    Microstructure,mechanical properties and wear resistance of Ti particles reinforced AZ31 magnesium matrix composites

    2022-10-25 09:29:10JunliuYeXinhuChenHunLuoJieZhoJinboLiJunTnHongYngBoFengKihongZhengFushengPn
    Journal of Magnesium and Alloys 2022年8期

    Junliu Ye ,Xinhu Chen,b,? ,Hun Luo ,Jie Zho ,Jinbo Li,b,? ,Jun Tn ,Hong Yng,Bo Feng,Kihong Zheng,Fusheng Pn,b,?

    a College of Materials Science and Engineering,Chongqing University,Chongqing 400045,China

    b National Engineering Research Center for Magnesium Alloys,Chongqing University,Chongqing 400045,China

    c Institute of New Materials,Guangdong Academy of Sciences,Guangzhou 510650,China

    Abstract The compromise between strength and plasticity has greatly limited the potential application of particles reinforced magnesium matrix composites (MMCs).In this work,the Ti particles reinforced AZ31 magnesium (Mg) matrix composites achieved simultaneous improvement in strength,elongation and wear resistance.The Ti particles reinforced AZ31 composites were fabricated by ultrasonic-assisted stir casting with hot extrusion.The results showed that a strong interfacial bonding was obtained at Ti/Mg interface because of the formation of semicoherent orientation relationship of TiAl/Mg,TiAl/Al2Ti and Al2Ti/Mg interfaces.The as-extruded 6 wt.%Ti/AZ31 composite presented the best compressive mechanical properties and wear resistance with ultimate tensile strength,elongation and wear rate of 327 MPa,20.4%and 9.026 × 10-3 mm3/m,obviously higher than those of AZ31 alloys.The enhanced mechanical properties were attributed to the grain refinement and strong interfacial bonding.The improved wear resistance was closely related to the increased hardness of composites and the formation of protective oxidation films.

    Keywords: Magnesium matrix composites;Ti particles;Microstructure;Mechanical properties;Wear resistance.?Corresponding authors at: College of Materials Science and Engineering,Chongqing University,Chongqing 400045,China.

    1.Introduction

    With the increasing requirement of energy saving and carbon emission reduction,the development of lightweight materials has been attracted wide attention [1,2].Due to the low density,high special strength,great special stiffness and excellent wear resistance,magnesium matrix composites (MMCs)have the potential to be applied in aerospace,automobile and military industries [3-5].The most commonly applied reinforcements in MMCs are discontinuous ceramic particles,such as SiC [6,7],TiC [8,9],Al2O3[10,11],B4C [12,13] etc.,which could significantly improve the strength,hardness,elastic modulus and thermal stability of MMCs.Nevertheless,due to the poor deformation characteristic of ceramic particles,the introduction of ceramic particles severely worsens the plasticity of MMCs [14-17],which would limit their potential application.Recently,metal reinforcements have been developed in MMCs.Compared to ceramic reinforcements,metal reinforcements show better plasticity and mechanical compatibility with MMCs [14,18].Therefore,metal reinforcements could be applied to improve the poor plasticity of MMCs.

    To select suitable metal reinforcements for MMCs,two factors should be considered [19,20].The one is that the reinforcement shows higher strength than the matrix for getting high strengthening effect.In this condition,Ti [21],Fe [22],Ni [23] and Cu [24] etc.can be the considerable reinforcements for MMCs.The other is that the reinforcements possess similar crystal structure to matrix to obtain good interfacial bonding.Both Ti and Mg have a hexagonal closed-packed(HCP) crystal structure [25-28].Thus,Ti particles can be considered as an ideal metal reinforcement for MMCs.Previous study showed that the wettability between Ti and Mg was very good,as their contact angle is 31° at 800 °C [29].Hence,a good interfacial bonding may be obtained between Mg and Ti.Besides,the solubility of Ti in Mg is negligible and Ti hardly reacts with Mg to form brittle compounds[25,30,31],which is conducive to the plasticity.Hassan and Gupta[32]synthesized Ti particles reinforced Mg composites,and the Mg composites showed a significant increase in yield strength but a decrease in ultimate tensile strength.Wang et al.[33,34] prepared Ti alloy particles reinforced AZ91 composites by stir casting.The composites presented a better plasticity than SiC particles reinforced AZ91 composites,but a lower elongation than AZ91 alloy.Jiang et al.indicated that the strong interfacial bonding between secondary phase andα-Mg could contribute to the plasticity of Mg alloys [35].This means that the plasticity of Ti particles reinforced MMCs might further be improved by the formation of strong interfacial bonding.Besides the mechanical properties,the wear resistance is another important property for MMCs.To date,the wear resistance of MMCs has been widely investigated[36,37].Unfortunately,those MMCs with good wear resistance showed poor plasticity.Ti is deformable and possesses higher hardness than Mg [38,39].Therefore,a simultaneous increase in strength,plasticity and wear resistance may be achieved in Ti particles reinforced MMCs with strong interfacial bonding at Ti/Mg interface.However,the interfacial bonding between Ti particles and Mg matrix,and wear mechanism of Ti particles reinforced MMCs are still unclear.The purpose of this work is to investigate the interfacial bonding of Ti/Mg interface,wear mechanism of Ti particles reinforced MMCs,and achieve a simultaneous increase in strength,plasticity and wear resistance of MMCs.

    In this work,the Ti particles reinforced AZ31 composites were fabricated by ultrasonic-assisted stir casting followed by hot extrusion.The microstructure,mechanical properties and wear resistance of as-extruded Ti/AZ31 composites were investigated.Especially,a strong interfacial bonding was achieved at Ti/Mg interface.The tensile strength,elongation and wear resistance of as-extruded Ti/AZ31 composites are increased simultaneously with the increment of Ti,which makes Ti/AZ31 composites possessing a prospect in aerospace,automobile industries.

    2.Experimental procedures

    2.1.Fabrication of Ti/AZ31 composites

    Spherical Ti particles of an average size of 8 μm and commercial AZ31 alloy ingot were used as raw materials.The Ti/AZ31 composites were prepared by ultrasonic-assisted stir casting followed by hot extrusion.Firstly,the AZ31 alloy was molten at 720 °C in a steel mold using an electronic resistance furnace under the protective atmosphere of CO2and SF6.The molten AZ31 was then cooled to 630 °C to obtain semi-solid condition.Ti particles were added in the molten AZ31 alloy in semi-solid state,and then mechanically stirred for 5 min.After stirring,the molten Ti/AZ31 composite was rapidly reheated to 660 °C to be in liquid state and ultrasonicated at 1600 W for 10 min.After ultrasonication,the molten Ti/AZ31 composite was quenched by water to get composite ingot.Before extrusion,the composite ingot was preheated at 350 °C for 1 h The preheated composite ingot was hot extruded at 350 °C with an extrusion ratio of 16:1.For comparison,the AZ31 alloy was prepared using the same method.

    2.2.Characterization

    The microstructures of as-extruded alloy and composites were investigated by optical microscope (OM,OLYMPUS OLS4000),emission scanning electron microscope (SEM,JEOL JSM-7800F) equipped with an energy dispersive spectrometer (EDS) and a HKL Chanel 5 electron backscattered diffraction (EBSD) system.For OM and SEM characterization,samples of 7 × 5 × 3 mm were mechanically ground with 2000 grid SiC paper.Samples for EBSD observation of 7 × 5 × 3 mm were electropolished with AC2 solution.The interfacial structure of 6 wt.%Ti/AZ31 composite was identified using transmission electron microscopy (TEM,FEI Talos F200x).For TEM characterization,thin foil samples were ground to~50 μm and ion-beam thinned using Gatan Precision Ion Polishing System.

    The tensile tests of as-extruded alloy and composites were determined parallel to the extrusion direction (ED) by an universal testing machine (GMT5105) at room temperature.The tensile toughness was obtained by calculating the area under the stress-strain curve of alloy and composites.The Vickers microhardness was conducted on a Zwick tester at a constant load of 0.1 g with dwell time of 10 s.Dry sliding test was conducted by pin-on-disk using an UTM-2 tribometer with a load of 20 N and sliding velocity of 50 mm/s at room temperature.Samples for wear test with dimensions of 12 × 9 × 3 mm were made from Ti/AZ31 composites as flat to against Al2O3ball.

    3.Results

    3.1.Microstructure

    Fig.1 shows the OM images of as-extruded Ti/AZ31 composites.In Fig.1(a),the unreinforced alloy contains dynamic recrystallization (DRX) zone and deformation zone.In Fig.1(b-d),the deformation zone disappears and the Mg matrix is composed of equiaxed grains.Thus,a full DRX is achieved in Ti-containing composites.In the zone close to Ti particles,the grains are much finer than those in Ti particle free zone,indicating the Ti particles can accelerate the DRX during extrusion.The measured average grain size is 4.6 μm for the unreinforced AZ31 alloy.While for the Ti/AZ31 composites,the measured average grain sizes are refined from 4.6 μm to 3.3 μm,as the content of Ti from 0 to 6 wt.%,respectively.However,with the further addition of Ti,the grain size of 9 wt.%Ti/AZ31 composite is increased inversely to 3.5 μm.Moreover,the distribution range of Ti/AZ31 composites shows a similar trend to the change of grain size.

    Fig.1.OM images and corresponding distribution maps of grain size of as-extruded Ti/AZ31 composites: (a) AZ31,(b) 3 wt.%Ti/AZ31,(c) 6 wt.%Ti/AZ31 and (d) 9 wt.%Ti/AZ31.

    Fig.2 shows the SEM microstructures of as-extruded Ti/AZ31 composites.In Fig.2(a),only a few secondary phases are observed.The magnified image shows that there are two kinds of secondary phases.One is Al8Mn5particles in micro size while the other is Mg17Al12particles below submicro.With the increment of Ti,the amount of secondary phase particles increases.In Fig.2(b,c),spherical Ti particles uniformly disperse in Mg matrix.However,agglomerate regions occur in 9 wt.%Ti/AZ31 composite (Fig.2d).The agglomerate of reinforcements has been widely reported in previous literature.When the reinforcements up to a high volume,the inter-spacing between reinforcements would be shorted,as compared to that for low volume reinforcements reinforced composites [40,41].As a result,the interaction between particles becomes inevitable,which leads to the agglomerate of reinforcements in composites during synthesis process.The agglomerate of reinforcements not only recedes the grain refinement of Mg matrix,but also serves as defects during deformation,which results in a decrease in mechanical properties.

    Fig.3 shows the inverse pole figures with corresponding pole figures of as-extruded Ti/AZ31 composites.It shows that the changes of grain size are consistent with the OM results.The value of the maximum texture intensity is 9.8,while the corresponding values are decreased to 6.3,5.5 and then increased to 6.7,with the addition of Ti from 0 to 9 wt.%.The change of the maximum texture of composites is the result of accumulated DRX process by Ti particles addition.

    Fig.4 shows the high angel annular dark field (HAADF)mapping of as-extruded 6 wt.%Ti/AZ31 composite.Based on Fig.4(b,c),it can be confirmed that the gray region is the spherical Ti particle while the black region is Mg matrix in Fig.4(a).At Ti/Mg interface,there are precipitates with a size of 10-20 nm as marked by orange circles.In Fig.4(c),it shows that a layer of Al element with a width of 50-100 nm occurs at the edge of spherical Ti.This indicates that there exists diffusion of Al atoms from Mg matrix to Ti particles forming Al-Ti compounds during synthesis process.

    Fig.5 presents the TEM line scanning of as-extruded 6 wt.%Ti/AZ31 composite.The scanning position and scanning direction are marked in Fig.5(a).The content of Mg increases sharply to 85 at.%,and the corresponding value of Ti decreases to 3 at.%at the position of~170 nm,which indicates the position of Ti/Mg interface (Fig.5b).At the side of Ti,there exists a plateau of Al,inferring that Al atoms diffuse in Ti particles forming Al-Ti compound.The content of Al close to the Ti/Mg interface is 40-50 at.%,while the value of Ti near the Ti/Mg interface is 40-45 at.%.Correspondingly,the atomic ratio of Al: Ti is about 1: 1.Therefore,the compound at Ti/Mg interface may be TiAl.

    Fig.2.SEM microstructures of as-extruded Ti/AZ31 composites: (a) AZ31,(b) 3 wt.%Ti/AZ31,(c) 6 wt.%Ti/AZ31 and (d) 9 wt.%Ti/AZ31.

    Fig.3.Inverse pole figures and pole figures of as-extruded Ti/AZ31 composites: (a) AZ31,(b) 3 wt.%Ti/AZ31,(c) 6 wt.%Ti/AZ31 and (d) 9 wt.%Ti/AZ31.

    The final mechanical properties of composites are highly dependent on the interfacial bonding between reinforcements and matrix.To reveal the interfacial structure of Ti/Mg,the TEM images of as-extruded 6 wt.%Ti/AZ31 composite are illustrated in Fig.6.Fig.6(b) is the magnified image of position B in Fig.6(a).It shows that there is an obvious interface.Thus,the upper of the image is denoted as region I,and the bottom of the image is region II.The measured d-spacings of region I are 0.1822 nm and 0.1798 nm,respectively,giving a parametera=0.4020 nm andc=0.4087 for TiAl.In region II,the measured d-spacings are 0.2765 nm and 0.1884 nm,respectively,which gives a parametera=3.191 nm andc=0.5139 nm for Mg matrix.The calculated lattice parameters and corresponding standard lattice parameters [42] are presented in Table 1.The calculated values are matched well with the standard values.Therefore,region I is TiAl,and region II is Mg.At the interface in Fig.6(c),TiAl and Mg matrix possess an obvious orientation relationship.The (012)plane of TiAl is parallel to the(0-112)plane of Mg.the calculated misfit between (012)TiAland (0-112)Mgis 3.2%,which is accordant with standard value of 5.1%.Baed on privious studies [43,44],a semi-coherent interface forms between Ti particles and Mg matrix.

    Fig.4.(a) HAADF image and corresponding EDS maps of 6 wt.%Ti/AZ31 composite: (b) Mg,(c) Ti,(d) Al,(e) Mn,(f) Zn.

    Fig.5.Line scanning maps of 6 wt.%Ti/AZ31 composite: (a) HAADF image,(b) line results of the dotted line in (a).

    Fig.6(d) is the magnified image of position D in Fig.6(a).It shows that rod-like particles (marked as region III) with a length of 20-50 nm and a width of 10 nm form at Ti/Mg interface.The EDS results indicate that the precipitates mainly consist of Al and Ti.The atomic ratio of Al:Ti is about 2: 1.It is deduced that the nanoprecipitates are Al2Ti.During synthesis process,Ti particles could stimulate the precipitation of secondary phase.Braszczynska-Malik and Prze?o˙zy′nska [30] reported that Al2RE phase formed on Ti particle in Mg-5Al-5RE alloy during casting.However,the effect of Al2RE on mechanical properties is still unknown.Zhang et al.[45] found that Al2Ti e forms on the surface of Ti particles,which finally contributed to mechanical properties.

    In region III,the measured d-spacings are 0.1965 and 0.2538 nm,giving a parametera=0.3930 nm andc=2.4926 nm for Al2Ti.The rod-like particles are confirmed to be Al2Ti.In Fig.6(e),it is clear that Al2Ti has an orientation relationship with TiAl.Namely,the (-2-10)plane of TiAl is parallel to the (0-20) plane of Al2Ti.The calculated misfit between TiAl and Al2Ti is 8.8%,matched well with the standard value of 10.4%.Therefore,the interface between TiAl and Al2Ti is semi-coherent.In Fig.7(f),the (114) plane of Al2Ti is parallel to the (10-11) plane of Mg.the calculated misfit between (114)Al2Tiand (10-11)Mgis 4.0%,which is accordant with the standard value of 3.8%.Thus,the interface between Al2Ti and Mg matrix is defined as a semi-coherent interface.

    Fig.6.Interfacial structure of 6 wt.%Ti/AZ31 composite: (a) TEM,(b) HRTEM of position B in (a),(c) TiAl/Mg interface,(d) HRTEM of position B in (a),MgO/Mg interface,(e) TiAl/Al2Ti interface and (f) Al2Ti/Mg interface.

    3.2.Mechanical properties

    Fig.7 displays the engineering tensile curves of asextruded Ti/AZ31 composites.And the yield strength (YS),Ultimate tensile strength (UTS),elongation and Vick hardness are presented in Table.2.The YS of unreinforced AZ31 alloy is 227 MPa,while the corresponding value of9 wt.%Ti/AZ31 composite is increased to 251 MPa finally.The UTS and elongation show a similar trend.The UTS,elongation and tensile toughness of Ti/AZ31 composites are increased firstly and then decreased with the increment of Ti.Especially,the 6 wt.%Ti/AZ31composite possesses the highest UTS of 327 MPa,elongation of 20.4% and tensile toughness of 63.4 MJ/m3,respectively.Furthermore,the hardness of Ti/AZ31 composites is increased with the increasing content of Ti from 64.3 to 68.2 HV.Therefore,the Ti/AZ31composites achieved a simultaneous increase in YS,UTS,elongation and hardness.

    Table 1 Experimental and standard values of the lattice parameters for TiAl,Al2Ti and Mg.

    Table 2 Mechanical properties and hardness of as-extruded Ti/AZ31 composites.

    Fig.7.Engineering tensile curves of as-extruded Ti/AZ31 composites.

    Fig.8 shows the comprehensive mechanical properties of Ti/AZ31 composites and other AZ31 composites [11,46-59].It shows Al2O3+Cu particles reinforced AZ31 composites possess UTS of 365 MPa,but their elongation is only~5.5%.The elongation of VN particles reinforced reaches to 14%.However,the UTS of VN/AZ31 composites is lower than 200 MPa.Those results indicate that it is still a great challenge to fabricate particles reinforced MMCs with both high strength and good elongation.It is noted that the Ti/AZ31 composites in this work show a simultaneous increase in strength and plasticity.

    Fig.8.The tensile strength and elongation of Ti/AZ31 composites and other AZ31 composites.

    3.3.Wear resistance

    Fig.9 shows the coefficient of friction (COF) of asextruded Ti/AZ31 composites.The friction of coefficient composites decreases firstly for 0.293-0.261 with the addition of Ti from 0 to 6 wt.%,indicating that the Ti particles can effectively reduce the COF of Ti/AZ31 composites during sliding.With further increment of Ti,the friction coefficient increases inversely to 0.272.

    Fig.9.(a) the coefficient of friction curves and (b) the average coefficient of friction of as-extruded Ti/AZ31 composites.

    Fig.10 shows the 3D morphology images and corresponding 2D profiles across the wear tracks of as-extruded Ti/AZ31 composites after wear tests.The morphology of composites shows a semicircle shape,accordant with the morphology of Al2O3milling ball.By measuring the values of peaks in 2D profiles in Fig.9,the maximum width and depth of wear scar are summarized in Fig.11(a,b),which illustrates that the wear width decreases firstly with increasing content of Ti and then increases with further increment of Ti.Besides,the wear depth reduces with Ti addition.The measured wear loss (volume loss) of composites shows a similar trend to the wear width.The measured wear loss and wear rate decrease from 1.045 to 0.813 mm3as the addition of Ti from 0 to 6 wt.%,indicating that Ti particles improve the wear resistance of Ti/AZ31 composites.The 6 wt.%Ti/AZ31 composite possesses the best wear resistance with wear volume and wear rate of 0.813 mm3and 9.026 × 10-3mm3/m.

    Fig.12 shows the sliding surface of as-extruded Ti/composites after sliding.Along the sliding direction,the grooves are observed in all samples.Therefore,the main characteristic of sliding of Ti/AZ31 composites is confirmed to be abrasive wear.In Fig.12(a),the delamination regions (as marked by blue dotted line) are observed and the sliding surface is quite rough.As the increment of Ti,the sliding surface becomes smoother as compared to the unreinforced alloy.Besides,circular-like and strip-like gray regions occur in Fig.12(b),as marked by yellow and red dotted lines,respectively.The EDS results show that the content of Ti is the highest in the circular-like regions and the circular-like regions present a similar shape to Ti particles.Therefore,the circular regions are the undeformed Ti particles.Before wear testing,the Ti particles are spherical as shown in Fig.2(b-d).However,the strip-like regions show similar EDS results to that of Ti particles.Moreover,the area of strip-like region is obviously bigger than that of circular-like region (Ti particles).Thus,it can be deduced that the strip-like regions are the deformed Ti particles.During dry sliding,the Ti particles deform under the repetitive press,and form films of Ti-Mg-O,which could protect the sliding surface.

    4.Discussion

    4.1.Grain refinement

    The microstructure evolution of as-extruded Ti/AZ31 composites reveals that Ti particles can effectively refine the grains of Mg matrix.The mechanisms of grain refinement for particles reinforced MMCs have been studied in literature.Generally,the reinforcements with different sizes show various mechanisms of grain refinement.Previous studies indicated that the reinforcements larger than 1 μm could promote the DRX process during extrusion (particle stimulated nucleation,PSN),while the reinforcements smaller than1 μm would hinder the growth of dynamic recrystallized (DRXed)grains by pinning the grain boundaries [41,60].In present work,the average size of used Ti particles is 8 μm larger than 1 μm.Therefore,the Ti particles will accelerate the nucleation process by PSN mechanism,which leads to the grain refinement of Ti/AZ31 composites.Besides the size of reinforcements,the interfacial structure between reinforcements and Mg matrix would also affect the grain refinement of composites.During synthesis process,a TiAl layer forms at Ti/Mg interface.It was reported that the crystallographic criterion for effective nucleation is that the misfit between match planes is lower than 10% along the closed packed direction [61].The misfit between TiAl layer and Matrix is 3.2% much lower than 10%.Thus,the Ti particles with the TiAl layer can serve as an effective nucleation substrate for Mg matrix,accelerating the nucleation effectiveness,and finally contributing to the grain refinement of composites.

    4.2.Interfacial bonding analysis

    Fig.10.3D morphology images and corresponding 2D profiles across the wear tracks of as-extruded Ti/AZ31 composites after wear tests: (a) AZ31,(b)3 wt.%Ti/AZ31,(c) 6 wt.%Ti/AZ31 and (d) 9 wt.%Ti/AZ31.

    The interfacial structure between reinforcements and Mg matrix has been reported in SiC [62],graphene [63],carbon nanotubes (CNTs) [44],and MgBO5[64] reinforced MMCs.In previous literature,a good interfacial bonding could be achieved,when no nano-crack or nanogap occurred at the interface between reinforcements and Mg matrix [65,66].Although,many graphene reinforced MMCs were fabricated,and no crack was observed at graphene/Mg interface.However,the graphene/Mg interface is defined as poor bonding interface,because of the poor wettability between graphene and Mg [67].The wettability between graphene and Mg is 120° [63].Yuan et al.[68] reported that the MgO nanoparticles at graphene/Mg interface could significantly improve the interfacial bonding of graphene/Mg owing to the formation of semi-coherent interface.Han et al.’ s work [69] indicated thatin-situformed Mg2Ni at CNTs/Mg interface possessed a coherent relationship with Mg matrix,finally contributing to the interfacial bonding of CNTs/Mg.Based on the studies above,it can be concluded that to obtain a strong interfacial bonding between reinforcements and Mg matrix,the following aspects need to be considered: (i) absence of nanogaps or nano-cracks at interface,(ii) a good lattice spacing matching.In the present work,a nanolayer of TiAl forms at Ti/Mg interface.The misfit between TiAl and Mg matrix is 3.2%,and the TiAl/Mg interface is semi-coherent interface.Moreover,many Al2Ti nanoparticles form at TiAl/Mg interface.The Al2Ti nanoparticles possess semi-coherent relationship with TiAl layer and Mg matrix,respectively.The semi-coherent interfacial bonding is commonly considered as strong interfacial bonding [41,43,44].Therefore,a strong interfacial bonding is achieved at Ti/Mg interface owing to the formation of semicoherent crystallographic orientation relationship of TiAl/Mg,TiAl/Ti2Al,Ti2Al/Mg.

    Fig.11.(a) Wear width,(b) wear depth,(c) volume loss and wear rate of as-extruded Ti/AZ31 composites.

    4.3.Strengthening and toughening mechanisms

    The tensile strength of Ti/AZ31 composites increases greatly,as the increment of Ti.The enhancement in tensile strength of composites can be attributed to the refined grain of Mg matrix,strong interfacial bonding of Ti/Mg interface.Therefore,four possible strengthening mechanisms contribute to the strength of Ti/AZ31 composites,namely grain boundary strengthening,load transfer strengthening,dislocation multiplication strengthening and Orowan strengthening.

    Firstly,the grain boundary strengthening significantly affects the YS of Ti/AZ31 composites.The improvement in YS is usually illustrated by the Hall-Petch equation:σy=σ0+kd-1/2[70].The YS shows an inverse relationship with the grain size.Namely,the finer the grain size,the higher the YS.As discussed in Section 4.1,the Ti particles in micro size can act as nucleation sites and then accelerate the PSN process.And the semi-coherent interface of TiAl/Mg improves the efficiency of nucleation for Mg matrix.As a result,shown the Fig.1,the average grain sizes of Ti/AZ31 composites were refined from 4.6 to 3.3 μm.The refined grains imply that the dislocations in grains are more probably to be impeded by the grain boundaries,which leads to an increase in YS of composites.Secondly,load transfer strengthening will significantly influence the YS of composites.Based on the TEM observations,a strong interfacial bonding is achieved at Ti/Mg interface.Therefore,during strength testing,the load could effectively transfer from Mg matrix to Ti particles,contributing to the increasement of YS.In addition,the dislocation multiplication strengthening has a great effect on YS.The thermal coefficient of Ti is 7.1 × 10-6K-1[71],while the corresponding value of Mg is 25 × 10-6K-1[67].The difference coefficient between Ti and Mg results in the multiplication of dislocations close to of Ti particles after extrusion,which leads to an increase in YS of composites.Orowan strengthening is commonly considered for MMCs.In present work,the contribution of Orowan strengthening may be insignificant.The Orowan strengthening highly depends on the volume fraction and particle size of reinforcements [72].In present work,the used Ti particles belong to micro size.As reported in previous literature,only a limited increasement could be achieved in microparticles reinforced MMCs [73].

    Fig.12.The sliding surface of as-extruded Ti/composites after sliding.(a) AZ31,(b) 3 wt.%Ti/AZ31,(c) 6 wt.%Ti/AZ31 and (d) 9 wt.%Ti/AZ31.

    In addition to the strength,the elongation of composites presents a comparable improvement as well.The increase in elongation of composites is due to the refined grains,weakened texture and deformable reinforcements.As presented in Fig.1,the grain sizes of Ti/AZ31 composites are obviously refined with the increment of Ti.For metal materials,on the one side,the fine grains are beneficial to offsetting stress to more grains and avoiding the inhomogeneous deformation[74].On the other side,the finer grains mean more grain boundaries,impeding the propagation of cracks [75].Therefore,the smaller the grains,the better the plasticity.Next,the texture could also influence the plasticity of composites.The unreinforced AZ31 alloy possesses the highest maximum texture intensity of 9.9,which means that there are more grains with their c-axis perpendicular to extrusion direction (ED).It is unfavorable to tensile deformation along ED.With the increment of Ti,the maximum texture of Ti/AZ31 composites decreases to 5.5,which means that the orientation of grains becomes more random in Ti-containing composites [65].The grains with random orientation can coordinate the deformation,contributing to the plasticity of composites.Moreover,Ti is a metallic material with high plasticity.Based on the studies [76,77],the yield strength of pure Ti is lower than the UTS of Ti/AZ31 composites in this work.Namely,when the stress equal to the UTS of Ti/AZ31 composites is conducted to Ti particles,both elastic deformation and plastic deformation will occur in Ti particles.Therefore,the Ti particles will synergistically deform with Mg matrix during tensile testing,which is conducive to plasticity.Moreover,a strong interfacial bonding is achieved at Ti/Mg interface,which can impede the debonding of Ti particles from Mg matrix during deformation and then contribute to the plasticity of composites [35,78].However,as the Ti content reaches 9 wt.%,the grain size becomes coarse and clusters of Ti particles occur.As a result,the elongation of 9 wt.%Ti/AZ31 composite deteriorates.

    4.4.Wear mechanism

    Many factors could affect the wear resistance of composites,including hardness,roughness of wear surface,lubrication and temperature etc.In the present work,the samples are dry slid against the Al2O3ball at room temperature.Therefore,the hardness will significantly influence the wear resistance of composites.On the one side,the grain size of Ti/AZ31 composites is reduced with the increment of Ti.Generally,the finer the grain,the higher the hardness [79].On the other side,high density dislocations occur in the vicinity of Ti particles during extrusion.The high density dislocations offer diffusion channels for atoms,and then stimulate the precipitation of secondary phase particles,increasing the amount of precipitation of secondary phase particles [73,80].In Mg-Al based alloy,the secondary phases,such as Mg17Al12and Al8Mn5,have higher hardness than Mg matrix [81,82],which improves the hardness of composites.Based on the Archard’s law [37]:

    Fig.13.Schematic of wear surface of Ti/AZ31 composites during sliding.

    WhereVis the volume loss,Kis the Archard’s constant,Fis the applied load,Lis the sliding distance,His the hardness of texted samples.The wear loss shows an inverse proportion to the hardness.The less wear loss means better wear resistance.Therefore,the wear resistance of Mg matrix is enhanced with the addition of Ti.

    Besides,the Ti particles greatly influence the wear resistance.The Ti particles have a hardness of 120 HV much higher than that of Mg matrix [38],which means that the Ti particles have better resistance than Mg matrix.Thus,it is more difficult to be ground off for Ti particles,as compared to the soft Mg matrix.As the surface layer of Mg is ground off,the emerged Ti particles from Mg matrix could further slide against the Al2O3ball,which improves the wear resistance of composites.In Fig.11(a),delamination regions are observed.The delamination is caused by repeated sliding loads.Under the repeated load,cracks nucleate and propagate at subsurface,which results in the removal of material,leaving caves on the sliding surface [83].With the addition of Ti,the delamination regions are reduced,which is beneficial to the decrease in the volume loss.In Fig.11(b-d),films of Ti-Mg-O form on the sliding surface.During the repeated sliding motion,the emerged Ti particles are deformed and oxidized,forming films of Ti-Mg-O.In previous studies,the oxidation film was commonly defined as tribofilm[84].The oxidation films coating on sliding surface can effectively protect sliding surface [85].As the increment of Ti,more oxidation films form on the sliding surface.Therefore,the wear resistance of composites is significantly improved.The schematic of wear surface during sliding is illustrated in Fig.13.During sliding,the soft Mg is ground off from the sample surface.Then,Ti particles emerge from Mg matrix and resist against the milling ball.Next,the Ti particles form oxidation films under repeated sliding to protect the sliding surface.

    5.Conclusions

    AZ31 composites reinforced with Ti particles were fabricated using ultrasonic-assisted stir casting followed by hot extrusion.The microstructure,mechanical properties and wear resistance of the as-extruded Ti/AZ31 composites were studied.The main conclusions can be summarized as follows:

    (1) With the increasing Ti content,the grains of Ti/AZ31 composites were refined and the basal texture was weakened.

    (2) The Al atoms diffused to the edge of Ti particles,forming a nanolayer of TiAl at Ti/Mg interface.Rod-like nanoparticles of Al2Ti precipitated at TiAl/Mg interface.A strong interfacial bonding was achieved because of the semi-coherent crystallographic orientation relationship of TiAl/Mg,TiAl/Al2Ti,Al2Ti/Mg interfaces.

    (3) The mechanical properties of Ti/AZ31 composites were obviously enhanced owing to the refined grains and strong interfacial bonding.The 6 wt.%Ti/AZ31 composite possessed YS,UTS and elongation of 245 MPa,327 MPa and 20.4%,respectively.

    (4) The Ti/AZ31 composites showed a higher wear resistance than the unreinforced AZ31 alloy,which was due to the increased hardness of the composites and the formation of protective oxidation films.

    Declaration of Competing Interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgments

    The authors would like to thank the financial supports from the Guangdong Major Project of Basic and Applied Basic Research (2020B0301030006),the National Natural Science Foundation of China (Nos.52171103,52171133),the Natural Science Foundation of Chongqing (cstc2019jcyjmsxmX0234),the “111 Project” (B16007) by the Ministry of Education,the Fundamental Research Funds for the Central Universities (No.2020CDJDPT001) and Graduate Research and Innovation Foundation of Chongqing,China (No.CYB21001).The author would like to thank joint lab for electron microscopy of Chongqing University.

    久久精品91蜜桃| 高清av免费在线| av视频在线观看入口| 亚洲国产色片| 国产亚洲av片在线观看秒播厂 | 日韩亚洲欧美综合| 乱码一卡2卡4卡精品| 伊人久久精品亚洲午夜| 中文天堂在线官网| 一边亲一边摸免费视频| 国产片特级美女逼逼视频| 久久99热6这里只有精品| 国产精品野战在线观看| 日韩av在线免费看完整版不卡| 黑人高潮一二区| av在线播放精品| 国产亚洲一区二区精品| 麻豆成人av视频| 午夜日本视频在线| 色综合站精品国产| 人妻少妇偷人精品九色| 免费人成在线观看视频色| 你懂的网址亚洲精品在线观看 | 直男gayav资源| 亚洲欧美成人精品一区二区| 99久久九九国产精品国产免费| 少妇熟女aⅴ在线视频| 久久鲁丝午夜福利片| 欧美激情久久久久久爽电影| 国产一级毛片七仙女欲春2| 寂寞人妻少妇视频99o| 日本黄色视频三级网站网址| 精品一区二区三区人妻视频| 久久热精品热| 黄片wwwwww| 亚洲怡红院男人天堂| 亚洲av.av天堂| 国产成年人精品一区二区| 高清av免费在线| 国产亚洲最大av| 久久综合国产亚洲精品| 一区二区三区乱码不卡18| 国内精品宾馆在线| 18禁动态无遮挡网站| 国产伦一二天堂av在线观看| 黄片wwwwww| 国产高清有码在线观看视频| 蜜桃亚洲精品一区二区三区| h日本视频在线播放| 国产 一区精品| 久久综合国产亚洲精品| 欧美高清性xxxxhd video| 国产毛片a区久久久久| 欧美日韩精品成人综合77777| 青青草视频在线视频观看| 日韩一区二区三区影片| 高清视频免费观看一区二区 | 免费大片18禁| 日本黄色片子视频| 91狼人影院| 中文欧美无线码| 18禁在线播放成人免费| 老司机福利观看| 亚洲欧美日韩东京热| 国产一区二区三区av在线| 一二三四中文在线观看免费高清| 久久久久久久国产电影| 全区人妻精品视频| 亚洲内射少妇av| 亚洲欧美日韩高清专用| 欧美高清成人免费视频www| 久久久午夜欧美精品| 亚洲最大成人av| 少妇人妻精品综合一区二区| 少妇熟女aⅴ在线视频| 男女下面进入的视频免费午夜| 亚洲aⅴ乱码一区二区在线播放| 一卡2卡三卡四卡精品乱码亚洲| 看免费成人av毛片| 色噜噜av男人的天堂激情| 亚洲欧美日韩卡通动漫| 日本三级黄在线观看| 波野结衣二区三区在线| 国产成人精品婷婷| 三级毛片av免费| 国产精品人妻久久久久久| 2022亚洲国产成人精品| 久久6这里有精品| 国产精品久久电影中文字幕| 午夜福利在线观看免费完整高清在| 天堂√8在线中文| 精品人妻熟女av久视频| 久久久久久久久久成人| 亚洲av男天堂| 亚洲欧美一区二区三区国产| 亚洲最大成人中文| 亚洲一级一片aⅴ在线观看| 国产亚洲av嫩草精品影院| 亚洲在线自拍视频| 神马国产精品三级电影在线观看| 国产成人福利小说| 色播亚洲综合网| 成人亚洲精品av一区二区| 伊人久久精品亚洲午夜| 成人国产麻豆网| 中文精品一卡2卡3卡4更新| 亚洲最大成人手机在线| 直男gayav资源| 久久鲁丝午夜福利片| 九九久久精品国产亚洲av麻豆| 能在线免费看毛片的网站| 国产 一区 欧美 日韩| 亚洲国产高清在线一区二区三| 日韩三级伦理在线观看| 能在线免费观看的黄片| 精品少妇黑人巨大在线播放 | 亚洲在线自拍视频| av播播在线观看一区| 成人午夜高清在线视频| 亚洲人成网站高清观看| 日产精品乱码卡一卡2卡三| 亚洲av一区综合| 亚洲人成网站在线播| av福利片在线观看| 色综合站精品国产| av线在线观看网站| 亚洲激情五月婷婷啪啪| 亚洲aⅴ乱码一区二区在线播放| 精品久久久久久久久久久久久| 国产一级毛片七仙女欲春2| 久久精品综合一区二区三区| 欧美另类亚洲清纯唯美| 国内少妇人妻偷人精品xxx网站| 久久久精品94久久精品| 精品99又大又爽又粗少妇毛片| av福利片在线观看| 国产亚洲午夜精品一区二区久久 | 国产精品熟女久久久久浪| 国产精品野战在线观看| 国产一区二区三区av在线| 嫩草影院入口| 精品久久久久久久人妻蜜臀av| 亚洲欧美日韩无卡精品| 春色校园在线视频观看| 国产精品99久久久久久久久| 免费不卡的大黄色大毛片视频在线观看 | 天美传媒精品一区二区| 精品久久久久久久久久久久久| 国产精品一区二区性色av| 欧美性猛交黑人性爽| 免费看av在线观看网站| 全区人妻精品视频| 中国国产av一级| 国产精品蜜桃在线观看| av在线蜜桃| 激情 狠狠 欧美| 久热久热在线精品观看| 国产免费一级a男人的天堂| 日韩强制内射视频| 18禁动态无遮挡网站| 亚洲中文字幕日韩| 69人妻影院| 精品人妻一区二区三区麻豆| 成人毛片a级毛片在线播放| 久久久久久大精品| av黄色大香蕉| av播播在线观看一区| 18禁在线无遮挡免费观看视频| 久久精品熟女亚洲av麻豆精品 | 免费av毛片视频| 午夜爱爱视频在线播放| 免费av不卡在线播放| 国产国拍精品亚洲av在线观看| 国产乱来视频区| 一个人看的www免费观看视频| 长腿黑丝高跟| 亚洲图色成人| 国产极品天堂在线| 亚洲国产精品成人综合色| 国产 一区 欧美 日韩| 久久欧美精品欧美久久欧美| 一个人观看的视频www高清免费观看| 久久久久久久亚洲中文字幕| 26uuu在线亚洲综合色| 美女cb高潮喷水在线观看| 人人妻人人看人人澡| 精华霜和精华液先用哪个| 最近手机中文字幕大全| 亚洲欧美日韩东京热| 国产精品人妻久久久影院| 麻豆av噜噜一区二区三区| 三级经典国产精品| 深爱激情五月婷婷| 欧美97在线视频| 日韩欧美精品v在线| 一本久久精品| 特级一级黄色大片| 床上黄色一级片| 国产精品伦人一区二区| 国产乱人视频| 一区二区三区免费毛片| 欧美+日韩+精品| 免费不卡的大黄色大毛片视频在线观看 | 国产精品国产三级国产av玫瑰| 人妻夜夜爽99麻豆av| 日本wwww免费看| 一级二级三级毛片免费看| 日韩亚洲欧美综合| 啦啦啦韩国在线观看视频| 三级国产精品欧美在线观看| 亚洲国产欧洲综合997久久,| 国产精品熟女久久久久浪| 国产一区有黄有色的免费视频 | 国产在视频线精品| 99久国产av精品| 人人妻人人看人人澡| 亚洲精品,欧美精品| 又粗又硬又长又爽又黄的视频| 国产精品美女特级片免费视频播放器| 国产午夜精品一二区理论片| 男人舔奶头视频| av又黄又爽大尺度在线免费看 | 男女那种视频在线观看| av在线蜜桃| 爱豆传媒免费全集在线观看| 一本一本综合久久| 在线播放国产精品三级| 人妻制服诱惑在线中文字幕| 国产三级在线视频| 亚洲av成人av| 丰满少妇做爰视频| 午夜久久久久精精品| 三级男女做爰猛烈吃奶摸视频| 日韩一本色道免费dvd| 国产精品精品国产色婷婷| 国产一级毛片在线| 在线a可以看的网站| 我的女老师完整版在线观看| 久久久色成人| 99热精品在线国产| 国产精品一区二区性色av| 一级毛片电影观看 | 男女那种视频在线观看| 国产成人精品久久久久久| 亚洲av成人精品一二三区| 一个人观看的视频www高清免费观看| 18禁动态无遮挡网站| 亚洲国产精品合色在线| www日本黄色视频网| 免费观看性生交大片5| 99久国产av精品| 国产黄片美女视频| 亚洲国产精品专区欧美| av国产久精品久网站免费入址| 国产又黄又爽又无遮挡在线| 精品国产露脸久久av麻豆 | 日韩精品青青久久久久久| 乱人视频在线观看| 亚洲精品456在线播放app| 亚洲电影在线观看av| 国产黄色小视频在线观看| 中文字幕久久专区| 国产成人免费观看mmmm| 麻豆av噜噜一区二区三区| 国产精品一区二区性色av| 国产成人a∨麻豆精品| 日韩欧美在线乱码| 九色成人免费人妻av| 国产乱人偷精品视频| 黄片无遮挡物在线观看| 人妻少妇偷人精品九色| 麻豆久久精品国产亚洲av| 色播亚洲综合网| 亚洲欧美成人精品一区二区| 男女边吃奶边做爰视频| 国产高清三级在线| 菩萨蛮人人尽说江南好唐韦庄 | 两个人的视频大全免费| 亚洲综合精品二区| 亚洲经典国产精华液单| 欧美激情在线99| 久久久欧美国产精品| 国产精品一及| 99久久人妻综合| 国产三级在线视频| 99热全是精品| ponron亚洲| videossex国产| 亚洲最大成人中文| 嫩草影院新地址| 国产又色又爽无遮挡免| 床上黄色一级片| 最近最新中文字幕大全电影3| 少妇丰满av| 国产中年淑女户外野战色| 国产精品久久久久久久电影| 卡戴珊不雅视频在线播放| 亚洲欧美成人精品一区二区| 狂野欧美激情性xxxx在线观看| 99热这里只有是精品50| 我的女老师完整版在线观看| 尤物成人国产欧美一区二区三区| 婷婷色综合大香蕉| 啦啦啦啦在线视频资源| 国内少妇人妻偷人精品xxx网站| 能在线免费看毛片的网站| 国产成人freesex在线| 最近视频中文字幕2019在线8| 又爽又黄a免费视频| 人人妻人人澡欧美一区二区| 成人性生交大片免费视频hd| 国产精品久久久久久久电影| 日韩高清综合在线| 久久久久久久久久久免费av| 色综合站精品国产| 国产精品麻豆人妻色哟哟久久 | 午夜福利在线观看吧| 天天一区二区日本电影三级| 欧美性感艳星| 天堂网av新在线| 亚洲综合色惰| 特大巨黑吊av在线直播| 日本五十路高清| 美女cb高潮喷水在线观看| 亚洲成色77777| 欧美zozozo另类| 国产午夜精品论理片| 国产视频首页在线观看| 看黄色毛片网站| 国产亚洲午夜精品一区二区久久 | 亚洲av不卡在线观看| 蜜臀久久99精品久久宅男| 成人性生交大片免费视频hd| 中文字幕av成人在线电影| 男人和女人高潮做爰伦理| 国产白丝娇喘喷水9色精品| 噜噜噜噜噜久久久久久91| 99热精品在线国产| 久久久久久国产a免费观看| 成人一区二区视频在线观看| av又黄又爽大尺度在线免费看 | 搡女人真爽免费视频火全软件| 干丝袜人妻中文字幕| 亚洲精品自拍成人| 久久6这里有精品| 亚洲最大成人中文| 卡戴珊不雅视频在线播放| 大香蕉久久网| 性插视频无遮挡在线免费观看| 亚洲无线观看免费| 欧美性猛交黑人性爽| 亚洲av中文字字幕乱码综合| 国产高清国产精品国产三级 | 欧美成人a在线观看| 中文字幕av成人在线电影| 插阴视频在线观看视频| 一个人看视频在线观看www免费| 中文字幕av成人在线电影| 国产人妻一区二区三区在| 中文天堂在线官网| 99热全是精品| 国产 一区精品| 国产一级毛片在线| 久久精品久久久久久噜噜老黄 | 午夜福利高清视频| 国产 一区精品| 91精品国产九色| 婷婷色综合大香蕉| 99久久人妻综合| 亚洲伊人久久精品综合 | 国产爱豆传媒在线观看| 久久韩国三级中文字幕| 午夜免费男女啪啪视频观看| 免费大片18禁| 国产精品国产高清国产av| 免费观看性生交大片5| 人妻制服诱惑在线中文字幕| 亚洲五月天丁香| 一级黄色大片毛片| 亚洲av一区综合| 日本熟妇午夜| 精品久久久久久久末码| 人体艺术视频欧美日本| 1024手机看黄色片| 久久欧美精品欧美久久欧美| 成人二区视频| 热99在线观看视频| 真实男女啪啪啪动态图| 亚洲av成人av| 97超碰精品成人国产| 欧美一区二区亚洲| 色视频www国产| 白带黄色成豆腐渣| 日本一二三区视频观看| 成人毛片a级毛片在线播放| 国产黄色视频一区二区在线观看 | 国产精品久久电影中文字幕| 99久久中文字幕三级久久日本| 成人性生交大片免费视频hd| 我的老师免费观看完整版| 久99久视频精品免费| 亚洲精品亚洲一区二区| 少妇猛男粗大的猛烈进出视频 | www.av在线官网国产| av在线播放精品| 网址你懂的国产日韩在线| 成人无遮挡网站| 高清视频免费观看一区二区 | 亚洲人成网站在线播| 日韩制服骚丝袜av| 久久久久久久亚洲中文字幕| 一级毛片电影观看 | 色哟哟·www| 国产精品人妻久久久久久| 在线观看美女被高潮喷水网站| 欧美3d第一页| 99久久精品热视频| 成人美女网站在线观看视频| 亚洲欧洲日产国产| 欧美激情国产日韩精品一区| 天天躁日日操中文字幕| 联通29元200g的流量卡| 欧美性感艳星| 人人妻人人澡人人爽人人夜夜 | 人妻系列 视频| 2021天堂中文幕一二区在线观| 99久国产av精品| 日本wwww免费看| 日本一本二区三区精品| 久久久久久大精品| 成人高潮视频无遮挡免费网站| 女人十人毛片免费观看3o分钟| 网址你懂的国产日韩在线| 亚洲欧美清纯卡通| 午夜福利高清视频| 国产一级毛片在线| 国产精品一及| 赤兔流量卡办理| 日韩成人av中文字幕在线观看| 国产白丝娇喘喷水9色精品| 最近手机中文字幕大全| 亚洲激情五月婷婷啪啪| 女的被弄到高潮叫床怎么办| 深夜a级毛片| 别揉我奶头 嗯啊视频| 国产成人免费观看mmmm| 免费一级毛片在线播放高清视频| 亚洲av电影在线观看一区二区三区 | 国产视频内射| 久久亚洲精品不卡| 国产高清三级在线| 亚洲最大成人av| 人妻制服诱惑在线中文字幕| 男插女下体视频免费在线播放| 午夜福利高清视频| 极品教师在线视频| 国产精品国产三级国产av玫瑰| 亚洲丝袜综合中文字幕| 校园人妻丝袜中文字幕| 亚洲av二区三区四区| 国产精品熟女久久久久浪| 欧美又色又爽又黄视频| 蜜桃久久精品国产亚洲av| 国产欧美另类精品又又久久亚洲欧美| 日韩在线高清观看一区二区三区| 一个人观看的视频www高清免费观看| 九色成人免费人妻av| 小蜜桃在线观看免费完整版高清| 日本av手机在线免费观看| 三级经典国产精品| 亚洲国产精品成人久久小说| 亚洲国产精品sss在线观看| av线在线观看网站| 亚洲欧洲日产国产| 九草在线视频观看| 最近手机中文字幕大全| 日产精品乱码卡一卡2卡三| 99热这里只有精品一区| 一边亲一边摸免费视频| 国产成人freesex在线| 亚洲va在线va天堂va国产| 国内少妇人妻偷人精品xxx网站| 婷婷色av中文字幕| 日日撸夜夜添| 亚洲精华国产精华液的使用体验| 两个人视频免费观看高清| 日本免费在线观看一区| 中文字幕精品亚洲无线码一区| eeuss影院久久| 久久久久久久亚洲中文字幕| 成人漫画全彩无遮挡| 国产精品.久久久| 中文乱码字字幕精品一区二区三区 | 久久久久久九九精品二区国产| 精品欧美国产一区二区三| 国产探花极品一区二区| 国产乱人视频| 午夜激情欧美在线| 日产精品乱码卡一卡2卡三| 人妻系列 视频| 深夜a级毛片| 午夜福利成人在线免费观看| 3wmmmm亚洲av在线观看| 嘟嘟电影网在线观看| 欧美日韩精品成人综合77777| 国产v大片淫在线免费观看| 少妇被粗大猛烈的视频| 成人亚洲精品av一区二区| 婷婷色综合大香蕉| 精品久久久久久成人av| 国产成人91sexporn| 国产成人精品一,二区| 九色成人免费人妻av| 成人综合一区亚洲| АⅤ资源中文在线天堂| 99热这里只有是精品50| 在线免费观看的www视频| 久久久久久久久久久丰满| 久久久久久久久大av| 国产色爽女视频免费观看| 五月玫瑰六月丁香| 国产探花在线观看一区二区| 男女边吃奶边做爰视频| 波多野结衣巨乳人妻| 亚洲av电影在线观看一区二区三区 | 又粗又爽又猛毛片免费看| 最近2019中文字幕mv第一页| 国产三级中文精品| 青春草国产在线视频| 午夜日本视频在线| 成年免费大片在线观看| 亚洲成人中文字幕在线播放| 国产亚洲精品av在线| 青青草视频在线视频观看| 久久鲁丝午夜福利片| 亚洲精品影视一区二区三区av| 人体艺术视频欧美日本| 亚洲精品国产av成人精品| 午夜福利在线观看免费完整高清在| 久久久久网色| 国产不卡一卡二| 99久久精品一区二区三区| 国产成人a∨麻豆精品| 亚洲精品亚洲一区二区| 天堂影院成人在线观看| 免费看美女性在线毛片视频| 人人妻人人澡人人爽人人夜夜 | 欧美高清性xxxxhd video| 国国产精品蜜臀av免费| 亚洲色图av天堂| 热99re8久久精品国产| 日韩制服骚丝袜av| 中国美白少妇内射xxxbb| 日本一二三区视频观看| 哪个播放器可以免费观看大片| 夜夜爽夜夜爽视频| 免费搜索国产男女视频| 神马国产精品三级电影在线观看| 老师上课跳d突然被开到最大视频| 偷拍熟女少妇极品色| 国产精品久久久久久久电影| 久久草成人影院| 亚洲内射少妇av| 亚洲成色77777| 麻豆精品久久久久久蜜桃| 97超视频在线观看视频| 少妇熟女aⅴ在线视频| 熟女人妻精品中文字幕| 免费av毛片视频| 欧美+日韩+精品| 亚洲最大成人手机在线| 久久精品久久久久久噜噜老黄 | 国产免费视频播放在线视频 | 亚洲成人中文字幕在线播放| 成人欧美大片| 91精品伊人久久大香线蕉| 久久久亚洲精品成人影院| 免费黄网站久久成人精品| 国产高清国产精品国产三级 | 国产单亲对白刺激| 美女黄网站色视频| 国产精品乱码一区二三区的特点| 99在线视频只有这里精品首页| 少妇被粗大猛烈的视频| 久久久久久久久中文| 亚洲精品国产av成人精品| av国产免费在线观看| 精品久久久噜噜| 国产成人a∨麻豆精品| 亚洲真实伦在线观看| av在线老鸭窝| 日韩av在线大香蕉| av在线观看视频网站免费| 夜夜爽夜夜爽视频| 亚洲精品影视一区二区三区av| 日本与韩国留学比较| 亚洲av成人精品一区久久| 久久精品久久精品一区二区三区| 91午夜精品亚洲一区二区三区| 精品人妻一区二区三区麻豆| 嫩草影院新地址| 亚洲精品亚洲一区二区| 久久久久久久亚洲中文字幕| 免费搜索国产男女视频| 免费看a级黄色片| 天堂网av新在线| 18禁在线无遮挡免费观看视频| 国产精品无大码| 麻豆一二三区av精品| 99久久精品国产国产毛片| 久久精品夜夜夜夜夜久久蜜豆| 亚洲欧美成人精品一区二区| 好男人在线观看高清免费视频| 26uuu在线亚洲综合色| 中文资源天堂在线|