.Fig.2 shows SEM images of ZN20 alloy after extrusion and ECAP(samples E,E1 and E2)and the bright-field images of MgZn2phase,Mg60Zn32Nd8phases and corresponding selected area diffraction (SAED) patterns taken on the longitudinal section.Two kinds of second phases mainly existed in ZN20 alloy,strip-like second phase and granular phase,no matter in samples E,E1 or E2.Table 1 is the EDS analysis of ZN20 alloy,in which it can be seen that strip-like phase wasa ternary phase composed of Mg,Zn and Nd,while granular phase was a binary phase composed of Mg and Zn.Besides,the kinds of second phases did not change during ECAP because the EDS results in Table 1 was similar.Therefore,TEM was carried on samples E to identify the second phases in ZN20 alloy.Based on the results in Fig.2 and some studies about Mg-Zn-Nd alloy,it can be identified that the strip-like phase is T phase,and the granular phase is MgZn2[28].The second phase particles in three samples were distributed along the extrusion direction (ED).The area fraction of the second phase particles in samples E,E1 and E2 calculated by Image J are 6.22%,5.45% and 6.29%,respectively,and the amount of second phase particles did not increase after ECAP.

    Table 1 EDS results of the regions marked by white arrows in Fig.2.

    Table 2The value of df,dc,ff and fc of samples E,E1 and E2.

    3.2.Texture evolution

    Fig.3 shows the (0001) pole figures of ZN20 alloy after extrusion and ECAP.The dominant textures in samples E,E1 and E2 exhibited a similar typical extrusion texture,in which(0001) planes were parallel to the ED.The maximum texture intensity decreased from 7.76 to 7.26 and 6.76 after 4 passes ECAP at 300 °C and 350 °C.The distribution of Schmid factor for (0001)<110>basal slip is shown in Fig.4.The value of Schmid factor was improved after 4 passes ECAP at 300 °C and 350 °C,leading to an improvement from 0.30 of sample E to 0.37 and 0.33 of samples E1 and E2,respectively.

    3.3.Mechanical properties

    The tensile stress-strain curves and tensile properties of ZN20 alloy after extrusion and ECAP at room temperature are depicted in Fig.5.Sample E,which was supplied as the original state,exhibited a relatively high ultimate tensile strength (UTS) (240MPa) and yield strength (YS) (210MPa)accompanied by limited ductility.After 4 passes ECAP at 300°C,UTS (240MPa) and YS (213MPa) could be kept at relatively high values.The UTS and YS decreased to 222MPa and 189MPa after the processing temperature was increased to 350 °C.Although the 4 passes ECAP at 300 °C and 350°C could not improve the strength of ZN20 alloy,the ductility was increased obviously.The ductility was increased by 40%after 4 passes ECAP at 300 °C.Fig.6 reveals SEM images of fracture surfaces of samples E,E1 and E2.A large number of dimples and cleavages can be observed on the fracture surface of ZN20 alloy.The number of dimples was increased after ECAP,indicating a better ductility of samples E1 and E2.

    Fig.1.EBSD orientation maps and grain size distribution of samples E (a),E1 (b) and E2 (c) taken on the longitudinal section.

    Fig.2.The distribution of second phase of the samples E (a),E1 (b) and E2 (c) and bright-field images of MgZn2 phases (d) and T phases (e,f) and corresponding SAED pattern.(e) Taken on longitudinal section.

    Fig.3.(0001) pole figures for samples E (a),E1 (b) and E2 (c).

    3.4.Immersion test

    Fig.7 shows the corrosion rates of samples E,E1 and E2 after immersion in simulated intestinal fluid for 14 days at 37°C.The corrosion rates of three different samples had similar variation trend in the 14 days immersion test.The corrosion rate was largest at first,and then decreased as the immersion time prolonged.Similar results have been reported before that the corrosion product formed on the surface of the magnesium alloy at early stage of immersion test could protect the alloy from contacting the simulated intestinal fluid [14,17].A clearly distinction in corrosion rate of three samples can be observed,sample E1 had the lowest corrosion rate compared with samples E and E2.The corrosion resistances of three samples decreased as follows: E1,E2 and E.

    Fig.4.Distributions of Schmid factor for (0001) <110>basal slip of samples E (a),E1 (b) and E2 (c).

    Fig.5.Engineering tensile stress-strain curves (a) and tensile properties (b) of samples E,E1 and E2 at room temperature.

    Fig.6.Fracture morphologies of samples E,E1 and E2 taken by SEM after tensile test.

    Fig.8 depicts the corrosion morphologies of samples E,E1 and E2 after immersion in simulated intestinal fluid for 14 days after removing the corrosion product by chromic acid.For sample E,the formation of large holes as a consequence of corrosion pits can be observed and the corrosion pits nearly cover the sample surface totally (Fig.8a2).While the local surface of samples E1 and E2 were still in good condition after immersion for 14 days.The corrosion pits on sample E2 were larger and deeper than those on sample E1,illustrating that the corrosion resistance of sample E1 was better than that of sample E2.

    3.5.Electrochemcial test

    Polarization curves,EIS Nyquist plots,equivalent circuit of samples E,E1 and E2 and fitting results of PD and EIS curves are shown in Fig.9.The corrosion potential of ZN20 alloy became more positive and the corrosion current density decreased after ECAP.Samples E1 has highest corrosion potential and lowest current density,which illustrates it has the best corrosion resistance.The Nyquist plots acquired in Fig.9b show two capacitance loop at high and intermediate frequencies and an inductance loop at low frequency.The dimension of Nyquist plots measured on E1 samples was the highest,indicating it has the best corrosion resistance.The corresponding equivalent circuit was shown in Fig.9 to illustrate the corrosion mechanism of ZN20 alloy in simulated intestinal fluid.Rsis the resistance of simulated intestinal fluid.The capacitance loop at high frequency is owing to the characteristics of electric double layer formed at between surface of ZN20 alloy and the electrolyte,which can be described by charge transfer resistance (Rct) and electric double-layer capacity (Qdl).And the capacitance loop at intermediate frequency is related to the existence of corrosion product layer,which can be described by the corrosion product layer resistance (Rf) and capacity (Qf).The inductance loop at low frequency is related to initiation of the corrosion process[30-33].The fitting results of EIS curves are shown in Fig.9d,the resistance of the corrosion system (Rp) can be calculated as follows:

    Fig.7.Corrosion rate of samples E,E1 and E2 after immersion in simulated intestinal fluid for 14 days at 37 °C.

    The value of Rpcan represents the corrosion resistance.Therefore,it can be deduced that the corrosion resistance decreased as follows: E1,E2 and E,which was consistent with the results of immersion test.

    4.Discussion

    4.1.Microstructure evolution

    The microstructure of as-extruded ZN20 alloy transformed from bimodal-grained structure to a relatively homogenous bimodal-grained structure after 4 passes ECAP at 300 °C,but the difference between coarse grains and fine grains was not as obvious as that in sample E.Although the microstructure of sample E2 remained the characteristic of bimodalgrained structure,grain growth could be observed after raising the processing temperature to 350 °C.This is contradictory to the conclusion in some literatures that ECAP made fine grains finer and coarse grains coarser [21,22].This should be mainly caused by the different original state of the materials.In this study,ECAP was performed on the extruded ZN20 alloy,and the extrusion was carried out at low temperature and high extrusion ratio.Therefore,there were lots of substructure grains in the as-extruded ZN20 alloy.Fig.10 is the recrystallized maps and recrystallized fractions of samples E,E1 and E2.The substructure in sample E was the most among three samples,and the recrystallized structure and deformed structure were increased obviously after ECAP.ECAP at lower temperature,which is beneficial for dynamic recrystallization and dynamic recovery,so the grains in sample E1 were fine and uniform.While it could cause grain coarsen when the processing temperature was 350 °C,it was induced by the relatively high temperature and the long inter-pass time at this processing temperature.

    Fig.8.Corrosion morphologies (1) and magnified images (2) of samples E (a),E1 (b) and E2 (c) after immersion in simulated intestinal fluid for 14 days with removal of corrosion product by chromic acid.

    Fig.9.Polarization curves (a),EIS Nyquist plots (b),equivalent circuit (c) of samples E,E1 and E2 and fitting results of PD and EIS curves (d).

    Fig.10.Recrystallized maps of samples E (a),E1 (b) and E2 (c) and recrystallized fractions (d).

    The second phase particles in three samples were distributed along ED.According to the mechanism of particle stimulating nucleation [34],a high stress zone can be formed around the hard particles during ECAP,which accelerates the DRX process and promotes the grain refinement.Sample E was extruded at low temperature and high extrusion ratio,so lots of second phase would precipitate along ED.Moreover,the number of second phases did not increase after ECAP because the alloying content was finite.

    The dominant textures in three samples exhibited a typical extrusion texture,basal plane paralleled to ED,while the texture intensity decreased after ECAP.The decrease of texture intensity was mainly caused by dynamic recrystallization occurring during ECAP.The specimen was rotated 90°around the ED after every pass,which resulted in a rotation of strain path around the ED during the processing of ECAP,so the texture was slightly rotated around ED (Fig.3).Jin et.al found there is a critical grain size (17μm) that will cause different Hall-Petch relation [35].Therefore,the microstructures of these three different samples were separated into coarse and fine grains to further clarify the role of bimodalgrained structure on mechanical properties.Coarse grains can be defined as those the diameter is larger than the critical grain size(>17μm),and fine grains corresponds to ones with finer grain size (<17μm).Fig.11 shows the EBSD orientation maps and pole figures (PF) of the coarse and fine grains,respectively.The basal plane of most grains was parallel to ED,except for the dominant texture of the coarse grains in sample E2,for which the basal planes were parallel to transverse direction(TD).The texture intensity of the coarse grains in sample E is 15.33,much higher than that (9.42) in sample E1,while the texture intensity of fine grains in sample E is the lowest (4.80).The texture intensity of coarse grains and fine grains in samples E1 and E2 are much closer compared with that in sample E.The bimodal-grained structure of sample E was composed of coarse grains with strong texture and fine grains with random texture.After ECAP,the characteristics of the bimodal-grained structure were retained,but the strong texture of the coarse grains was weakened,and the texture intensity of the fine grains was increased.

    4.2.Strength mechanism in bimodal-grained structure ZN20 alloy

    The strength did not change too much after 4-passes ECAP at 300 °C,while it decreased slightly when the temperature of ECAP was increased to 350 °C.Grain boundary strengthening,precipitates strengthening and solid solution strengthening are three main strengthening mechanisms in extruded and ECAPed ZN20 alloy.The contributions of these three strengthening mechanisms on the strength of the alloy were calculated based on the characteristics of microstructure and second phase distribution,interactions of alloying elements.

    Fig.11.EBSD orientation maps (a,b) and PF (c,d) of coarse grains (a,c) and fine grains (b,d) in samples E (1),E1 (2) and E2 (3).

    4.2.1.Grain boundary strengthening

    The grain boundary strengthening can be calculated by Hall-Petch relation,and there is a liner relation between the strength of the alloy and the grain size.The contribution of grain boundary strengthening on yield strength can by analyzed according to Hall-Petch relation as follows:

    whereσyis the yield stress,σ0is the friction stress when dislocations glide on the slip plane,k is a constant that depends on texture,grain size,temperature and strain,d is the average grain size.Jin et al.studied the Hall-Petch relation and strengthening mechanism of bimodal grained AZ31 alloy with an average grain size of 6-42μm [35].They found that there was a critical grain size (17μm) will cause different Hall-Petch relation which has different value ofσ0and k.σ0is related to the ratio between the resolved shear stress(CRSS) of non-basal slip and that of basal slip.And the ratio between CRSS of basal slip and CRSS of basal slip will decrease as the grain size increase because the influence of grain boundary strengthening on basal system is more potent than that on non-basal system [36].The value of k is related to the variation of deformation mode,and it is proportional to the CRSS of deformation mode.Generally,twinning is main deformation mode in the samples with coarse grains,while basal slip is dominate in the samples with fine grains [37].Therefore,σ0in coarse grains is lower than that in fine grains,while k in coarse grains is higher than that in fine grains.The accurate values ofσ0and k in the equation needs to determine in the further work,because they will be different for different kinds of alloy.And the contribution of grain boundary strengthening on the strength (σgs) in bimodal grainedstructure samples can be expressed as follows:

    whereσf,kfanddfare the friction stress,constant and grain size of fine grains,σc,kcanddcare the friction stress,constant and grain size of coarse grains,ffandfcare the volume fraction of fine grains and coarse grains.Table 2 is the value ofdf,dc,ffandfcof three samples,which were calculated by Channel 5.Although the Hall-Petch relation between coarse grains and fine grains is different,the strength is always inversely proportional to the grain size.And the contribution of fine grains to the strength is larger than that of coarse grains.Therefore,σgsof samples Ex with finer grains and larger volume fraction of fine grains was highest,whileσgsof samples E2 with coarser grains and smaller volume fraction was lowest.

    4.2.2.Precipitates strengthening

    The strength of magnesium alloy can be improved effectively because the existence of second phase can inhibit the motion of dislocation.Orowan strengthening mechanism can illustrate the influence of second phase on inhibiting the motion of dislocation.Accordingly,the contribution of precipitates strengthening(σps)on strength can be written as follows:

    where M is Taylor factor with a range of 2.1-2.5.G is shear modulus (1.66 × 104MPa),b is burgers vector(3.2× 10-10m),v is Poisson ration (0.35),dpand f are the average size and volume fraction of second phase.The value ofdpand f were listed in Table 2.Substituting the data above into Eq.(3),σpsof samples E,E1 and E2 were 8.07,7.17 and 8.34MPa,respectively.

    4.2.3.Solid solution strengthening

    Solid strengthening was caused by the inhibition of solute atoms to dislocation glide.According to Deruyttere and Gypen theoretical,the contribution of solid solution strengthening (σss) on the strength can be calculated as follows:

    where k and C represents the solution strengthening constant and atom fraction,n is constant and usually treated as 1/3 or 2/3.In this study,n is determined as 2/3,kZnandkNdare 905 and 813MPa (at%)-2/3,CZnandCNdare 1.84% and 0.52%.Substituting the data above into Eq.(4),σssof samples E,E1 and E2 were 72.82MPa.

    Based on the results above,the yield strength (σy) of samples E,E1 and E2 can be calculated as follows:

    The yield strength of samples E,E1 and E2 decreased as follows: E,E1 and E2,which was similar with the trend of experiment results.Besides,it can be deduced that grain boundary strengthening and solid solution strengthening were dominant strengthening mechanism.The contribution of precipitates strengthening on the strength was negligible due less second phase in the alloy.

    4.3.Role of bimodal-grained structure on ductility

    The texture of fine grains in the bimodal-grained structure of samples E,E1 and E2 were random,but the coarse grains with strong texture in sample E was weakened after ECAP.Fine grains can coordinate the deformation by providing more grains,and has a positive influence on ductility.However,the effect of the coarse grains in bimodal grained structure on ductility should be much more complicated,lying in two aspects.Firstly,the coarse grains have negative influence on the ductility because the number of grains that participates in deformation decrease.Secondly,the texture intensity can decide the difficulty of basal slip as the loading direction is parallel to the ED,and can also affect the generation of twins during the deformation indirectly.Therefore,the effect of coarse grains in bimodal-grained structure on the mechanical properties needs to be discussed in details.

    Basal slip and twinning are the main deformation modes for magnesium alloys at room temperature due to their low CRSS.The type of twinning during deformation is mainly related to the relationship between thec-axis and loading direction.Tension twins are produced when the sample is stretched along thec-axis,but only contraction twins are produced when compressed along thec-axis.Moreover,tension twins more easily occur,because their CRSS is much lower than that of contraction twins.Such a phenomenon was also found by Wei [24] that tension twins were formed during tensile test firstly.In terms of bimodal-grained structure composed of coarse grains with strong texture and fine grains with random texture,basal slips in the fine grains can be more easily activated than the twinning due to the random texture of fine grains.It makes the fine grains are prior to undertake the deformation by basal slips instead of twinning.But when the basal slips in the fine grains cannot satisfy the deformation processing,twinning will occur in coarse grains because basal slip is difficult to act under the influence of strong texture.Therefore,tension twinning is more likely to appear in sample E due to the stronger texture intensity,and finally cause the lowest ductility among three samples by providing the crack nucleation.After ECAP,the strong texture in coarse grains was weakened,and twinning did not appear as early as those in samples E.Therefore,the ductility was improved after ECAP.But it still caused a different performance in ductility for samples E1 and E2 due to different grain size.The ductility of samples E1 with finer grains and higher volume fraction of fine grains is better than samples E2 with coarser grains and higher volume fraction of coarse grains.

    4.4.Role of bimodal-grained structure on corrosion resistance

    Magnesium oxide is easily formed on the surface of magnesium alloy because of the much lower chemical potential of MgO than Mg.The cubic magnesium oxide will transform into the hexagonal magnesium hydroxide as it contacts the corrosion medium.The compressive stress,which can cause the breakage of corrosion product layer,will generate between the corrosion product layer and the oxide layer [38].Fine grains can stabilize the corrosion product layer by increasing the grain boundary and releasing the compressive stress between the corrosion product layer and oxide layer,and improve the corrosion resistance.Besides the grain size,texture also have their own influence on the corrosion resistance of magnesium alloy.It has been reported that the surface energies of basal plane (0001),prismatic plane(100)and pyramidal plane(110)of magnesium are 1.54×104J mol-1,3.04×104J mol-1and 2.99×104J mol-1,respectively [39].Lower surface energy means that the diffusion rate of magnesium atoms is slow.Therefore,the corrosion resistance should decrease as follows: basal plane,pyramidal plane and prismatic plane.

    The role of bimodal-grained structure on corrosion resistance of magnesium alloy depends on two aspects,grain size and texture.As for samples E,the coarse grains would cause the corrosion product layer unstable,firstly.Then,the strong basal texture in coarse grains parallel to ED also had a negative influence on the corrosion resistance.Because the sample in immersion test was cut along the cross section,which would cause many non-basal plane contacting simulated intestinal fluid,finally cause the worst corrosion resistance of sample E.Therefore,some deep corrosion pits can be observed in Fig.8.After ECAP,the basal texture intensity was weakened,so the corrosion resistance of samples E1 and E2 were improved.Besides,the coarse grains in sample E1 were much finer than those in sample E (Table 2),so the corrosion resistance was the best after 4 passes ECAP at 300 °C.And some places were still in good condition on the surface of sample E1 after immersion test (Fig.8b2).The basal plane in coarse grains in samples E2 was parallel to TD,which would have a positive influence on the corrosion resistance.But the grain size in samples E2 was larger than that in samples E1,and the negative influence of coarse grains suppressed the positive influence of texture,finally causing a decrease of the corrosion resistance after increasing the processing temperature from 300 °C to 350 °C.

    5.Conclusions

    Extrusion and ECAP were performed on the ZN20 alloy to obtain a bimodal-grained structure and the effect of such structure on mechanical property and corrosion resistance was investigated.The conclusions can be summarized as follows:

    1.A bimodal-grained structure ZN20 alloy can be obtained by extrusion at low temperature and high extrusion ratio.The coarse grains in such bimodal-grained structure can be refined to 10μm on average after 4 passes ECAP at 300°C.

    2.The coarse grains in sample E exhibits strong basal texture,while fine grains exhibit a relatively random texture.Such strong basal texture of coarse grains can be weakened from 15.33 to 9.42 and 8.15 after ECAP for samples E1 and E2,respectively.

    3.The grain refinement and texture weakening can lead to an improvement of strength and ductility.Grain boundary strengthening and solid solution strengthening were dominant strengthening mechanism.The texture weakening in fine grains after ECAP has a positive influence on the ductility.

    4.The corrosion resistance can be improved after ECAP,and it was the best after 4 passes ECAP at 300 °C.Grain refinement and basal plane have a positive role on the corrosion resistance.Although the basal plane is parallel to ED no matter for ZN20 alloy after extrusion or ECAP,texture weakening can also lead to an improvement of corrosion resistance after ECAP.

    Declaration of Competing Interest

    None.

    Acknowledgment

    This work was financially supported by the National Key Research and Development Program of China(No.2016YFC1101804,2016YFC1100604),Natural Science Foundation of Liaoning Province of China (No.2019-MS-326),Youth Innovation Promotion Association,CAS and National Natural Science Foundation of China (No.51971222,51801220).

    成年女人看的毛片在线观看| 日韩制服骚丝袜av| 色播亚洲综合网| 久99久视频精品免费| 99久久人妻综合| 久久久欧美国产精品| 午夜福利在线观看免费完整高清在| 婷婷六月久久综合丁香| 嫩草影院入口| 高清毛片免费看| 日本熟妇午夜| 最新中文字幕久久久久| 日韩强制内射视频| 国产成人aa在线观看| 国产免费又黄又爽又色| 午夜福利在线观看免费完整高清在| 亚洲av男天堂| videossex国产| 内地一区二区视频在线| 少妇熟女aⅴ在线视频| 午夜日本视频在线| 青青草视频在线视频观看| 在线免费观看不下载黄p国产| 午夜精品一区二区三区免费看| 亚洲色图av天堂| 五月伊人婷婷丁香| 能在线免费看毛片的网站| 亚洲美女搞黄在线观看| 色网站视频免费| 成人国产麻豆网| 国产黄色小视频在线观看| 国产视频内射| 亚洲欧美日韩东京热| 欧美日本亚洲视频在线播放| 18禁在线播放成人免费| 中文字幕亚洲精品专区| .国产精品久久| 3wmmmm亚洲av在线观看| 欧美xxxx黑人xx丫x性爽| 亚洲不卡免费看| 国产精品.久久久| 少妇人妻一区二区三区视频| 亚洲aⅴ乱码一区二区在线播放| 成人鲁丝片一二三区免费| 日韩成人伦理影院| 26uuu在线亚洲综合色| 搡老妇女老女人老熟妇| 直男gayav资源| 亚洲成色77777| 免费播放大片免费观看视频在线观看 | 国产女主播在线喷水免费视频网站 | 少妇的逼好多水| 免费观看的影片在线观看| 日韩欧美国产在线观看| 小说图片视频综合网站| 亚洲av福利一区| 久久国内精品自在自线图片| 日韩一区二区视频免费看| 精品一区二区三区人妻视频| 日韩强制内射视频| 中文字幕制服av| 黄色配什么色好看| 精品国产三级普通话版| 欧美激情在线99| 成人鲁丝片一二三区免费| 国产成人精品婷婷| 免费在线观看成人毛片| 高清视频免费观看一区二区 | 偷拍熟女少妇极品色| 久久久久性生活片| 欧美+日韩+精品| 欧美日本亚洲视频在线播放| 深爱激情五月婷婷| 18禁动态无遮挡网站| 久久久久国产网址| 国产不卡一卡二| 日韩av在线大香蕉| 亚洲精品乱码久久久v下载方式| 三级经典国产精品| 亚洲av免费在线观看| 毛片女人毛片| 日韩欧美在线乱码| 少妇人妻一区二区三区视频| 最后的刺客免费高清国语| 国产在视频线在精品| 美女脱内裤让男人舔精品视频| 99热网站在线观看| 麻豆成人午夜福利视频| 国产午夜精品论理片| 91aial.com中文字幕在线观看| 一级毛片久久久久久久久女| 久久久久久久国产电影| 国产精品久久久久久久电影| 国产亚洲最大av| 少妇熟女欧美另类| 国产探花极品一区二区| av免费在线看不卡| 最近的中文字幕免费完整| 国产成人午夜福利电影在线观看| 哪个播放器可以免费观看大片| 久久99热这里只频精品6学生 | 午夜福利在线在线| 日日干狠狠操夜夜爽| 99热这里只有精品一区| 亚洲中文字幕一区二区三区有码在线看| 精品午夜福利在线看| 久久久国产成人免费| 国产精品野战在线观看| 91av网一区二区| 99久久无色码亚洲精品果冻| 欧美一级a爱片免费观看看| 日本免费一区二区三区高清不卡| 国产精品女同一区二区软件| 亚洲精品456在线播放app| 国产白丝娇喘喷水9色精品| 久久久成人免费电影| 亚洲综合精品二区| 欧美高清成人免费视频www| 亚洲真实伦在线观看| 岛国在线免费视频观看| 国产日韩欧美在线精品| 汤姆久久久久久久影院中文字幕 | 一区二区三区乱码不卡18| av在线老鸭窝| 国产亚洲5aaaaa淫片| 国产黄片视频在线免费观看| 精品久久久噜噜| 91午夜精品亚洲一区二区三区| 国产高清国产精品国产三级 | 国产一区亚洲一区在线观看| 一级黄片播放器| 欧美激情国产日韩精品一区| 免费不卡的大黄色大毛片视频在线观看 | 熟女人妻精品中文字幕| 人人妻人人看人人澡| 国产真实伦视频高清在线观看| 欧美zozozo另类| 国产 一区 欧美 日韩| 亚洲国产高清在线一区二区三| 久久精品影院6| a级毛色黄片| 日韩,欧美,国产一区二区三区 | 欧美变态另类bdsm刘玥| 男人舔女人下体高潮全视频| 乱系列少妇在线播放| 中国美白少妇内射xxxbb| 欧美bdsm另类| 亚洲欧美中文字幕日韩二区| 少妇高潮的动态图| 国国产精品蜜臀av免费| 欧美成人午夜免费资源| 日韩人妻高清精品专区| 99久久无色码亚洲精品果冻| 中文字幕av在线有码专区| 亚洲欧美精品专区久久| 男人的好看免费观看在线视频| 麻豆一二三区av精品| 国产真实伦视频高清在线观看| 精品久久久久久久末码| 91狼人影院| 日本wwww免费看| 男人和女人高潮做爰伦理| 亚洲无线观看免费| 国产精品国产三级国产av玫瑰| 亚洲欧美中文字幕日韩二区| 亚洲成色77777| 国产成人福利小说| 色尼玛亚洲综合影院| 边亲边吃奶的免费视频| 一二三四中文在线观看免费高清| av专区在线播放| 亚洲精品成人久久久久久| 免费观看的影片在线观看| 欧美高清成人免费视频www| 成人国产麻豆网| 国产老妇伦熟女老妇高清| 亚洲国产日韩欧美精品在线观看| 日日撸夜夜添| 一级av片app| 欧美日韩一区二区视频在线观看视频在线 | 亚洲无线观看免费| 国产男人的电影天堂91| 久久精品久久久久久久性| av福利片在线观看| 成人漫画全彩无遮挡| 高清毛片免费看| 亚洲精品aⅴ在线观看| 一级毛片久久久久久久久女| 啦啦啦韩国在线观看视频| 日本色播在线视频| av女优亚洲男人天堂| 伊人久久精品亚洲午夜| 精品久久国产蜜桃| 在线播放国产精品三级| 亚洲乱码一区二区免费版| 亚洲五月天丁香| 波多野结衣巨乳人妻| 国内揄拍国产精品人妻在线| 午夜激情欧美在线| 99久久九九国产精品国产免费| 长腿黑丝高跟| 国产在视频线在精品| 午夜福利在线在线| 精品一区二区三区视频在线| 亚洲av二区三区四区| 亚洲av福利一区| 干丝袜人妻中文字幕| 在线天堂最新版资源| 最近视频中文字幕2019在线8| 国产久久久一区二区三区| 男的添女的下面高潮视频| 日韩av在线大香蕉| 国产精品不卡视频一区二区| 亚洲精品色激情综合| 成人鲁丝片一二三区免费| 日本黄色视频三级网站网址| 深爱激情五月婷婷| 国产激情偷乱视频一区二区| 一本—道久久a久久精品蜜桃钙片 精品乱码久久久久久99久播 | 听说在线观看完整版免费高清| av黄色大香蕉| 深夜a级毛片| 在现免费观看毛片| 小说图片视频综合网站| 女人十人毛片免费观看3o分钟| 啦啦啦观看免费观看视频高清| 婷婷色综合大香蕉| 国产真实乱freesex| 九草在线视频观看| 日本猛色少妇xxxxx猛交久久| 国产精品蜜桃在线观看| 国产精品国产三级专区第一集| 能在线免费看毛片的网站| 日日摸夜夜添夜夜添av毛片| 精品久久久久久久久av| 亚洲天堂国产精品一区在线| 欧美日韩精品成人综合77777| 久久久国产成人免费| 免费无遮挡裸体视频| 久久久精品94久久精品| 欧美97在线视频| 黄片wwwwww| 日韩 亚洲 欧美在线| 夫妻性生交免费视频一级片| 岛国在线免费视频观看| 高清视频免费观看一区二区 | 国产精品一区www在线观看| 国语自产精品视频在线第100页| 男女国产视频网站| 免费人成在线观看视频色| 亚洲欧洲国产日韩| 婷婷色av中文字幕| 亚洲av中文av极速乱| 亚洲综合精品二区| 夫妻性生交免费视频一级片| 欧美zozozo另类| 国产精品人妻久久久久久| 久久久久久久久久黄片| 99久久成人亚洲精品观看| 国产精品福利在线免费观看| 少妇人妻精品综合一区二区| 久久精品91蜜桃| av视频在线观看入口| 秋霞伦理黄片| 国产av不卡久久| 精品久久久久久成人av| 亚洲精品成人久久久久久| 午夜激情欧美在线| 日本免费一区二区三区高清不卡| 国产片特级美女逼逼视频| 亚洲色图av天堂| av在线天堂中文字幕| 亚洲在线观看片| 男女下面进入的视频免费午夜| 国产精品国产三级国产专区5o | 成人鲁丝片一二三区免费| 欧美精品一区二区大全| 久久国内精品自在自线图片| 精品国产露脸久久av麻豆 | 2021少妇久久久久久久久久久| 免费看光身美女| 91久久精品国产一区二区三区| 国产成人精品一,二区| 26uuu在线亚洲综合色| 国产视频内射| 日日啪夜夜撸| 亚洲成人久久爱视频| 国产av码专区亚洲av| 精品免费久久久久久久清纯| 熟妇人妻久久中文字幕3abv| 美女xxoo啪啪120秒动态图| 欧美97在线视频| 久久久久久伊人网av| 亚洲av不卡在线观看| 久久欧美精品欧美久久欧美| 最近2019中文字幕mv第一页| 永久免费av网站大全| av国产久精品久网站免费入址| 内射极品少妇av片p| 淫秽高清视频在线观看| 成人午夜精彩视频在线观看| 国产成年人精品一区二区| 成年av动漫网址| 亚洲成人精品中文字幕电影| 韩国av在线不卡| 男的添女的下面高潮视频| 一夜夜www| 亚洲国产精品国产精品| 久久亚洲精品不卡| 日本黄色片子视频| av.在线天堂| 少妇裸体淫交视频免费看高清| 小蜜桃在线观看免费完整版高清| 色综合站精品国产| 少妇的逼水好多| 亚洲18禁久久av| 亚洲天堂国产精品一区在线| 99久久中文字幕三级久久日本| 欧美成人午夜免费资源| 99久久精品热视频| 日本三级黄在线观看| 婷婷色综合大香蕉| 欧美极品一区二区三区四区| 少妇丰满av| 啦啦啦啦在线视频资源| 亚洲自拍偷在线| 午夜激情福利司机影院| 亚洲激情五月婷婷啪啪| 国产精品美女特级片免费视频播放器| 男女啪啪激烈高潮av片| 国产精品美女特级片免费视频播放器| 日韩一本色道免费dvd| 日本欧美国产在线视频| 国产极品精品免费视频能看的| 丰满少妇做爰视频| 亚洲中文字幕日韩| 亚洲四区av| 精品国产一区二区三区久久久樱花 | 欧美成人午夜免费资源| 亚洲怡红院男人天堂| 中文字幕免费在线视频6| 免费观看a级毛片全部| 超碰97精品在线观看| 免费看a级黄色片| 国产乱来视频区| 中文字幕av成人在线电影| 亚洲国产精品成人久久小说| 91午夜精品亚洲一区二区三区| 国产人妻一区二区三区在| 国产精品一区二区性色av| 大香蕉97超碰在线| 午夜福利网站1000一区二区三区| 乱系列少妇在线播放| ponron亚洲| 国产人妻一区二区三区在| 午夜福利网站1000一区二区三区| 熟女人妻精品中文字幕| 久久久午夜欧美精品| 国产中年淑女户外野战色| 日韩精品青青久久久久久| 国产美女午夜福利| 日日啪夜夜撸| 成人二区视频| 久久久久精品久久久久真实原创| 久久久久久久久久久丰满| 色噜噜av男人的天堂激情| 成人亚洲精品av一区二区| 久久国产乱子免费精品| 国产精品久久久久久久久免| 97人妻精品一区二区三区麻豆| 久久精品久久久久久久性| 日本与韩国留学比较| 99热全是精品| 神马国产精品三级电影在线观看| 免费看av在线观看网站| 久久精品国产自在天天线| 一卡2卡三卡四卡精品乱码亚洲| 91av网一区二区| 晚上一个人看的免费电影| 精品久久久久久久久亚洲| 午夜福利成人在线免费观看| 精品一区二区免费观看| 夜夜爽夜夜爽视频| 国产精品日韩av在线免费观看| 国产精品野战在线观看| 综合色av麻豆| 麻豆成人av视频| 久久综合国产亚洲精品| 国产精品99久久久久久久久| 91久久精品国产一区二区成人| 亚洲国产精品合色在线| av国产久精品久网站免费入址| 国产老妇女一区| 亚洲综合精品二区| 国产高潮美女av| 欧美xxxx性猛交bbbb| 天天躁夜夜躁狠狠久久av| 国产中年淑女户外野战色| 国产亚洲5aaaaa淫片| 干丝袜人妻中文字幕| av国产免费在线观看| 欧美极品一区二区三区四区| 国产成人免费观看mmmm| 亚洲精品一区蜜桃| 国产精品一区二区三区四区久久| 久久这里有精品视频免费| 久久精品综合一区二区三区| 亚洲性久久影院| 搡老妇女老女人老熟妇| av福利片在线观看| 久久久色成人| 亚洲精品自拍成人| 嘟嘟电影网在线观看| 欧美日韩精品成人综合77777| 亚洲国产成人一精品久久久| 久久婷婷人人爽人人干人人爱| 老司机福利观看| 国内揄拍国产精品人妻在线| 男女那种视频在线观看| 一级毛片电影观看 | 床上黄色一级片| 久久久久久久久中文| 舔av片在线| 高清视频免费观看一区二区 | 亚洲图色成人| 亚洲精品色激情综合| 亚洲丝袜综合中文字幕| 99九九线精品视频在线观看视频| 国产精品国产高清国产av| av国产久精品久网站免费入址| 日本黄色视频三级网站网址| 国产麻豆成人av免费视频| 男人舔奶头视频| 国产亚洲一区二区精品| 看非洲黑人一级黄片| 亚洲精品乱码久久久v下载方式| 国产精品久久久久久精品电影| 久久人妻av系列| 亚洲自偷自拍三级| 国产色婷婷99| 丰满乱子伦码专区| 中国美白少妇内射xxxbb| 免费看美女性在线毛片视频| 久久鲁丝午夜福利片| 18禁在线无遮挡免费观看视频| 插逼视频在线观看| 人妻少妇偷人精品九色| 人妻夜夜爽99麻豆av| 久久久久网色| 亚洲精品乱码久久久久久按摩| 免费黄色在线免费观看| 深夜a级毛片| 亚洲久久久久久中文字幕| 美女国产视频在线观看| 国产日韩欧美在线精品| 91久久精品国产一区二区三区| 国产午夜精品论理片| 岛国在线免费视频观看| 美女脱内裤让男人舔精品视频| 亚洲av免费高清在线观看| 精品人妻偷拍中文字幕| 国产单亲对白刺激| 精品一区二区免费观看| 国产淫语在线视频| 99九九线精品视频在线观看视频| 国产白丝娇喘喷水9色精品| 18禁裸乳无遮挡免费网站照片| 我的老师免费观看完整版| 精品人妻熟女av久视频| 日本午夜av视频| 直男gayav资源| 国产一区亚洲一区在线观看| 日韩在线高清观看一区二区三区| 国产精品女同一区二区软件| 久久热精品热| 久久精品久久久久久久性| 日韩精品有码人妻一区| 又黄又爽又刺激的免费视频.| 精品久久久久久久久av| 久久久久免费精品人妻一区二区| 女人十人毛片免费观看3o分钟| 小说图片视频综合网站| 1024手机看黄色片| 亚洲精品久久久久久婷婷小说 | 成人亚洲欧美一区二区av| 毛片女人毛片| 亚洲精品久久久久久婷婷小说 | 亚洲自拍偷在线| 国产av一区在线观看免费| 精品久久国产蜜桃| 亚洲国产精品合色在线| 毛片女人毛片| 国产午夜精品久久久久久一区二区三区| 蜜桃久久精品国产亚洲av| 爱豆传媒免费全集在线观看| 亚洲无线观看免费| 性色avwww在线观看| 91午夜精品亚洲一区二区三区| 亚洲国产成人一精品久久久| 亚洲av成人av| 国产精品99久久久久久久久| 日本一二三区视频观看| 国产三级在线视频| 老师上课跳d突然被开到最大视频| 丰满乱子伦码专区| 国语自产精品视频在线第100页| 麻豆成人午夜福利视频| eeuss影院久久| 国产成人精品一,二区| 深爱激情五月婷婷| 你懂的网址亚洲精品在线观看 | 亚洲av成人精品一二三区| 青春草视频在线免费观看| 天美传媒精品一区二区| 欧美日韩一区二区视频在线观看视频在线 | 五月伊人婷婷丁香| 夜夜爽夜夜爽视频| 91在线精品国自产拍蜜月| 国产免费福利视频在线观看| 桃色一区二区三区在线观看| 色吧在线观看| 色5月婷婷丁香| 一本久久精品| 中文欧美无线码| 十八禁国产超污无遮挡网站| 偷拍熟女少妇极品色| 插逼视频在线观看| 成年免费大片在线观看| 精品久久久久久电影网 | 少妇猛男粗大的猛烈进出视频 | 天堂中文最新版在线下载 | 一区二区三区四区激情视频| 国产精品一区二区性色av| 91精品国产九色| 国产亚洲91精品色在线| 少妇熟女aⅴ在线视频| 老司机影院成人| 国产精品无大码| 99热这里只有是精品50| 久久99热这里只频精品6学生 | 亚洲国产最新在线播放| 波多野结衣高清无吗| 高清在线视频一区二区三区 | 国产淫语在线视频| 丝袜美腿在线中文| 久久久亚洲精品成人影院| 国产久久久一区二区三区| 男女国产视频网站| 精品不卡国产一区二区三区| 久久人人爽人人片av| 久久久久久伊人网av| 久久久久免费精品人妻一区二区| 美女cb高潮喷水在线观看| 亚洲欧美日韩无卡精品| 成人综合一区亚洲| 国产免费视频播放在线视频 | 最近视频中文字幕2019在线8| 美女脱内裤让男人舔精品视频| 国产亚洲一区二区精品| 亚洲18禁久久av| 欧美激情久久久久久爽电影| 日韩 亚洲 欧美在线| 色综合亚洲欧美另类图片| 中文资源天堂在线| 大香蕉97超碰在线| 婷婷色综合大香蕉| 成人午夜精彩视频在线观看| av国产久精品久网站免费入址| 亚洲真实伦在线观看| 国产一区有黄有色的免费视频 | 亚洲美女视频黄频| kizo精华| 大香蕉97超碰在线| 黄片wwwwww| 中文字幕av在线有码专区| 一区二区三区乱码不卡18| 亚洲欧美日韩无卡精品| 免费人成在线观看视频色| 亚洲精品影视一区二区三区av| 蜜臀久久99精品久久宅男| 男女那种视频在线观看| 久久6这里有精品| 两个人的视频大全免费| 久久精品国产亚洲av天美| 国产精品精品国产色婷婷| 日本黄大片高清| 免费黄网站久久成人精品| 亚洲欧洲日产国产| 美女脱内裤让男人舔精品视频| 男人狂女人下面高潮的视频| 精品久久国产蜜桃| 最近中文字幕2019免费版| 国产淫片久久久久久久久| 男的添女的下面高潮视频| 国产av一区在线观看免费| 免费观看人在逋| 国内精品美女久久久久久| 蜜桃久久精品国产亚洲av| 最近视频中文字幕2019在线8| 国产熟女欧美一区二区| 国产精品蜜桃在线观看| 亚洲精品国产成人久久av| 久久精品91蜜桃| 99热这里只有精品一区| av在线天堂中文字幕| 成人毛片60女人毛片免费| 色尼玛亚洲综合影院| 少妇裸体淫交视频免费看高清| 男的添女的下面高潮视频| 级片在线观看| 国产高清有码在线观看视频| 男人舔奶头视频| 欧美一级a爱片免费观看看| 六月丁香七月| 精品人妻视频免费看|