    Enhancement of corrosion resistance of AZ31 Mg alloys by one-step in situ synthesis of ZnAl-LDH film intercalated with organic anions (ASP, La)

    2021-05-21 03:32:38YuhnSongYnTngLingFngFngWuXinGungZengJiHu
    Journal of Magnesium and Alloys 2021年2期

    Yuhn Song, Yn Tng, Ling Fng, Fng Wu, XinGung Zeng, Ji Hu,

    Shu Fang Zhange, Bin Jiangd, HaiJun Luof,*

    aState Key Laboratory of Power Transmission Equipment & System Safety and New Technology, Chongqing Key Laboratory of Soft Condensed Matter Physics and Smart Materials, College of Physics, Chongqing University, Chongqing 400044, PR China

    b School of Chemical &Environmental Engineering, China University of Mining & Technology, Beijing 100083, PR China

    cMaterial Corrosion and Protection Key Laboratory of Sichuan Province, Institute of Materials Science and Engineering, Sichuan University of Science and Engineering, Zigong, Sichuan Province 643000, PR China

    d National Engineering Research Center for Magnesium Alloys, College of Materials Science and Engineering, Chongqing University, Chongqing 400044, PR China

    e College of Software, Chongqing College of Electronic Engineering, Chongqing 401331, PR China

    fKey Laboratory on Optoelectronic Functional Materials, College of Physics and Electronic Engineering, Chongqing Normal University, Chongqing 401331,PR China

    Received 22 December 2019; received in revised form 5 March 2020; accepted 21 March 2020

    Available online 10 October 2020

    Abstract

    Keywords: ZnAl-LDHs; Magnesium alloy; Organic anions; Corrosion resistance; Aspartic acid; Lauric acid.

    1. Introduction

    Magnesium alloys are widely used in automobile manufacturing, electronics industry, aerospace and other field due to their high stiffness ratio, excellent electrical and thermal conductivity, good cast and process ability, and ease of recycling

    [1]. However, the low standard potential (-2.36V relative to a standard hydrogen electrode) of Mg alloys cause them being prone to corrosion in humid air,sea water,acids and salts,greatly limiting their widely application[2-5].So a lot of surface modificatio methods have been proposed to improve its corrosion protection property. Among these various protective coatings approaches, layered double hydroxides (LDHs) have got increasingly attention on their prevention Mg alloys from corrosion in recent years [6-9].

    LDHs are a class of an anionic intercalated compounds with a special laminated structure which can be expressed by a general formula: [M2+1-xM3+x(OH)2]x+(An-)x/n·yH2O. The hydrotalcite layer consists of M2+and M3+cationslocating in the octahedral pores, An-is interlayer anions, x is the molar ratio of M3+/(M2++M3+), and m is the number of water molecules in the interlayer [10-13]. The unique inter-layer anion exchange ability makes LDHs can capture aggressive anions such as Cl- and retard corrosion reactions. Furthermore, the corrosion inhibitors exchanged with the LDHs laminates may protect the substrate from local corrosion [14]. Therefore,encapsulating corrosion inhibitor into the hierarchical LDHs was proposed to a new approach to achieve high corrosion resistance or obtain a self-healing protection for metallic substrates [14-21]. But the proper types of LDH and the corrosion inhibitor maybe quite different for various substrates, so it is worth findin out the most suitable one for the protection of Mg alloy.

    Up to now, two kinds of typical LDHs, MgAl-LDHs and ZnAl-LDHs, have been mainly explored to encapsulate corrosion inhibitor. For example, Montemor et al. fabricated MgAl-LDH inserted with mercaptobenzothiazolate(MBT)anions and got an enhanced corrosion resistance to chloridecontaining solution[15].Chen et al.deposited MgAl-PA-LDH by embedding organic phytic acid (PA) into the synthesized MgAl- CO32--LDH laminate [16]. Zeng, et al. intercalated the molybdate into MgAl hydrotalcite coating on AZ31 Mg alloy[17].Wang et al.found their MgAl-LDHs film prepared using a hydrothermal method consist of graded nanosheets(NSs) and uniformly cover the substrate surface [18], thus effectively improve the corrosion resistance of Mg alloys. But the graded LDH NSs structure was destroyed after immersion in a 3.5 wt.% NaCl solution for 6 h, indicating that the MgAl-LDH was not so stable in corrosion solution.

    Besides MgAl-LDH, due to its excellent structural stability and ion exchange capacity, ZnAl-LDHs have been also employed as a matrix container to load corrosion inhibitors to protect Mg alloys [19-21]. The electrochemically deposited ZnAl-NO3-LDH [19], and the superhydrophobic ZnAl-CO3-LDH [20], ZnAl-LDH, respectively intercalated with Cl-and VOx-anions [21] were tried to increase the anti-corrosion performance of AZ91D Mg alloy.

    However, inorganic compounds are generally employed as the corrosion inhibitor on MgAl-LDH or ZnAl-LDH[17,19-21]. Due to special functional groups and containing nitrogen, oxygen, phosphorus, sulfur and multiple bonds or aromatic rings, the organic compounds may have better inhibition effect than the inorganic ones [22], so surface treatments with organic coating can be adopted to protect metal surface from corrosion.

    Aspartic acid (ASP) and lauric acid (La), two natural environmentally friendly organic compounds, were found to have the ability to improve the anti-corrosion of Al alloys [22-23].For instance, in order to increase the corrosion resistance of Al alloys, the ZnAl-LDH coating intercalated with lauric acid(La) [23], and ZnAl- and MgAl-LDHs loaded with quinaldate(QA) and 2-MBT anions were explored [24]. Zeng et al. synthesized the ZnAl-LDH/poly(lactic acid) composite coating on AZ31 Mg alloy [25]. But to the best of our knowledge,there are few reports about the application of ZnAl-LDHs with ASP or La for the protection of Mg alloy. Meanwhile,most of the LDH-based anti-corrosion coatings were obtained by a complicated two-step process (the corrosion inhibitors are usually inserted into the LDH layers by ion-exchange after the formation of LDH), so some facile and more costeffective approaches, especially one-step methods are urgent to develop. In our previous work, ZnAl-LDHs encapsulated with different inorganic anions(NO3-, Cl-, VO43-, PO43-,and MoO42-) [26] and rose-like MgAl-LDH coating with organic ASP [27] were synthesized on AZ31 Mg alloys with a simple hydrothermal method, and their corrosion resistance or self-healing were observed.

    Therefore,in this work,the ASP and La were chosen as the corrosion inhibitor and embedded into the ZnAl-LDH laminate to form ZnAl-ASP-LDHs and ZnAl-La-LDHs coating on AZ31 Mg alloy by a simple hydrothermal method.The effects of ASP or La organic anions on the morphologies, structures and corrosion resistance of ZnAl-LDHs were investigated by XRD, FTIR, SEM and electrochemical test systems.

    2. Experimental method

    2.1. Materials

    AZ31 Mg alloy sheets (Al:8.5-9.5 wt%, Zn:0.45-0.9 wt%, Mn: 0.17-0.4 wt%, Si <0.08 wt%, Fe<0.004 wt%, Ni<0.001 wt% and balanced Mg) with a size of 20mm×25mm×2.0mm were employed as the substrates.All the chemical reagents used in this experiment, including Zn(NO3)2·6H2O, Al(NO3)3·9H2O, C4H7NO4, C12H23NaO2,NaCl and NaOH, were analytical grade.

    2.2. Experimental Details

    Both the ZnAl-ASP-LDHs and ZnAl-La-LDHs film were synthesized by a hydrothermal method. First, the AZ31 Mg alloys were ground with 400, 800, 1200, and 2000 grit SiC sand paper, ultrasonically cleaned in ethanol for 15 minutes and dried by cold air, respectively. Then, in order to remove impurities and oxides on the substrate surface, the Mg sheets were immersed in 0.2 M NaOH solution for ultrasonic cleaning for 1 minute, and placed in a 333K oven for drying after ultrasonically washed with ethanol for 10 minutes. In a typical synthesis, 0.04 M Zn(NO3)2·6H2O and 0.02 M Al(NO3)3·9H2O were dissolved in deionized(DI)water to form a homogeneous solution under nitrogen atmosphere, then the above mixture was added dropwise to 0.04 M C4H7NO4and 0.04 M C12H23NaO2solution, respectively.The pH was adjusted to 10.0 by addition 2 M NaOH solution during the synthesis process. The above two turbid liquids obtained and the pretreated Mg sheets were separately transferred to PTFE autoclave and heated to 393K for 12h. After the reaction, the Mg sheets were washed with DI water and vacuum dried at 333 K for 12h. Finally, the ZnAl-La-LDHs and ZnAl-ASP-LDHs film were obtained.

    2.3. Characterization and measurements

    The morphology of the samples was characterized by scanning electron microscopy (SEM, JEOL JSM-7800F) equipped with an energy dispersive X-ray spectrometer (EDS). The crystal structure of the film was tested using a powder Xray diffraction (XRD).The XRD instrument is Rigaku D/max 2500 type X-ray diffractometer (Cu Ka, λ=0.1540598nm,50kV/250MA) at a scanning rate of 0.02s-1in the scanning range of 5°-75°. The functional groups on the film surface were analyzed using a Fourier transform infrared spectrometer(Nicolet iS50).

    2.4. Electrochemical test

    The polarization curves and electrochemical impedance spectroscopy (EIS) were used to judge the corrosion resistance of the coating, which were performed by an electrochemical workstation (CHI760E, Shanghai Chenhua) in a 3.5 wt.% NaCl solution at room temperature (RT). A classic three-electrode system was applied, in which the sample (area 1cm2) is used as the working electrode, a platinum plate as the counter electrode and saturated calomel electrode (SCE)as a reference electrode. Prior to measurement, the working electrode was immersed in 3.5 wt.% NaCl solution until the open circuit voltage was stable. In order to obtain stable output electrical signal, the electrochemical test usually starts after the samples have been immersed the solution for 30 minutes. The potentiodynamic polarization curve was recorded at a scan rate of 2mV/s. The EIS measurements were carried out from 100mHz to 100kHz with an amplitude disturbance of 5mV.

    3. Results and discussion

    3.1. Morphology, composition and structure of the ZnAl-LDHs films intercalated with ASP and La anions

    The SEM images and EDS spectra of ZnAl-ASP-LDHs and ZnAl-La-LDHs film are given in Fig. 1. It shows that both the two LDHs film densely grow on Mg alloy(Fig. 1a and 1b), and exhibit a uniform and dense NSs structure (Fig. 1c and 1d). Both the NSs of the ZnAl-ASP-LDHs and ZnAl-La-LDHs film are alternately staggered on Mg alloy, but the NSs of the latter film (Fig. 1d) are larger in size, slanted stagger, more uniform and denser, which can more effectively block the penetration of aggressive ions and prevent the substrate from being exposed to aggressive environments, thereby improving the corrosion resistance of the Mg alloy. From the cross-section SEM diagrams (Fig. 1e, f),the thickness of ZnAl-ASP-LDHs film and ZnAl-La-LDHs film were obtained to be 15.65 and 17.39μm, respectively.The thicker the films the more resistant to the infiltratio of aggressive Cl- to the substrate, consequently ZnAl-La-LDHs film have better ability to protect the Mg alloy.

    The chemical composition of ZnAl-LDHs film intercalated with ASP and La anions was analyzed by EDS and the results were shown in Fig.1e and 1f. It can be seen that the main components of the both two ZnAl-LDHs film (Fig. 1e)are Zn, Al, C, N and O elements, the content of Mg is mainly derived from the substrate. The organic anions are mainly composed of C, O and H elements. Although there are a large number of these elements in the air, the C and O peak intensities of ZnAl-LDHs film intercalated with organic ASP and La are significantl stronger than those of the corresponding ZnAl-LDHs film intercalated with inorganic anions in our previous work [26]. This indicates that the ASP and La were successfully embedded in ZnAl-LDHs film on Mg alloys.

    The XRD patterns of the Mg alloy substrate, ZnAl-ASPLDHs film and ZnAl-La-LDHs film were displayed in Fig. 2. It reveals that the typical (003) and (006) layered characteristic peaks of LDHs appear in the XRD pattern of ZnAl-ASP-LDHs films but only (006) (2θ≈5.2°) and (009)(2θ≈7.8°) peaks occur in ZnAl-La-LDHs films According to the report of Y.H. Cao and F.Z. Zhang, the characteristic peak of (003) is estimated to be between 0~5° [28,23]. Due to the limitation of the detection range of our XRD instrument,it is impossible to accurately measure the diffraction peak of 0~5°, so the (003) peaks for ZnAl-La-LDHs film was not observed. Our results of (006) and (009) characteristic peaks of ZnAl-La-LDHs film are consistent with the reports of Yarger and Whilton [29,30], indicating that the layered ZnAl-La-LDHs were successfully prepared on Mg alloy.

    According to the Bragg equation, the crystalline interplanar spacing of d(003)of ZnAl-ASP-LDHs film was calculated to be 0.824nm. Since the (003) peak of ZnAl-La-LDHs film shifts to a smaller 2θ angle, its d(003)spacing should be much larger than 0.824nm, meaning that the ZnAl-LDHs intercalated with different anions will have different layer spacing and the one intercalated with La has larger spacing than that with ASP, this may be related to the order of the interlayer anions and the size of the anions [31].

    Fig. 1. SEM images, cross-sectional views and the corresponding EDS spectra of ZnAl - ASP - LDHs (a, c and e) and ZnAl-La-LDHs(b, d and f) films

    The FT-IR spectra of ZnAl-ASP-LDHs and ZnAl-La-LDHs film are shown in Fig. 3. The absorption band at 3694cm-1is attributed to the lattice vibration of M-OH in the LDHs laminate (e.g. Zn-OH, Al-OH, and Mg-OH) [32]. The band at about 3450cm-1corresponds to O-H due to water molecules absorbed on the surface and interlayer water molecules. The band at 1637cm-1can be ascribed to the bending vibration of water molecules. The characteristic absorption band at 1378cm-1of ZnAl-ASP-LDHs film is caused by the asymmetric and symmetric tensile vibration of -COOH group [33].In the ZnAl-La-LDHs films the spectra at 2849cm-1and 2918cm-1are attributed to the tensile vibration of the alkyl C-H group, and the absorption peak at 1409cm-1is related to the symmetrical and asymmetric vibration of the COOgroup [28]. These results show that the ASP and La anions are successfully intercalated into the ZnAl-LDHs films In addition, there are some absorption peaks at 472 cm-1, which may be related to the lattice vibration of the metal (e.g.M-O, M-O-M) [34]. From the above FT-IR spectra, it was further confirme that the ZnAl-LDHs film intercalated with ASP and La anions have been successfully prepared on Mg alloy.

    3.2. Corrosion resistance of the ZnAl-LDHs films intercalated with ASP and La anions

    The potentiodynamic polarization curves of AZ31 Mg alloy, ZnAl-ASP-LDHs and ZnAl-La-LDHs film immersed in 3.5 wt.% NaCl aqueous solution are demonstrated in Fig.4, and the corresponding results are listed in Table 1.It shows that the corrosion potential (Ecorr) of AZ31 Mg alloy bare substrate,ZnAl-ASP-LDHs and ZnAl-La-LDHs film are -1.511V, -1.503V and -1.074V (vs. SCE), respectively, indicating that ZnAl-La-LDHs film have the highest Ecorr, then the best corrosion resistance. The corrosion current density (icorr) of bare AZ31 Mg alloy, ZnAl-ASPLDHs and ZnAl-La-LDHs film decreases from 7.472×10-5to 2.772×10-7A/cm2. Compared with the icorrof the substrate, the icorrof the ASP and La -contained ZnAl-LDHs film are reduced by two orders of magnitude.It is known that the less icorr, the slower the interface reaction, the better corrosion resistance, means that the samples coated with ZnAl-ASP-LDHs or ZnAl-La-LDHs have better anti-corrosion performance. Meanwhile, their icorrvalues were compared with that of ZnAl-NO3--LDHs film reported in our previous work[26], and it is found (from in Table 1) that the corrosion resistance of the film ZnAl-LDHs film intercalated with organic ASP/La anion is much better. These results illustrate that the ZnAl-LDHs film intercalated with ASP/La prepared by one-step in situ method can effectively improve the corrosion resistance of the AZ31 Mg alloy.

    Table 1 The polarization measurements(corrosion potential (Ecorr) and corrosion current densities (icorr)) of the magnesium alloy substrate, ZnAl-ASP-LDHs, ZnAl-La-LDHs and ZnAl-NO3--LDHs films

    Fig. 2. XRD patterns of the magnesium alloy substrate, ZnAl-ASP-LDHs and ZnAl-La-LDHs films

    Fig. 3. FT-IR spectra of ZnAl-ASP-LDHs and ZnAl-La-LDHs films

    Fig. 4. Potentiodynamic polarization curves of the magnesium alloy substrate, ZnAl- ASP- LDHs and ZnAl-La-LDHs films

    Electrochemical impedance spectroscopy (EIS) was also used to evaluate the anticorrosion behaviors of the LDHs films The Nyquist plot is shown in Fig.5a, from which one clear loop could be observed for our three samples and the order of the radius of curvature is ZnAl-La-LDHs >ZnAl-ASP-LDHs >AZ31 alloy. Usually the larger the curvature radius, the better the corrosion resistance, so it indicates that the two ZnAl-LDHs increase the corrosion property of AZ31 alloy, and the ZnAl-La-LDHs has the better anti-corrosion performance than ZnAl-ASP-LDHs.

    The Bode plot is displayed in Fig.5b, from which a clear peak at high-mid frequency and a weak peak at low frequency were found, indicating that two time constants exist in the phase angle plot, which are corresponding to two capacitive loops.Similar results about the bare substrate and LDHs film were also reported in previous researches [21,27].

    Fig. 5. Nyquist (a) and Bode (b) plots of the magnesium alloy substrate, ZnAl-ASP-LDHs and ZnAl-La-LDHs films

    Table 2 Fitting results of EIS spectrum for magnesium alloy substrate, ZnAl-ASP-LDHs and ZnAl-La-LDHs films

    Fig. 6. The equivalent electrical circuit of ZnAl-LDHs films

    Based on the above results, the proposed equivalent electrical circuit of ZnAl-LDHs film is exhibited in Fig. 6, in which Rsis the solution resistance, RCTis the charge transfer resistance and the constant phase element (CPEDL) is the electric double layer capacity and RLrepresents the fil resistance and CPELrepresents the fil capacity. Based on the equivalent circuits, the EIS spectra were fitte and the data fittin results listed in Table 2. It shows that the RCTvalue of the bare AZ31 substrate is only 61.36Ωcm2, which is much lower than that of the ZnAl-ASP-LDHs (9841Ωcm2)and ZnAl-La-LDHs (1.409×104Ωcm2). The CPEDLvalues of the bare AZ91substrate is 22.76μFcm-2, which is higher than that of the ZnAl-ASP-LDHs(0.7179μFcm-2)and ZnAl-La-LDHs (0.0813μFcm-2). It indicated that the ZnAl-LDHs film play an important role in improving the protection performance of the Mg alloy.

    It is generally believed that the higher RCT, the lower CPEL, the better anticorrosion performance [21,27]. Compared with the RCTand CPEDLvalues of the LDHs film with different anions, it also suggested that their corrosion resistance should be: ZnAl-La-LDHs >ZnAl-ASP-LDHs >AZ 31 alloy, which is consistent with the results of the Nyquist plot (Fig.5a).

    3.3. Morphology and composition of the ZnAl-LDHs films after immersion

    The ZnAl-ASP-LDHs and ZnAl-La-LDHs film were immersed in a 3.5 wt.% NaCl solution for 168h. Then the morphology and composition of the samples were measured. The SEM images were shown in Fig.7. From the photos with lower magnificatio (Fig.7a and b), it can be seen that the surface of ZnAl-LDHs film intercalated with ASP and La on the Mg alloy looks very flat no obvious corrosion marks were observed after corrosion. At larger magnification the surface of ZnAl-ASP-LDHs film (Fig.7c and e) seems still very smooth,which is attributed to the dissolution of the LDH NSs, and the dissolved product are evenly covered on the surface of Mg alloy, which can effectively slow down the corrosion of Mg alloy. Compared with the SEM imagines of ZnAl-La-LDHs film before corrosion (Fig.1b and d), it can be seen from Fig.7d and f that the complete NSs structure still exists and uniform and densely covers on Mg alloy after corrosion, the only change is the NSs structure transforming from oblique staggered to vertical staggered, resulting from the anion exchange of Cl-during the corrosion process, indicating that the ZnAl-La-LDHs film can absorbs Cl-in the corrosion solution to protect the Mg alloy.

    Fig. 7. SEM images and the corresponding EDS spectra of the ZnAl-ASP-LDHs (a, c and e) and ZnAl-La-LDHs (b, d and f) film after corrosion.

    The chemical compositions of the samples after the immersion experiment were shown in Fig. 7e and f. Compared with the pre-etched films the immersed ZnAl-LDHs film have Cl element after corrosion, which is attributed to the fact that the organic anion contained ZnAl-LDHs can effectively absorb and retain the aggressive Cl-between the interlayer, this result is consistent with the findin of the previous experiments[26].

    As shown in Fig. 8, the FT-IR spectrum of the samples after immersion reveals that after the corrosion, the absorption band of the ASP/La anions is still present, which indicates that the structure of film can effectively resist corrosion, but the intensity of absorption band at 3694cm-1of ZnAl-La-LDHs film is obviously stronger than that of ZnAl-ASP-LDHs films The 3694cm-1band is usually ascribed to the precipitation of Mg(OH)2,so the weaker intensity of 3694cm-1band of ZnAl-La-LDHs film means that the Mg(OH)2precipitate formed from ZnAl-La-LDHs film after corrosion is less than that of ZnAl-ASP-LDHs films which implying that the La contained ZnAl-LDHs film has better corrosion resistance.

    Fig. 8. FT-IR spectra of the ZnAl-ASP-LDHs and ZnAl-La-LDHs film after corrosion.

    3.4. Anti-corrosion mechanism of ZnAl-LDHs films with ASP and La anions

    Based on the above analysis, the anticorrosion mechanism of the Zn-Al LDHs film with different anions could be depicted as follows: (1) the ZnAl-LDHs film with high density of nanosheets act as a protective barrier coating to block the direct contact of the chloride anions to Mg alloys,which delay the initiation of the corrosion; (2) due to the anion-exchange of LDHs, the intercalated ASP or La anions exchange with the aggressive chloride anions, means, the harmful chlorides are entrapped and its concentration will decrease; (3) the released ASP or La anions in the aggressive environment can form a corrosion inhibitor protective layer on the surface of Mg alloy. This process is usually also called as self healing. In a short word, the ASP or La-intercalated Zn-Al LDHs film play three roles to enhance the improve corrosion resistance: barrier coating, the entrapment of harmful chlorides and the formation of inhibition protective layer. Our proposed mechanism is accordance with the results of Tedim,et al.[35].Schematic diagram of ion exchange of ASP or La anions with Cl-and formation of corrosion inhibition protective layer on Mg alloy is demonstrated in Fig. 9.

    Eddy [36,37] and Sorkhabi et al. [38] reported that corrosion inhibition efficien y of organic compounds is dependent on the molecule structure (molecular size, molecular mass,internal structure, the nature and adsorptive tendencies of the hetero-atoms) and the number of adsorption-active centers usually originating from some functional groups. The ASP molecular (C4H7NO4) has three polar groups (one -N2H and two -OH), means, it has three active adsorption sites. The structural formula of the La molecule (C12H24O2) is HOOC-10CH2-COOH, which has two active adsorption sites (two polar groups: one -CH3 and one -OH), implying that La have one less active adsorption sites than ASP. On the other hand, the molecular weight (MW) of La (200.32) is larger than that of ASP (MW:133.1). Usually the larger the MW or the more adsorption sites, the better the corrosion inhibition efficien y. So it is hard to judge ASP or La, which one have a better the corrosion inhibition efficien y, since the effect of the more active adsorption sites of ASP offsets against its lighter MW.

    Fig. 9. Schematic diagram of ion exchange of organic ions and formation of corrosion inhibition protective layer on Mg alloy (Inh=ASP or La).

    More importantly, the larger molecule size of La caused the larger d(003)spacing of the ZnAl-La-LDHs, resulting in a better ability to absorb Cl-and release interlayer anions than ZnAl-ASP-LDHs.Meanwhile the NSs of ZnAl-La-LDHs film stagger slanted and are thicker, denser and more uniform, which can more effectively block the penetration of aggressive ions and prevent the substrate from being exposed to aggressive environments.

    Therefore, owing to the total effect of the above comprehensive factors, the ZnAl-La-LDHs film shows better anticorrosion property than the ZnAl-ASP-LDHs films

    3.5. Comparison of corrosion resistance of ZnAl-DHs films with different organic anions

    The corrosion resistance of ZnAl -LDHs film intercalated with different organic anions is briefl compared and the result is given in Table 3. It is found that the corrosion potential of LDH coating is in the range of -1.50— 0.90V, and the corrosion current density of the metal substrate is tens of μA/cm2, ie, at the 10-5A/cm2order of magnitude; and the corrosion current density of the LDH coating is usually at the 10-5~10-9A/cm2order of magnitude, indicating LDH coating can greatly increase the corrosion resistance. Among the LDHs intercalated with organic anions,the La-intercalated ZnAl-LDH coatings fabricated by Zhang et al.[23]on Al alloy got the lowest corrosion current density (~10-9A/cm2). The

    Table 3 Comparison of corrosion resistance of ZnAl-DHs film intercalated with different anions (corrosion solution: 3.5wt.% NaCl).

    corrosion current density of the ZnAl-ASP-LDH and ZnAl-La-LDH prepared in this work is lower than that of the MgAl-PA-LDH deposited by Chen et al.[16],but near that of MgAl-ASP-LDH reported in our previous work [27], implying that our ASP- or La-intercalated ZnAl-ASP-LDH have better corrosion resistance than the PA-intercalated MgAl-LDH and almost the same corrosion resistance to the ASP-intercalated MgAl-LDH.

    4. Conclusions

    In this paper, the ZnAl-ASP-LDHs and ZnAl-La-LDHs film were prepared by the hydrothermal method on AZ31 Mg alloy. The effects of different organic anions on the morphology, structure and corrosion resistance of ZnAl-LDHs film were investigated. It was found that both ZnAl-ASP-LDHs and ZnAl-La-LDHs film grow uniformly and densely on AZ31 Mg alloy. The ZnAl-ASP-LDHs film exhibited a vertical growth of NSs structure, while the ZnAl-La-LDHs film showed mutual interlaced tilted NSs structure, which is more conducive to block the penetration of corrosive liquid into the Mg alloy. The ZnAl-La-LDHs has a much larger d(003)spacing value than ZnAl-ASP - LDHs, indicating that ZnAl-La-LDHs film have better ability to absorb Cl-and release interlayer anions. The corrosion resistance of ZnAl-La-LDHs film is obviously better than that of ZnAl-ASP-LDHs films and the corrosion current density (2.772×10-7A/cm2) is reduced by two orders of magnitude compared to that of bare Mg alloy (7.482×10-5A/cm2). The morphology still shows a uniform and dense complete NSs structure after corrosion,which indicates that the ZnAl-LDHs film intercalated with organic La anions can significantl improve the corrosion resistance of Mg alloy.

    Acknowledgments

    This work was supported by the Natural Science Foundation of Chongqing (cstc2019jcyjmsxmX0566, cstc2018jcyjAX0450, cstc2018jcyjA2923,cstc2017jcyjAX0393), Projects of President Foundation of Chongqing University (2019CDXZWL002), Fundamental Research Funds for the Central Universities (2019CDXYWL0029, 2018CDJDWL0011,106112017CDJQJ328839, 106112016CDJZR288805), Science and Technology Research Program of Chongqing Municipal Education Commission (KJKJQN201800102,KJQN201800619, KJ1703042), NSFC (11544010, 11374359,11304405 and 1155305),the Sharing Fund of Large-scale Equipment of Chongqing University (201903150094). We also thank Analytical and Testing Center of Chongqing University for performing XRD, XPS, TEM tests.

    一边摸一边抽搐一进一出视频| 国产色婷婷99| 狠狠精品人妻久久久久久综合| 国产免费视频播放在线视频| 久久ye,这里只有精品| svipshipincom国产片| 少妇的丰满在线观看| 国产熟女午夜一区二区三区| 久久久亚洲精品成人影院| 看十八女毛片水多多多| 久久久欧美国产精品| 精品视频人人做人人爽| 国产精品久久久av美女十八| 国产色婷婷99| 亚洲国产毛片av蜜桃av| 亚洲av成人不卡在线观看播放网 | 精品少妇黑人巨大在线播放| 免费在线观看完整版高清| 无遮挡黄片免费观看| 极品少妇高潮喷水抽搐| 久久久久久人人人人人| 亚洲成人一二三区av| 亚洲av综合色区一区| 亚洲精品成人av观看孕妇| 最近2019中文字幕mv第一页| 国产 精品1| 日韩欧美精品免费久久| 欧美另类一区| 777米奇影视久久| 亚洲av福利一区| 欧美日韩亚洲国产一区二区在线观看 | 秋霞伦理黄片| 欧美黑人精品巨大| 亚洲精品一区蜜桃| 搡老岳熟女国产| 天天影视国产精品| 免费少妇av软件| 精品一区二区三卡| 午夜免费观看性视频| 少妇被粗大的猛进出69影院| 久久精品熟女亚洲av麻豆精品| 国产精品久久久av美女十八| 精品国产一区二区三区四区第35| 在线观看免费视频网站a站| 精品人妻在线不人妻| 人妻 亚洲 视频| 日韩一区二区视频免费看| av视频免费观看在线观看| 国产成人一区二区在线| 国产一区二区激情短视频 | 男男h啪啪无遮挡| 最近手机中文字幕大全| 中文乱码字字幕精品一区二区三区| 美女国产高潮福利片在线看| 亚洲国产精品成人久久小说| 在线免费观看不下载黄p国产| 欧美日韩av久久| 99热全是精品| 三上悠亚av全集在线观看| 高清在线视频一区二区三区| 免费少妇av软件| 国产又色又爽无遮挡免| 日本黄色日本黄色录像| 免费高清在线观看日韩| 国产免费福利视频在线观看| 亚洲av欧美aⅴ国产| 在线观看免费日韩欧美大片| 国产一区二区三区av在线| 精品一区二区三区四区五区乱码 | 免费不卡黄色视频| av有码第一页| 欧美最新免费一区二区三区| 久久人妻熟女aⅴ| 久久天躁狠狠躁夜夜2o2o | 婷婷色综合大香蕉| 极品人妻少妇av视频| 美女扒开内裤让男人捅视频| svipshipincom国产片| 天堂8中文在线网| 亚洲精品av麻豆狂野| 欧美日韩国产mv在线观看视频| 亚洲欧美清纯卡通| 曰老女人黄片| 最近的中文字幕免费完整| 亚洲精品中文字幕在线视频| 九九爱精品视频在线观看| 日韩视频在线欧美| 成人午夜精彩视频在线观看| 欧美人与善性xxx| 看十八女毛片水多多多| 黄频高清免费视频| 日本午夜av视频| 成人国语在线视频| av天堂久久9| 99久久综合免费| 97人妻天天添夜夜摸| 国产精品蜜桃在线观看| 天天躁狠狠躁夜夜躁狠狠躁| 考比视频在线观看| 国产成人精品福利久久| 国产有黄有色有爽视频| 纵有疾风起免费观看全集完整版| 91国产中文字幕| e午夜精品久久久久久久| 日本猛色少妇xxxxx猛交久久| 精品少妇久久久久久888优播| netflix在线观看网站| 最近2019中文字幕mv第一页| 欧美成人精品欧美一级黄| 国产一区有黄有色的免费视频| 亚洲视频免费观看视频| 欧美人与善性xxx| 男女下面插进去视频免费观看| 如日韩欧美国产精品一区二区三区| 极品人妻少妇av视频| 激情五月婷婷亚洲| 久久青草综合色| 五月天丁香电影| 国产成人欧美| 国产亚洲av片在线观看秒播厂| 少妇被粗大的猛进出69影院| 国产免费现黄频在线看| 亚洲激情五月婷婷啪啪| 亚洲欧美成人综合另类久久久| 亚洲国产中文字幕在线视频| 亚洲av福利一区| 搡老乐熟女国产| 亚洲成人手机| 水蜜桃什么品种好| 狠狠精品人妻久久久久久综合| 亚洲国产毛片av蜜桃av| 亚洲,欧美,日韩| 丝袜美腿诱惑在线| 国产精品国产三级专区第一集| 男人操女人黄网站| 中文字幕色久视频| 搡老乐熟女国产| 日日摸夜夜添夜夜爱| 欧美精品亚洲一区二区| 亚洲av在线观看美女高潮| 久久狼人影院| 黄色视频不卡| 亚洲精品日韩在线中文字幕| 国产精品秋霞免费鲁丝片| 久久久久精品国产欧美久久久 | 亚洲第一av免费看| 十八禁网站网址无遮挡| 国产精品av久久久久免费| 日韩大码丰满熟妇| 七月丁香在线播放| 久久青草综合色| 国产精品一区二区精品视频观看| 成年av动漫网址| 亚洲欧美成人精品一区二区| 中文字幕人妻丝袜制服| 亚洲熟女精品中文字幕| 一级毛片 在线播放| 亚洲国产精品一区三区| 高清欧美精品videossex| 久久久久久免费高清国产稀缺| 国产精品久久久av美女十八| 伦理电影大哥的女人| 汤姆久久久久久久影院中文字幕| av片东京热男人的天堂| 中国国产av一级| 一本大道久久a久久精品| 热re99久久精品国产66热6| tube8黄色片| 国产探花极品一区二区| 免费女性裸体啪啪无遮挡网站| 国产 一区精品| 成年女人毛片免费观看观看9 | 亚洲第一av免费看| 亚洲国产日韩一区二区| 男的添女的下面高潮视频| 久久久久视频综合| 国产不卡av网站在线观看| 亚洲国产精品999| 成人亚洲欧美一区二区av| 又大又爽又粗| 中国三级夫妇交换| av国产精品久久久久影院| 久久人人爽人人片av| 亚洲欧美色中文字幕在线| 国产精品.久久久| 18在线观看网站| 日韩av免费高清视频| 精品久久久精品久久久| 另类精品久久| 成人午夜精彩视频在线观看| 99精国产麻豆久久婷婷| 亚洲一卡2卡3卡4卡5卡精品中文| 午夜久久久在线观看| 婷婷色综合www| 久久人人97超碰香蕉20202| 亚洲成av片中文字幕在线观看| 美女大奶头黄色视频| 日韩大片免费观看网站| 少妇猛男粗大的猛烈进出视频| 欧美精品亚洲一区二区| 极品少妇高潮喷水抽搐| 女性生殖器流出的白浆| 国产黄频视频在线观看| 免费久久久久久久精品成人欧美视频| 国产精品久久久久成人av| 飞空精品影院首页| 亚洲,欧美精品.| 在线看a的网站| 七月丁香在线播放| av卡一久久| 亚洲精品成人av观看孕妇| 搡老岳熟女国产| 最近中文字幕2019免费版| 亚洲天堂av无毛| 男女高潮啪啪啪动态图| 亚洲精品国产av成人精品| 熟妇人妻不卡中文字幕| 男女床上黄色一级片免费看| 亚洲av中文av极速乱| 一级片'在线观看视频| 9191精品国产免费久久| 国产成人欧美| 蜜桃在线观看..| 中文天堂在线官网| 久久久久视频综合| av电影中文网址| 成年av动漫网址| 男女床上黄色一级片免费看| 日韩av在线免费看完整版不卡| 色吧在线观看| av国产久精品久网站免费入址| 晚上一个人看的免费电影| 另类亚洲欧美激情| 男女下面插进去视频免费观看| 国产精品人妻久久久影院| 亚洲精品国产av成人精品| 97在线人人人人妻| 老汉色av国产亚洲站长工具| 成人黄色视频免费在线看| 欧美国产精品一级二级三级| 免费在线观看视频国产中文字幕亚洲 | 男女无遮挡免费网站观看| 中文字幕人妻丝袜制服| 亚洲av男天堂| 9191精品国产免费久久| 韩国精品一区二区三区| 人人妻人人澡人人爽人人夜夜| 99香蕉大伊视频| 黑人欧美特级aaaaaa片| 一边摸一边做爽爽视频免费| 国产av一区二区精品久久| 天堂中文最新版在线下载| 日韩中文字幕视频在线看片| 女人爽到高潮嗷嗷叫在线视频| 99久久人妻综合| av有码第一页| 久久久精品国产亚洲av高清涩受| 少妇猛男粗大的猛烈进出视频| 国产成人欧美| 捣出白浆h1v1| 亚洲一卡2卡3卡4卡5卡精品中文| 人人妻人人澡人人看| 精品一区二区三区四区五区乱码 | 久久人人97超碰香蕉20202| 在线观看www视频免费| 亚洲精品,欧美精品| 视频区图区小说| 国精品久久久久久国模美| 晚上一个人看的免费电影| 欧美人与善性xxx| 亚洲一卡2卡3卡4卡5卡精品中文| 国产成人av激情在线播放| 建设人人有责人人尽责人人享有的| 午夜免费观看性视频| 久久久久久久久久久久大奶| 亚洲国产中文字幕在线视频| 黄色视频在线播放观看不卡| 成人午夜精彩视频在线观看| 电影成人av| 久久午夜综合久久蜜桃| 国产日韩欧美视频二区| 免费看不卡的av| av在线观看视频网站免费| 两个人看的免费小视频| 亚洲熟女毛片儿| 欧美老熟妇乱子伦牲交| 午夜日本视频在线| √禁漫天堂资源中文www| 久热爱精品视频在线9| 国产一卡二卡三卡精品 | 国产精品 欧美亚洲| 久久久久国产精品人妻一区二区| 亚洲精品一二三| 国产成人精品久久二区二区91 | 丰满少妇做爰视频| 男女午夜视频在线观看| 免费观看av网站的网址| 日韩中文字幕视频在线看片| 免费在线观看视频国产中文字幕亚洲 | 精品免费久久久久久久清纯 | 国产一区二区激情短视频 | 亚洲国产成人一精品久久久| 人人妻人人爽人人添夜夜欢视频| 又大又爽又粗| 久久热在线av| 国产一级毛片在线| av有码第一页| 久久久精品国产亚洲av高清涩受| 一区二区三区乱码不卡18| 美女中出高潮动态图| 国产成人精品久久二区二区91 | 欧美日韩av久久| 亚洲欧美成人精品一区二区| 黄片无遮挡物在线观看| 日日摸夜夜添夜夜爱| 国产亚洲精品第一综合不卡| 精品国产露脸久久av麻豆| 亚洲精品乱久久久久久| 一二三四中文在线观看免费高清| 欧美日韩精品网址| 天天躁狠狠躁夜夜躁狠狠躁| 亚洲,欧美精品.| 欧美精品一区二区免费开放| 亚洲,一卡二卡三卡| 三上悠亚av全集在线观看| 久久精品人人爽人人爽视色| 女人精品久久久久毛片| 老司机在亚洲福利影院| 久久久欧美国产精品| 波多野结衣一区麻豆| 亚洲成人手机| 搡老岳熟女国产| 国产成人精品无人区| 熟女少妇亚洲综合色aaa.| 一级a爱视频在线免费观看| 91精品三级在线观看| 亚洲欧美成人综合另类久久久| 日本欧美国产在线视频| kizo精华| 免费在线观看黄色视频的| 一本久久精品| 久久毛片免费看一区二区三区| 日韩伦理黄色片| 精品久久久精品久久久| 秋霞伦理黄片| 日本色播在线视频| 午夜福利影视在线免费观看| 亚洲国产毛片av蜜桃av| 亚洲激情五月婷婷啪啪| 色视频在线一区二区三区| 人人妻,人人澡人人爽秒播 | 国产伦理片在线播放av一区| 国产黄频视频在线观看| 夜夜骑夜夜射夜夜干| 精品一区二区三卡| 美女脱内裤让男人舔精品视频| 在线观看三级黄色| 丰满饥渴人妻一区二区三| 国产精品.久久久| 亚洲欧洲日产国产| 久久久精品区二区三区| 国产高清不卡午夜福利| 午夜久久久在线观看| 中文字幕亚洲精品专区| 男女免费视频国产| 久久影院123| 午夜精品国产一区二区电影| 天堂中文最新版在线下载| 亚洲av电影在线观看一区二区三区| 韩国精品一区二区三区| 国产福利在线免费观看视频| 9色porny在线观看| 国产在线一区二区三区精| av网站免费在线观看视频| 观看美女的网站| 午夜福利视频在线观看免费| 一级,二级,三级黄色视频| 一区二区三区四区激情视频| 十八禁高潮呻吟视频| 国产免费福利视频在线观看| 中国国产av一级| 亚洲美女搞黄在线观看| 亚洲国产精品一区二区三区在线| 久久人人爽av亚洲精品天堂| 乱人伦中国视频| 亚洲av中文av极速乱| 色播在线永久视频| 青春草视频在线免费观看| 最黄视频免费看| 五月天丁香电影| 精品人妻熟女毛片av久久网站| 777米奇影视久久| 亚洲精品国产av蜜桃| 亚洲国产精品一区二区三区在线| 青春草亚洲视频在线观看| videos熟女内射| 久久性视频一级片| 高清欧美精品videossex| 国产毛片在线视频| 自拍欧美九色日韩亚洲蝌蚪91| 久久久久国产精品人妻一区二区| 五月开心婷婷网| 日本猛色少妇xxxxx猛交久久| 亚洲精品国产av蜜桃| 日韩人妻精品一区2区三区| 黄色毛片三级朝国网站| 久久久精品免费免费高清| 亚洲欧洲国产日韩| 最近的中文字幕免费完整| 香蕉丝袜av| 欧美日韩视频高清一区二区三区二| 日本欧美视频一区| 99香蕉大伊视频| 午夜激情av网站| 色网站视频免费| 综合色丁香网| 天天躁狠狠躁夜夜躁狠狠躁| 制服诱惑二区| 久久久久网色| 夫妻性生交免费视频一级片| 欧美精品av麻豆av| 亚洲成人免费av在线播放| 国产一区二区三区av在线| 久久久久网色| 性高湖久久久久久久久免费观看| 国产精品免费大片| av在线app专区| 中文欧美无线码| 老司机亚洲免费影院| 黄色视频不卡| 黑人猛操日本美女一级片| 国产精品一区二区在线观看99| 精品一区在线观看国产| 97在线人人人人妻| 国产精品一国产av| 黄色视频在线播放观看不卡| 色网站视频免费| 日本av手机在线免费观看| 巨乳人妻的诱惑在线观看| 亚洲熟女精品中文字幕| 欧美日韩精品网址| 欧美日韩亚洲综合一区二区三区_| 看免费av毛片| h视频一区二区三区| 一级毛片 在线播放| 999精品在线视频| 视频在线观看一区二区三区| 超碰成人久久| 国产在线免费精品| 欧美久久黑人一区二区| 日本欧美视频一区| 亚洲av成人精品一二三区| 秋霞在线观看毛片| 男女免费视频国产| 亚洲欧美一区二区三区久久| 1024香蕉在线观看| 十分钟在线观看高清视频www| 亚洲国产欧美日韩在线播放| 国产精品久久久久久人妻精品电影 | 国产精品女同一区二区软件| 国产xxxxx性猛交| 亚洲av成人精品一二三区| 老司机在亚洲福利影院| 岛国毛片在线播放| 青青草视频在线视频观看| 久久精品熟女亚洲av麻豆精品| 亚洲色图 男人天堂 中文字幕| 最近的中文字幕免费完整| 亚洲精品aⅴ在线观看| 各种免费的搞黄视频| 欧美成人精品欧美一级黄| 母亲3免费完整高清在线观看| 我要看黄色一级片免费的| 亚洲人成77777在线视频| 丁香六月欧美| 欧美黑人欧美精品刺激| 久久久久精品国产欧美久久久 | 欧美日韩福利视频一区二区| 精品少妇一区二区三区视频日本电影 | 国产熟女欧美一区二区| 校园人妻丝袜中文字幕| 国产又色又爽无遮挡免| 中文字幕色久视频| av线在线观看网站| 婷婷色综合大香蕉| 国产无遮挡羞羞视频在线观看| 又大又爽又粗| 最近2019中文字幕mv第一页| 国产av精品麻豆| 丁香六月欧美| 亚洲国产日韩一区二区| 日本爱情动作片www.在线观看| 国产一卡二卡三卡精品 | 老司机影院成人| 国产熟女欧美一区二区| 午夜日韩欧美国产| 在线天堂中文资源库| 9色porny在线观看| 1024香蕉在线观看| 黑人猛操日本美女一级片| 一级爰片在线观看| 中文字幕色久视频| 欧美av亚洲av综合av国产av | 伊人久久国产一区二区| 久久久久精品久久久久真实原创| 久久久精品区二区三区| 国产极品天堂在线| 久久久久精品性色| 国产成人精品久久二区二区91 | 亚洲精品久久成人aⅴ小说| 成人国语在线视频| 极品少妇高潮喷水抽搐| 一区二区av电影网| 999精品在线视频| 日本色播在线视频| 久久精品久久久久久久性| 麻豆av在线久日| 国产精品99久久99久久久不卡 | 日韩免费高清中文字幕av| 天天添夜夜摸| 卡戴珊不雅视频在线播放| 国产一区二区激情短视频 | 中文字幕另类日韩欧美亚洲嫩草| 9191精品国产免费久久| 亚洲成色77777| 欧美国产精品一级二级三级| 久久精品aⅴ一区二区三区四区| 亚洲av福利一区| 在线观看一区二区三区激情| 亚洲精品乱久久久久久| 天天影视国产精品| 国产男人的电影天堂91| 久久国产精品男人的天堂亚洲| 国产精品人妻久久久影院| 国产色婷婷99| av网站在线播放免费| 美女午夜性视频免费| 国产男女内射视频| 一区福利在线观看| 国产精品欧美亚洲77777| 国产精品国产av在线观看| 国产一区二区 视频在线| 男女床上黄色一级片免费看| 国产成人av激情在线播放| 免费在线观看完整版高清| 成人18禁高潮啪啪吃奶动态图| 另类亚洲欧美激情| 久久影院123| 欧美人与善性xxx| av在线播放精品| 久久精品人人爽人人爽视色| 国产1区2区3区精品| 国产精品.久久久| 午夜日韩欧美国产| 欧美日韩亚洲综合一区二区三区_| 高清欧美精品videossex| 国产免费福利视频在线观看| 久久精品亚洲熟妇少妇任你| 男女免费视频国产| 国产 精品1| 亚洲一区二区三区欧美精品| 亚洲欧美激情在线| 哪个播放器可以免费观看大片| 女的被弄到高潮叫床怎么办| 免费在线观看黄色视频的| 老熟女久久久| 各种免费的搞黄视频| 国产淫语在线视频| 熟女少妇亚洲综合色aaa.| 久久久欧美国产精品| 精品一区二区三区av网在线观看 | 国产淫语在线视频| √禁漫天堂资源中文www| 国产精品国产av在线观看| 我的亚洲天堂| 亚洲国产日韩一区二区| 午夜日韩欧美国产| 国产免费视频播放在线视频| 午夜影院在线不卡| 成人三级做爰电影| 免费看不卡的av| 我的亚洲天堂| 性高湖久久久久久久久免费观看| 亚洲婷婷狠狠爱综合网| 黑丝袜美女国产一区| 人妻人人澡人人爽人人| 大话2 男鬼变身卡| 亚洲精品第二区| 两性夫妻黄色片| 韩国精品一区二区三区| 亚洲免费av在线视频| 免费少妇av软件| 国产高清国产精品国产三级| 99re6热这里在线精品视频| 91精品国产国语对白视频| 黑丝袜美女国产一区| 亚洲国产精品成人久久小说| 18在线观看网站| 婷婷成人精品国产| 日本vs欧美在线观看视频| 在线观看一区二区三区激情| 国产精品 欧美亚洲| 一本一本久久a久久精品综合妖精| 中文字幕av电影在线播放| 精品国产乱码久久久久久男人| 亚洲欧美中文字幕日韩二区| 亚洲精品日韩在线中文字幕| 在线观看www视频免费| 日本wwww免费看| 欧美在线黄色| 成人影院久久| www.av在线官网国产| 日韩免费高清中文字幕av| 母亲3免费完整高清在线观看| 免费看av在线观看网站|