    Effect of lithium content on the mechanical and corrosion behaviors of HCP binary Mg-Li alloys

    2021-05-21 03:32:56ChuanqiangLiYibinHeHuaipeiHuang
    Journal of Magnesium and Alloys 2021年2期

    Chuanqiang Li, Yibin He, Huaipei Huang

    School of Materials and Energy, Guangdong University of Technology, Guangzhou 510006, China

    Received 4 December 2019; received in revised form 3 January 2020; accepted 13 February 2020

    Available online 29 September 2020

    Abstract

    Keywords: Mg-Li alloys; Recrystallization; Texture; Mechanical properties; Corrosion behavior.

    1. Introduction

    Alloying Mg with the lightest metal element of Li(0.53g/cm3) could be further lightweight, allowing for an increase in plasticity [1-6]. The ultra-lightweight structured Mg-Li alloys presented significan promise in automotive,aerospace and electronics [5,6]. Compared with traditional hexagonal close-packed (HCP) Mg alloys, the Mg-Li system exhibited different crystal structure based on the lithium content, which was unique in comparison to other alloying addition to Mg. The stable room-temperature phase of Mg-Li alloy was: i) a hexagonal close-packed (HCP) α-Mg with less than 5.5 wt% Li; ii) a body centered cubic (BCC) β-Li with more than 10.3 wt% Li; and iii) a duplex (α-Mg+β-Li)structure between 5.5 wt% and 10.3 wt% Li [7,8]. However,the mechanical strength and corrosion resistance of Mg-Li alloys were generally inferior to the Mg alloys without lithium[9-13].

    As for the strengthening strategies of metal materials, the mechanical processing (extrusion, rolling, forging, etc.) was the common approach to optimize microstructure with the fin gains and/or broken second phases [14-17]. Regarding of Mg alloys,the deforming Mg alloys always exhibited strong basal textures, making the c-axis of most grains nearly parallel to the normal direction (ND) of the sheet [18-20]. However, the lithium addition could weaken the basal texture of Mg alloys as the rotation of basal plane to the transverse direction would be promoted by the decreased c/a ratio of Mg-Li alloys [13,21-23]. Compared with AZ31 alloy, Mg-4Li alloy possessed weak basal (0002) and prismatic (10-10) texture at the same cold-rolling reduction [13]. Previous works reported that the addition of Li could restrained the 〈a〉 basal slip and promoted the 〈a〉 prismatic slip of hexagonal Mg-Li alloys [24-26]. For example, lower critical resolved shear stress (CRSS) in the 〈a〉 prismatic slip and higher in the〈a〉 basal slip occurred in the Mg-4 wt% Li single crystals[24]. Agnew et al. demonstrated that the 〈c+a〉 pyramidal slip in Mg alloys could be activated by the adding lithium[25]. At the same time, the increase of 〈c+a〉 pyramidal slip could lead to the enhanced ductility of Mg alloys, which was proved by the viscoplastic self-consistent simulations [25].To confir the former studies, abundant uniformly distributed〈c+a〉 dislocations of deformed Mg-Li alloys were found by transmission electron microscopy(TEM)[26].Compared with a conventional magnesium AZ31 alloy, Al-Samman reported that lithium addition to magnesium (Mg-4 wt% Li) exhibited remarkable room temperature ductility improvement owing to enhanced activity of non-basal slip, particularly, <c+a>-slip mode [13]. Many reports had focused on the texture evolution of α-Mg phase in Mg-Li alloys, and the results showed that the addition of Li weakened (0001) basal texture and increased the deflectio of basal planes along normal direction to rolling direction or transverse direction, which was associated with the activation of non-basal slip systems and the formation of DRX grains [21,27-29]. Recently, Li and Xu revealed the different effect of quasicrystal phases on the crystal texture and mechanical of three typical Mg-Li alloys(HCP, HCP+BCC and BCC) [30-32]. However, so far, few reports could be referred to clarify the effect of lithium concentration on the texture and/or mechanical behaviors on the single Mg-Li system (HCP, HCP+BCC or BCC).

    Compared with massive reports on the mechanical properties of Mg-Li alloys, the research on the corrosion behaviors of strengthening Mg-Li alloy was deficien to date. It was well known that lithium was much more electrochemical/chemical active than magnesium, the addition of Li into multicomponent Mg matrix could further deteriorate the integrity of Mg matrix in aqueous solution and caused a worse corrosion resistance than conventional Mg alloys [33-35]. To improve the corrosion resistance of Mg-Li alloys, regulating the matrix microstructure (alloying, second phases, deformation, heat treatment) and surface modificatio were the common methods [36-40]. For example, the formation of I-phase by alloying with a certain Zn/RE ratio could effectively retard the corrosion proceeding of as-cast Mg-6Li alloy and the corrosion resistance of Mg-8.8Li alloy was improved remarkably by the phosphate conversion fil [36,37]. Recently,high-corrosion-resistant Mg alloy was reported in Mg-Li system, which was ascribed to the protective and self-healing Li2CO3fil deposited on the surface [41-46]. Li et al. reported that corrosion resistance of binary BCC Mg-14Li alloy was enhanced with immersion time in 0.1M NaCl solution and always higher than those of HCP Mg-4Li and HCP+BCC Mg-7.5Li alloys[43].Following this hypothesis,the corrosion behaviors or surface fil of Mg-Li alloys should be correlated closely with lithium concentration,implying the possible difference of corrosion resistance for HCP Mg-Li alloys with different lithium content. On the other hand, it seems that the effect of lithium concentration on the mechanical and corrosion performance of Mg-Li alloys can not be covered for all the Mg-Li system as their crystallographic structure would be altered with lithium content. As a result, it was necessary and significan to separate the HCP, HCP+BCC and BCC Mg-Lialloys and elucidated the concrete effect of lithium content on the mechanical and corrosion behaviors for each Mg-Li system.

    Table 1 Chemical composition of Mg-Li alloys in experiment.

    Based on the aforementioned descriptions and analysis, to deepen the fundamental understanding on the mechanical and corrosion behaviors of Mg-Li alloys, binary HCP Mg-Li alloys was used herein to isolate the effects of additional alloying elements and crystallographic structure. Moreover, the underneath failure mechanisms of tension and corrosion for HCP Mg-Li alloys with different lithium content would be characterized and compared in detail.

    2. Material and methods

    2.1. Materials and microstructural analysis

    The initial materials used herein were as-extruded Mg-1Li,Mg-3Li and Mg-5Li (in wt.%) alloys plates whose chemical composition was determined by inductively coupled plasma atomic emission spectrum (ICP-AES) apparatus and the results were shown in Table 1. After casting, the ingots were homogenized at 400°C for 6h with the protection of several layers of wrapped Al foil.Then,the ingots were extruded into thick plate with cross section of 12mm×50mm at 300°C,with an extrusion ratio of about 6.5. Sample pieces cut from the extruded plates were ground with SiC papers up to 5000 grit finis and then finel polished up to a 1μm finis with ethanol.

    Microstructure of the alloys were observed by optical microscopy (OM), scanning electron microscopy (SEM; JEOL JSM-IT100) and electron back-scattering diffraction (EBSD).To reveal the difference of grain structure between the alloys,polished samples were etched with 5%nitric acid+95%ethanol.Average grain size was determined by using the mean linear intercept method. Distributed intensity of the (0002),(11-20) and (10-10) pole figure for the three alloys were measured by EBSD analysis. For EBSD tests, one surface of the sample was mechanically polished and followed by electropolishing in a commercial electrolyte (AC2). EBSD analyses were conducted on a scanning electron microscope (SEM,FEI NOVA400 SEM with Oxford-EBSD system) using a step size of 2μm. All EBSD measurement were conducted from a normal plane of as-extruded plate and all EBSD data were analyzed using the Channel 5 software.

    2.2. Mechanical testing

    Fig. 1. Optical observations to the etched (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li samples.

    Tensile samples with a gauge length of 20mm, width of 3mm and thickness of 3mm were machined from the as-extruded plates. Moreover, samples with axial direction parallel to the transverse and extrusion directions of the plates were define as “TD” and “ED” samples, respectively. Tensile tests were conducted on a SHIMADZU (Servo, 5 KN)testing machine at a constant strain rate of 1×10-3s-1at room temperature and all measurements were repeated at least three times. For tensile samples, one side of the gauge section were finel polished before testing. Afterwards, the wide surface near fractures and fracture surfaces was observed by SEM with the modes of secondary electron (SE).

    2.3. Corrosion testing

    2.3.1. Immersion and mass loss testing

    To study corrosion performance, the Mg-Li alloys samples with dimensions of 12mm×10mm×3mm were immersed in 0.1M neutral NaCl solution (pH=6.9) for a certain time at room temperature. After immersion, samples were cleaned to remove corrosion products from surface using a chromic acid consisting of 180g/L CrO3[47]. Afterwards, surface morphology of the cleaned samples was observed by OM, confocal laser scanning microscopy (CLSM, OLYMPUS LEXT OLS4000)and SEM.Regarding of mass loss testing,the samples were immersed in 0.1M NaCl solution at room temperature for 3 days. Following the exposure period, a cleaning solution was used to remove corrosion products and then calculated the mass loss rates. Three replicates were carried out for each condition to ensure the reproducibility.Surface chemistry of specimens subjected to 2h immersion in 0.1M NaCl was analyzed by X-ray photoelectron spectroscopy (XPS, Escalab 250Xi, Thermo Fisher). The measured binding energy values were calibrated by the C1s (hydrocarbon C-C, C-H)of 285eV.

    2.3.2. Electrochemical analysis

    Potentiodynamic polarization measurements were carried out with a scan rate of 1mV/s by using a Wuhan CorrTest electrochemistry test system (CS350H). A classical threeelectrode cell was used with platinum as counter electrode,saturated calomel electrode (SCE) as reference electrode and the samples with an exposed area of 1 cm2as working electrode. The measurements were performed in 0.1M NaCl solution at room temperature. The scan frequency of electrochemical impedance spectroscopy (EIS) was executed over a frequency range from 100kHz to 10 mHz with 10mV of amplitude of sinusoidal potential signals with respect to the open circuit potential (OCP). To ensure the reliability, at least three replicates were carried out for each test and initial delay of 600s was set for polarization and EIS measurements to ensure a relative stabilized testing system at OCP [48].

    3. Results

    3.1. Microstructure and texture analysis

    The microstructure of as-extruded Mg-1Li, Mg-3Li and Mg-5Li alloys are shown in Fig.1,indicating that the deforming characteristics of the microstructure is trivial (especially for Mg-1Li and Mg-3Li alloys) and equiaxial grain structure forms in the three alloys. On the other hand, the grain size is not uniform for the three alloys with larger grains(>20μm) and smaller ones (<5μm). The average grain size of Mg-1Li, Mg-3Li and Mg-5Li alloys are 23.1μm, 24.8μm and 17.5μm,respectively.The results illustrates that the grain size of HCP Mg-Li alloy grows up slightly and then decreases with the increasing lithium content.

    The presence of equiaxial grains of the three as-extruded alloys demonstrates the occurrence of recrystallization during hot extrusion. To further confir the volume fraction of recrystallized, substructured and deformed grains, EBSD analysis was conducted, as shown in Fig. 2. The blue, yellow and red regions represent the recrystallized, substructured and deformation grains, respectively. It can be seen that the Mg-1Li and Mg-3Li alloys present the approximative percentage of each typed grain. However, the counterparts of Mg-5Li alloy change apparently, i.e. the volume fraction of recrystallized grains decrease from ~96% of Mg-1Li and Mg-3Li alloys to ~86% of Mg-5Li alloy; the substructured grains increase from 2~3% of Mg-1Li and Mg-3Li alloys to ~7% of Mg-5Li alloy; the deformed grains increase from ~1% of Mg-1Li and Mg-3Li alloys to ~6.5% of Mg-5Li alloy. Based on the above analysis, almost completed recrystallization occurs in both Mg-1Li and Mg-3Li alloys, whilst the Mg-5Li alloy possess more substructured and deformed grains.Therefore,it can be deduced that the increasing lithium concentration can restrain the occurrence of recrystallization for HCP Mg-Li alloy.

    Fig. 2. Recrystallized (a-c) maps and (d-f) histograms of as-extruded (a) (d) Mg-1Li, (b) (e) Mg-3Li and (c) (f) Mg-5Li alloys analyzed by EBSD.

    Fig. 3. Orientation maps of as-extruded (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li alloys analyzed by EBSD.

    The grain orientation of Mg alloys would be altered after deformation and the strong base texture was a general character, whilst the addition of lithium could change the texture of traditional magnesium alloys [28,29]. In this work, the oriented grain distribution of Mg-1Li, Mg-3Li and Mg-5Li alloys are shown in Fig. 3, where the different colors indicate different crystallographic orientations of the grains.It should be noted that the near red grains decrease with the increasing lithium concentration, whilst it is reversed for the green and blue grains. Namely, the near base (0001) texture gradually transforms into the prismatic (11-20) and (10-10)texture with the increasing lithium in HCP Mg-Li alloy. In addition, the grain size of Mg-5Li alloy is refined whilst the counterparts of Mg-1Li and Mg-3Li alloys are similar and larger than that of Mg-5Li alloy, which is corresponding to the OM results (Fig. 1).

    To further clarify the texture of the three alloys,the(0001),(11-20) and (10-10) pole figure are shown in Fig. 4. It can be seen that the base(0001)texture of Mg-1Li alloy is weaker than that of non-lithium Mg alloys, i.e. the c-axis of Mg-1Li alloy deviated 45° from ND (normal direction) and presents 45°with respect to ED(extrusion direction)and TD(transversal direction)simultaneously in the projective ED×TD plane,which can be define as 45° base texture herein. Meanwhile,the(11-20)and(10-10)prismatic texture are scattered.When the lithium content increases up to 3wt%, the c-axis of Mg-3Li alloy tilts about 60° away ND and exhibits about 10°toward TD (80° away ED). In addition, the (10-10) prismatic texture emerges, i.e. the (10-10) plane is approximately vertical to the ED. Regarding of Mg-5Li alloy, the c-axis further tilts about 85° away ED (almost paralleling to TD). Besides,the(10-10)prismatic texture is also apparent.Furtherly,based on the texture intensity and grain orientation distribution, the base (0001) texture become weaker and the prismatic (10-10)and (11-20) texture enhance obviously with the increasing lithium content in HCP Mg-Li system. Therefore, the increasing lithium content can alter the crystallographic texture from the 45° (0001) base texture of Mg-1Li alloy to (10-10)and (11-20) prismatic texture of Mg-5Li alloy effectively.

    3.2. Mechanical behaviors and fracture analysis

    Fig. 4. Pole figure of as-extruded (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li alloys analyzed by EBSD.

    Fig. 5. Engineering stress-strain curves of as-extruded (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li alloys along the extrusion direction (ED) and transverse direction (TD).

    Fig. 5 shows the stress-stain tensile curves evaluated along ED and TD of as-extruded Mg-xLi (x=1, 3, 5, wt%) alloys. It can be seen that the Mg-1Li alloy shows the mechanical isotropy along both ED and TD, whilst the mechanical anisotropy occurs for Mg-3Li alloy. Namely, ED sample of Mg-3Li alloy presents high mechanical strength and low elongation, whilst it is reversed for TD sample. When the lithium content increases up to 5wt%, the similar mechanical anisotropy of Mg-5Li alloy still exists. Additionally, it should be noted that the stress-strain curves of Mg-5Li alloy show serrated characterization when the tension is conducted along both ED and TD direction (Fig. 5c), which is define as Portevin-Le Chatelier effect. In general, the main mechanism of PLC effect could be ascribed to the dynamic strain aging (DSA), i.e. the repeated pinning and unpinning process of dislocations at solute atoms occurs when the diffusion velocity of solute atoms was compared to the moving rate of mobile dislocations in magnitude [49-52]. On the other hand,some other possible mechanisms had also been proposed to account for the PLC effect, such as extensive twins, shearing of precipitates by dislocations [51,52]. It should be notable that no precipitations are formed in the binary Mg-5Li alloy(Fig. 1) and deformation twins are also hardly observed on the fracture side surface (shown in Fig. 6 described as following). As a result, the PLC effect occurring in Mg-5Li alloy can be ascribed to the DSA. In terms of Mg-1Li and Mg-3Li alloys with less lithium concentration, the diffusion velocity of solute atoms should be lower than that the moving rate of mobile dislocations at this temperature, resulting in smooth stress-strain curves. Therefore, the PLC effect (serrated fl w)of Mg-Li alloy is closely related to the lithium content and the critical value needs to be confirme in the future work.

    To describe and compare the measured data, the mechanical properties of 0.2% proof yield strength (YS), ul-timate tensile strength (UTS) and elongation ratio to failure (EL) of the three alloys are listed in Table 2. Compared with the YS (93MPa/97MPa of ED/TD sample) and UTS (162MPa/163MPa of ED/TD sample) of Mg-1Li alloy, the YS (65MPa/61MPa of ED/TD sample) and UTS(154MPa/144MPa of ED/TD sample) of Mg-3Li alloy are slightly low, whereas the EL is inverse. Moreover, the mechanical strength of Mg-5Li alloy presents an elevation when compared with Mg-3Li alloy, which is ascribed to the refine ment strengthening and/or solution strengthening of lithium.As a result, the effect of lithium on the mechanical performance of HCP Mg-Li alloy is dependent on the lithium concentration, which is also in consistent with the previous work [21].

    Table 2 Tensile properties of as-extruded three Mg-Li alloys along ED and TD orientations.

    Fig. 6. SEM Observations to the fracture surfaces and side surfaces of (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li alloys.

    To reflec and compare the deformed microstructures of the three HCP Mg-Li alloys along differently orientations,the fracture surfaces and morphologies of side surfaces within a distance of about 1mm from the fracture sites are observed,as shown in Fig.6.For the Mg-1Li alloy,the fracture surfaces of both ED and TD samples are quite similar and mainly composed of tearing ridge and cleavage plane, which is a typical mixed ductile-brittle fracture. The side morphologies reveal that the surface is fla and no necking occurs in the lowmagnifie observation, whilst the obvious deformation bands and micro-cracks can be observed in the high magnificatio for both ED and TD samples. Meanwhile, micro-cracks initiate and propagate preferentially along the deformed bands,which is corresponding to the tearing ridge and/or plane in the fracture surface. In terms of Mg-3Li alloy, the fracture surface of ED and TD samples present a little difference, the tearing ridge of ED sample gradually transforms into tearing dimple of TD sample. Generally, plastic dimples can accommodate plastic strain during the tensile testing. As a result,the plasticity of TD sample is better than that of ED sample,which is in consistent with the tensile curves shown in Fig.5b.The side fracture morphologies of Mg-3Li alloy show that the necking occurs in TD sample and the deformation characterization with high density of slip bands and more micro-cracks is conspicuous.Therefore,all the deformation evidences prove a better deforming capacity when the tension of as-extruded Mg-3Li alloys is conducted along TD direction. Additionally,the side fracture morphology of ED sample is fla and only sparse slips can be observed, concomitant with a lower EL value. As for Mg-5Li alloy, the ductile fracture of ED and TD samples is obvious since a lot of dimples occur on the fracture surface. Compared with ED sample, the TD sample possess much more and deeper dimples, corresponding to a better plasticity shown in Fig. 5c. Besides, more dense slip bands with some cross-slips occurs in TD sample of Mg-5Li alloy compared with the ED sample, which further elucidates higher EL of TD sample. Moreover, the size of micro-cracks initiated at slip bands of Mg-5Li alloy decreases compared with the side fracture morphologies of Mg-1Li and Mg-3Li alloys, implying a relative uniform deformation occurred in HCP Mg-Li alloy with high lithium content.

    Fig. 7. Weight loss of Mg-1Li, Mg-3Li and Mg-5Li alloys exposed to 0.1M NaCl for 3 days.

    3.3. Corrosion behaviors

    The immersion testing is a practicable way to evaluate the corrosion prosperity of magnesium alloy by calculating the weight loss ratio, and the achieved weight loss rate of the Mg-1Li, Mg-3Li and Mg-5Li alloys are shown in Fig. 7. In general, the mass loss results represent corrosion rate directly and the average mass loss rate determined for Mg-1Li, Mg-3Li and Mg-5Li immersed in 0.1M NaCl for 3 days are 2.7,1.9 and 1.5mg/cm2/day, respectively. Namely, the mass loss rate of Mg-5Li alloy is less than those of Mg-1Li and Mg-3Li alloys, indicating that the high Li content is capable of reducing the corrosion rate in the HCP Mg-Li system.

    The surface morphologies of Mg-1Li, Mg-3Li and Mg-5Li alloys immersed in 0.1M NaCl for 16h are shown to rely strongly on the Li content, as shown in Fig. 8. The corrosion of Mg-1Li alloy reveals a deep groove-like corrosion morphology propagating along the ED direction preferentially. Such a groove-like corrosion morphology is associated with the reported scenario whereby local anode and cathode sites dynamically evolve[53-55].With the lithium content increasing up to 3wt.%, the groove-like corrosion morphology of Mg-3Li alloy becomes weaker. Compared with Mg-1Li and Mg-3Li alloys, the corrosion of Mg-5Li alloy is superficia and no obvious groove-like corrosion morphology is observed, consistent with the results of mass loss measurements. Besides, it is noted that the other areas on the surface of the Mg-Li alloys following 16h immersion appears to be also corroded apart from the apparent groove-like morphology, and therefore it is deemed essential to carry out SEM observation.

    The SEM observations to the corroded surfaces of three Mg-Li alloys after immersion in 0.1M NaCl for 2h are shown in Fig. 9, clarifying the microstructure dependent corrosion behavior. It should be notable that all the three HCP Mg-Li alloys show the typical feature of filifor corrosion in the lower magnification Besides, the corrosion ‘filaments with different orientations in different areas of the sample surface are seen in the high-magnifie observation, which is associated with the anisotropy of different grains where the corrosion is occurring. On the other hand, larger and deeper corrosion pits also occur in Mg-1Li alloys and the corrosion filament (Fig. 9d) are destroyed, corresponding to the worst corrosion resistance amongst the three Mg-Li alloys.The number of corrosion pits with smaller size occurring in Mg-3Li alloy decrease and the corrosion filament are prominent but slender, implying a better corrosion resistance than that of Mg-1Li alloy. With the lithium content increasing,the Mg-5Li alloy shows no corrosion pits on its surface after 2h immersion and the apparent corrosion filament are much fine than that of Mg-3Li alloy (Fig. 9f), indicating the best corrosion resistance of Mg-5Li alloy.

    Regarding the corrosion process in depth, typical 3D CLSM images illustrates the effect of lithium content on the depth of corrosion pits after immersion in 0.1M NaCl solution for different time (Fig. 10). Corrosion depth and width of Mg-1Li alloy are very sensitive to the immersion time, as shown in Fig. 10a-c. The shallow corrosion pits (177μm) of Mg-1Li alloy after 4h immersion turn into larger and a little deeper pits (222μm) of 8h immersion and then to much deeper corrosion grooves (391μm) of 16h immersion. For Mg-3Li and Mg-5Li alloys, the corrosion depth is not sensitive to the immersion time before 8h and only the corroded width enlarges, whereas the corrosion depth of Mg-5Li alloy is always less than that of Mg-3Li alloy at the same immersion time. However, the corrosion depth of Mg-3Li alloy shows an dramatic increment from 172μm of 8h immersion to 390μm of 16h immersion, whilst the ascending value of corroded depth (from 148μm, 8h to 267μm, 16h) for Mg-5Li alloy is slow relatively. Based on the above analysis and description, the high lithium concentration in HCP Mg-Li alloys can suppress corrosion sensitivity to the immersion time in NaCl solution.

    Fig. 8. Surface corrosion following the removal of corrosion products for (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li alloys imposed to 0.1M NaCl for 16h.

    Fig. 9. SEM observations to specimen surfaces following the removal of corrosion products for (a) Mg-1Li, (b) Mg-3Li and (c) Mg-5Li exposed to 0.1M NaCl for 2h. Images (d), (e) and (f) are higher-magnificatio observations to the localization in images (a), (b) and (c), respectively.

    Fig. 10. Representative 3D CLSM images of (a-c) Mg-1Li, (d-f) Mg-3Li and (g-i) Mg-5Li alloys subjected to immersion in 0.1M NaCl solution for (a) (d)(g) 4h, (b) (e) (h) 8h and (c) (f) (i) 16h.

    Fig. 11. (a) Potentiodynamic polarization curves and (b) EIS spectra (Nyquist plots) of Mg-1Li, Mg-3Li and Mg-5Li alloys measured in 0.1M NaCl solution.

    Table 3 Tafel fittin results derived from the polarization curves of the three Mg-Li alloys in 0.1M NaCl.

    Additionally, electrochemical testing is also an rational and acceptant approach generally to evaluate the corrosion resistance and/or mechanisms of the materials. Herein, the potentiodynamic polarization and electrochemical impedance spectroscopy (EIS) measurements are carried out to further elucidate electrochemical response of the three Mg-Li alloys,and the corresponding polarization curves and Nyquist plots are shown in Fig. 11. Based on the measured polarization response of the three Mg-Li (Fig. 11a), it is possible to speculate that the cathodic hydrogen evolution reaction (HER) kinetics decrease gradually with the increasing lithium content(denoted by the arrow). The anodic reaction kinetics of the studied Mg-Li alloys in 0.1M NaCl implies a low anodic Tafel slope and no apparent passivation. Even though a visual shift in the polarization curves, it seems that the anodic Tafel slope associated with the anodic partial reaction is essentially unchanged with the alteration of lithium concentration, such that the controlling factor (in terms of corrosion current density)is where the cathodic kinetics intersect to form corrosion potential (Ecorr). It is rationalized from the potentiodynamic polarization data that Ecorris increased with the descending lithium content. The detailed corrosion parameters are fitte by Tafel extrapolation and the results are listed in Table 3.The Mg-5Li alloy presents the lowest corrosion current density(icorr) of 6.89×10-6A/cm2, whilst icorrvalues of Mg-1Li and Mg-3Li alloys are about 1.05×10-5A /cm2and 8.03×10-6A/cm2, respectively. Therefore, Mg-5Li alloy containing the highest lithium content exhibits the best corrosion resistance.

    The Nyquist plots of the three Mg-Li alloys present the form characteristic of Mg alloys [56], whereby there is a high frequency capacitive loop, and an additional mediumto-low frequency capacitive loop that extends into the third quadrant with decreasing frequency (often termed an inductive loop) (Fig. 11b). The high frequency capacitance loops are attributed to the electric double layer at the interface between Mg substrate and 0.1M NaCl electrolyte [37,43,57].The medium frequency capacitance loops are related to the surface fil [35]. Existence of low frequency inductive loop can be ascribed to the surface fil with insufficientl protective function and corrosion nucleation at the initiation stage of localized corrosion. In addition, the capacitance loop dimension is enlarged obviously with the increasing lithium content in the three Mg-Li alloys. In general, the larger capacitance loop of Mg alloys indicate the lower dissolution rate, which also demonstrates that compact film are formed on the surface. As a result, the corrosion rate of the HCP Mg-Li alloys decreases and the fil protection function enhances with the increasing lithium content.

    4. Discussion

    4.1. Effect of lithium content on the microstructure and mechanical behavior

    As for the three HCP Mg-Li alloys studied in this work,the natural difference is the lithium content as their casting and processing technologies/parameters are always constant.On the other hand, the different lithium addition can result in different recrystallized microstructure and/or crystallographic texture during hot extrusion. In general, it is acceptant that non-basal slip of magnesium can be activated with the addition of lithium at room temperature [21-29]. In a previous study of Mg-Li single crystal deformation at room temperature and below, a strong evidence for the enhancement of〈c+a〉 slip by lithium additions was found as the critical resolved shear stress (CRSS) of 〈c+a〉 slip was lower than that of prismatic 〈a〉 slip at low temperatures [26]. Herein,the texture and grain orientation characters of the as-extruded Mg-5Li alloy(Figs.3 and 4)imply that large amounts of nonbasal slips can be activated during the tension. In terms of the fine grains in Mg-5Li alloy, it can be possibly explained as following:more non-basal dislocations appear in the extrusion process, which turn into the potential nucleation sites in the following dynamic recrystallization (DRX) process and then promote grain refinement DRX is a process involving nucleation and growth of new grains, which is influence by many factors including deformation degree, deformation temperature, solute atoms and second phases. Because the extrusion temperature is same and no other third alloying element in the studied Mg-Li alloys, the change of their microstructure can be attributed only to the lithium composition. Generally, the nucleation rate and growth rate of recrystallization decrease with the increase of alloying element content [23]. Moreover, it has been reported that recrystallization temperature of Mg-Li alloys increases with increasing Li content [23]. As a result, the DRX fraction of Mg-5Li alloy is the lowest in the studied HCP Mg-Li alloys. On the other hand, the refin grain size can further improve the mechanical performance of Mg-5Li alloy based on the Hall-Petch relationship [58].

    Furthermore, the texture analysis indicates that as-extruded HCP Mg-xLi (x=1, 3, 5) alloys present a texture element with basal planes rotated ~45° of Mg-1Li, ~80° of Mg-3Li and ~85° of Mg-5Li with respect to the extrusion direction(ED). A texture element of rotated basal planes of ~90° with respect to ED (i.e. the c-axis is approximately perpendicular to ED) was found in as-extruded Mg-4Li alloy with and without icosahedral phase [30]. On the other hand, the 45° basal texture of Mg-1Li alloy is altered into prismatic texture with the increasing lithium content in Mg-3Li and Mg-5Li alloys,concomitant with the similar results documented by previous works [21,29]. In the research of effect of Li content on the texture of Mg-Li alloys, Zeng et al. found that with the Li content increasing up to 2wt%, the basal texture weakened by ~24% compared with the as-extruded Mg-1Li sheet, yet both of them showed a strong basal texture [21]. While in the as-extruded Mg-3Li sheet, the basal texture intensity dropped by ~80% and tilted towards the transverse direction (TD)by ~63°, and the prismatic pole figur showed a preferred orientation along the extrusion direction (ED) [21]. In this work, when the room temperature tensile test is conducted on the as-extruded Mg-1Li alloy, the c-axes of these grains will present about 45° with ED and TD tensile direction. At this point, the Schmid factor for the basal slip is maximum,and the non-basal slip is hardly to activate for its large CRSS at room temperature. Herein, Schmidt factor (SF) can be expressed as [30,59]: SF=cosΦcosλ, where Φ and λ (angles Φ and λ are complementary (Φ+λ=90°)) are the angles of tensile direction with respect to the normal direction of slip plane and optimal slip direction, respectively. Therefore, the mechanical anisotropy of Mg-1Li alloy along ED and TD is trivial due to the equivalent slip capacity along the basal planes presenting 45° with both ED and TD. With increasing lithium content, such as for Mg-3Li and Mg-5Li alloys, the c-axes of grains are inclined to tilt away ED and parallel to TD (Fig. 4), indicating a lower SF for the basal slip along ED and a reversed result for TD sample. Therefore, the apparent mechanical anisotropy with high strength and low ductility along ED occurs for Mg-3Li and Mg-5Li alloys.

    4.2. Effect of lithium content on the corrosion behavior

    In general, the refine grain size could improve the corrosion resistance of Mg in neutral NaCl electrolytes with little dissent [60,61]. The grain boundary can act as a physical corrosion barrier and the refine grain microstructure means much more grain boundaries in matrix, indicating a better corrosion resistance of small-grained microstructure than that of coarse-grained microstructure in magnesium [62]. As such,in this work, the refine grains are correlated with the high corrosion resistance of Mg-5Li alloy containing more lithium.Actually, the effect of crystallographic orientation on the corrosion of magnesium should also be considered herein. For magnesium alloys,one study examined Mg in 0.1M NaCl and study grains after EBSD where near the {0001} planes were argued to be most corrosion resistant [63]. Recently, Bland and coauthors reported that the Mg {0001} surface exhibited corrosion susceptibility at the open circuit potential (OCP)while the {1010} and {1120} surfaces were passive at open circuit and pitting only initiated at potentials slightly anodic to their open circuit potentials in a similar environment [64].As for the studied Mg-1Li alloy herein, its worst corrosion resistance should be correlated with the inclined 45° basal texture, as shown in Fig. 4. Based on the analysis of grain orientated distribution (Fig. 3), more and more {0110} and{1210} planes (the green and blue grains) are inclined to the normal direction when the lithium content is elevated in HCP Mg-Li alloys. Therefore, the grains with normal orientations along the{0110}and{1210}plane(the green and blue grains in Fig. 3) are difficul to be corroded in Mg-5Li alloy compared with 45° base (0001) plane in Mg-1Li alloy, leading to the high corrosion resistance of Mg-5Li alloy.

    In fact, the variation in corrosion rate derived from thermomechanical processing effects, although a real effect, was not as large as the effect imparted by changes in alloying elements [65]. In this work, the surface fil should play a key role in improving the binary HCP Mg-Li alloy with increasing lithium content, concomitant with the enlarged capacitive loops as shown in EIS plots (Fig. 11). In general,the composition of surface fil on the traditional Mg alloys exposure to NaCl solution was porous Mg(OH)2combined with less MgO [66,67]. In terms of the Mg-Li alloys herein,the Mg(OH)2and MgO are inevitable in the surface fil as that of traditional magnesium, whilst compounds containing lithium should also be existed due to its higher electrochemical/chemical activity. The XPS analysis of C 1s on the MgxLi (x=1, 3, 5, wt%) alloys after immersion in 0.1M NaCl for 2h are shown in Fig.12.It can be seen that the peak corresponding Li2CO3is enhanced with increasing lithium content.As a result,the effect of Li2CO3on the surface fil should be considered to elaborate the improving corrosion resistance of Mg-5Li alloy with more lithium content. Besides, the protective function of Li2CO3fil on BCC Mg-Li alloys was also reported recently [41-46]. Generally, the occurrence of degradation for Mg alloys could be attributed to:1) magnesium was an active metal and the passivation fil composed of its oxide and hydroxide was only partially protective; 2) Cl-adsorption was believed to be able to penetrate the surface fil and destabilized the Mg atoms on the surface by weakening the bonding between the metallic atoms on the surface [34,68].However, some attractive works could be referred recently to prove that high corrosion resistant Mg alloys were possibly classifie to BCC Mg-Li systems due to the excellent Li2CO3protective fil deposited on the surface [41]. The underlaying mechanism on improving corrosion resistance of HCP Mg-Li alloy with increasing Li can be revealed as following:the high lithium concentration in Mg-5Li matrix accelerates the deposition of Li2CO3compounds on the surface and the insoluble Li2CO3compounds can further seal the porous Mg(OH)2to some extent, mitigating the permeation of aggressive Cl-to destroy the surface film Nevertheless, the protective fil on the HCP Mg-Li alloys is not insistent like that on the BCC Mg-Li alloy, resulting in severe corrosion occurring in Mg-5Li alloy with a long term immersion(Fig.10),similar results were reported in previous work [43].

    Fig. 12. XPS analysis of the surface fil on Mg-1Li, Mg-3Li and Mg-5Li alloys after immersion in 0.1M NaCl solution for 2h.

    5. Conclusions

    Through investigating the effect of lithium content on the texture, mechanical and corrosion behaviours of HCP MgxLi (x=1, 3, 5wt%) alloys, the following conclusions can be drawn:

    1 The increasing lithium content could reduce the dynamic recrystallization (DRX) of HCP Mg-Li alloys during hot extrusion and alter the 45° base (0001) texture of Mg-1Li alloy into prismatic texture of Mg-3Li and Mg-5Li alloys.

    2 The 45°base(0001)texture causes the mechanical isotropy of Mg-1Li alloy, whilst the obvious mechanical anisotropy of Mg-3Li and Mg-5Li alloys are attributed to the strong prismatic (10-10) and (11-20) texture.

    3 The groove-like corrosion of HCP Mg-Li alloys is weakened with increasing lithium content and the Mg-5Li alloys present the higher corrosion resistance, which is ascribed to the protective surface film combined with the refine grains and the alteration of orientated prismatic(10-10)and(11-20)planes to the exposed surface in NaCl solution.

    Declaration of Interest statement

    None.

    Acknowledgement

    This work was supported financiall by the National Natural Science Foundation of China (Grant No. 51901047), the Start-up Foundation of Guangdong University of Technology(No. 220413701) and National College Students Innovation and Entrepreneurship Training Program (Nos. 201911845185 and xj201911845345).

    人人妻人人添人人爽欧美一区卜| 国产精品一区二区精品视频观看| 亚洲色图 男人天堂 中文字幕| 欧美日本亚洲视频在线播放| 级片在线观看| 五月开心婷婷网| 天堂动漫精品| 丰满的人妻完整版| 超碰97精品在线观看| 制服诱惑二区| 国产午夜精品久久久久久| 一本综合久久免费| 成人18禁在线播放| 欧美人与性动交α欧美精品济南到| 久久99一区二区三区| 嫩草影院精品99| 俄罗斯特黄特色一大片| x7x7x7水蜜桃| 日韩高清综合在线| 亚洲五月婷婷丁香| 桃红色精品国产亚洲av| 90打野战视频偷拍视频| 国产在线观看jvid| 欧美成人午夜精品| 老司机深夜福利视频在线观看| 91大片在线观看| 亚洲avbb在线观看| 免费观看精品视频网站| 一边摸一边抽搐一进一出视频| 日日爽夜夜爽网站| av国产精品久久久久影院| 中出人妻视频一区二区| av电影中文网址| 极品人妻少妇av视频| 精品国产一区二区久久| 国产av精品麻豆| 亚洲精品粉嫩美女一区| 亚洲精品美女久久av网站| 久久中文看片网| 波多野结衣av一区二区av| 欧美一区二区精品小视频在线| 色播在线永久视频| 国产99久久九九免费精品| 我的亚洲天堂| 国内久久婷婷六月综合欲色啪| √禁漫天堂资源中文www| 夜夜夜夜夜久久久久| 亚洲中文日韩欧美视频| 精品少妇一区二区三区视频日本电影| 日日摸夜夜添夜夜添小说| 十八禁人妻一区二区| 18禁裸乳无遮挡免费网站照片 | www.自偷自拍.com| 99久久久亚洲精品蜜臀av| 搡老熟女国产l中国老女人| 无限看片的www在线观看| 看免费av毛片| 黑人欧美特级aaaaaa片| 午夜久久久在线观看| 精品日产1卡2卡| 成熟少妇高潮喷水视频| 国产日韩一区二区三区精品不卡| 人人澡人人妻人| 亚洲欧美日韩高清在线视频| 可以在线观看毛片的网站| 国产精品久久久久成人av| 在线十欧美十亚洲十日本专区| 一边摸一边做爽爽视频免费| 久久精品91蜜桃| 国产男靠女视频免费网站| 国产又爽黄色视频| 侵犯人妻中文字幕一二三四区| 日韩精品中文字幕看吧| 久久久久国产精品人妻aⅴ院| 波多野结衣一区麻豆| 啦啦啦免费观看视频1| 亚洲av成人一区二区三| 日韩欧美在线二视频| 最新美女视频免费是黄的| 亚洲国产中文字幕在线视频| 91麻豆av在线| 国产亚洲精品久久久久5区| 色综合站精品国产| av网站免费在线观看视频| 91精品三级在线观看| 日韩 欧美 亚洲 中文字幕| 亚洲 国产 在线| 天天影视国产精品| 99国产极品粉嫩在线观看| 黄频高清免费视频| 少妇裸体淫交视频免费看高清 | 欧美乱色亚洲激情| 高潮久久久久久久久久久不卡| 亚洲avbb在线观看| 高潮久久久久久久久久久不卡| √禁漫天堂资源中文www| 日本vs欧美在线观看视频| 亚洲九九香蕉| 在线观看免费视频网站a站| 国产亚洲精品第一综合不卡| 韩国精品一区二区三区| 黄色成人免费大全| 在线观看免费视频日本深夜| 亚洲人成网站在线播放欧美日韩| 999精品在线视频| 99久久人妻综合| 男女下面进入的视频免费午夜 | av有码第一页| 色精品久久人妻99蜜桃| 午夜精品在线福利| 亚洲五月婷婷丁香| 91av网站免费观看| 成在线人永久免费视频| 日韩视频一区二区在线观看| 另类亚洲欧美激情| 新久久久久国产一级毛片| 亚洲av成人不卡在线观看播放网| 亚洲少妇的诱惑av| 天天影视国产精品| 18禁国产床啪视频网站| 99久久人妻综合| 好男人电影高清在线观看| 99久久人妻综合| 久久狼人影院| 成年人免费黄色播放视频| 91av网站免费观看| 日韩大码丰满熟妇| 美女 人体艺术 gogo| 老司机福利观看| 午夜久久久在线观看| 精品高清国产在线一区| 超碰成人久久| 亚洲成人免费电影在线观看| 18禁观看日本| 欧美在线黄色| 十八禁网站免费在线| 日韩欧美免费精品| a在线观看视频网站| 他把我摸到了高潮在线观看| 精品一区二区三区视频在线观看免费 | 国产亚洲欧美在线一区二区| 伊人久久大香线蕉亚洲五| 亚洲成人精品中文字幕电影 | 男女午夜视频在线观看| 黑人巨大精品欧美一区二区mp4| 欧美日韩瑟瑟在线播放| 可以在线观看毛片的网站| 日韩免费高清中文字幕av| 高清欧美精品videossex| 成人永久免费在线观看视频| 精品久久久精品久久久| 午夜两性在线视频| 好男人电影高清在线观看| 国产xxxxx性猛交| 欧美日本中文国产一区发布| 51午夜福利影视在线观看| 色精品久久人妻99蜜桃| x7x7x7水蜜桃| 欧美日韩亚洲国产一区二区在线观看| 在线播放国产精品三级| 美女福利国产在线| 国产无遮挡羞羞视频在线观看| 亚洲国产毛片av蜜桃av| 18禁国产床啪视频网站| 亚洲国产欧美日韩在线播放| 国产精品影院久久| 女人被躁到高潮嗷嗷叫费观| 午夜激情av网站| 久久久国产一区二区| 啪啪无遮挡十八禁网站| 欧美色视频一区免费| 国产麻豆69| 国产成人一区二区三区免费视频网站| 中文字幕色久视频| 色尼玛亚洲综合影院| 91在线观看av| 天天躁夜夜躁狠狠躁躁| 天天躁夜夜躁狠狠躁躁| 国产高清视频在线播放一区| 18禁观看日本| 日本五十路高清| 99re在线观看精品视频| 国产欧美日韩一区二区三| 久久草成人影院| 在线播放国产精品三级| 男女高潮啪啪啪动态图| 成人18禁在线播放| 一本大道久久a久久精品| 亚洲va日本ⅴa欧美va伊人久久| 999久久久精品免费观看国产| 18禁观看日本| av视频免费观看在线观看| 亚洲男人天堂网一区| 男女床上黄色一级片免费看| 午夜亚洲福利在线播放| 天天添夜夜摸| 免费在线观看黄色视频的| 级片在线观看| 欧美 亚洲 国产 日韩一| 精品国产亚洲在线| 精品国产一区二区三区四区第35| 国产一区二区在线av高清观看| 99国产精品一区二区蜜桃av| 制服诱惑二区| 欧美日韩亚洲国产一区二区在线观看| 中文字幕高清在线视频| 精品电影一区二区在线| 黄片小视频在线播放| 女性生殖器流出的白浆| 中文字幕人妻丝袜一区二区| av有码第一页| 在线观看免费日韩欧美大片| 三级毛片av免费| 亚洲精品国产色婷婷电影| 久久 成人 亚洲| 麻豆成人av在线观看| 日韩精品青青久久久久久| 亚洲少妇的诱惑av| 国产精品久久久人人做人人爽| 亚洲中文av在线| 麻豆av在线久日| 很黄的视频免费| 级片在线观看| 欧美 亚洲 国产 日韩一| 女同久久另类99精品国产91| 欧美最黄视频在线播放免费 | 精品卡一卡二卡四卡免费| 美国免费a级毛片| 日韩人妻精品一区2区三区| 9色porny在线观看| 每晚都被弄得嗷嗷叫到高潮| 90打野战视频偷拍视频| 久久久久国产一级毛片高清牌| 国产伦一二天堂av在线观看| 自线自在国产av| 国产免费现黄频在线看| 久久久久国产一级毛片高清牌| 久久精品国产综合久久久| 涩涩av久久男人的天堂| 国产亚洲精品久久久久5区| 久久草成人影院| 国产精品国产高清国产av| 午夜福利欧美成人| 久久久久久久久久久久大奶| 伦理电影免费视频| 成人特级黄色片久久久久久久| 国产精品国产av在线观看| 一边摸一边抽搐一进一小说| av天堂久久9| 激情视频va一区二区三区| 亚洲av美国av| 99在线视频只有这里精品首页| 丁香六月欧美| 国产av在哪里看| 男女之事视频高清在线观看| 99久久综合精品五月天人人| 午夜激情av网站| 久久中文看片网| 久久久国产成人免费| 国产成人精品久久二区二区免费| 新久久久久国产一级毛片| 天堂中文最新版在线下载| 91麻豆av在线| 亚洲专区国产一区二区| 国产精品免费一区二区三区在线| 欧美色视频一区免费| 男男h啪啪无遮挡| 波多野结衣av一区二区av| 人成视频在线观看免费观看| 久久午夜综合久久蜜桃| 久久婷婷成人综合色麻豆| 国产免费现黄频在线看| 欧美中文日本在线观看视频| 老司机在亚洲福利影院| 宅男免费午夜| 国产欧美日韩综合在线一区二区| 91在线观看av| 国产不卡一卡二| 18美女黄网站色大片免费观看| 国产精品一区二区免费欧美| 老熟妇仑乱视频hdxx| 俄罗斯特黄特色一大片| 国产亚洲欧美精品永久| www.自偷自拍.com| 真人一进一出gif抽搐免费| 男女高潮啪啪啪动态图| 丰满饥渴人妻一区二区三| 免费av毛片视频| 久久久国产成人免费| 在线观看舔阴道视频| 午夜福利欧美成人| 久久久久国内视频| 人人澡人人妻人| 男人舔女人的私密视频| 亚洲激情在线av| 成人黄色视频免费在线看| 精品国产国语对白av| 精品一区二区三卡| 18美女黄网站色大片免费观看| 怎么达到女性高潮| av中文乱码字幕在线| 久久久久久久精品吃奶| av天堂久久9| 日本免费一区二区三区高清不卡 | 亚洲激情在线av| 操出白浆在线播放| 欧美性长视频在线观看| 在线观看一区二区三区| 国产精华一区二区三区| 精品久久久久久久久久免费视频 | 午夜福利一区二区在线看| 丝袜美腿诱惑在线| 久久中文看片网| 中国美女看黄片| av天堂久久9| 丰满饥渴人妻一区二区三| 成年版毛片免费区| 1024香蕉在线观看| 国产国语露脸激情在线看| 成人永久免费在线观看视频| 另类亚洲欧美激情| 久久九九热精品免费| 中文字幕av电影在线播放| 欧美+亚洲+日韩+国产| 欧美日韩乱码在线| 一个人免费在线观看的高清视频| av片东京热男人的天堂| 亚洲五月色婷婷综合| 黄片小视频在线播放| 欧美日韩福利视频一区二区| 在线观看舔阴道视频| 国产av一区二区精品久久| 中文字幕人妻熟女乱码| 女性被躁到高潮视频| 国产欧美日韩精品亚洲av| 桃色一区二区三区在线观看| 午夜91福利影院| 亚洲自拍偷在线| 久久久久九九精品影院| 日日摸夜夜添夜夜添小说| 女人高潮潮喷娇喘18禁视频| 亚洲性夜色夜夜综合| 亚洲欧美精品综合久久99| 国产视频一区二区在线看| 久久久久久久午夜电影 | 欧美日韩瑟瑟在线播放| 一进一出好大好爽视频| 中国美女看黄片| 亚洲精品av麻豆狂野| 乱人伦中国视频| 国产成人精品无人区| 在线播放国产精品三级| 久久久久久免费高清国产稀缺| 男女床上黄色一级片免费看| 中文字幕人妻熟女乱码| 美国免费a级毛片| 一级a爱片免费观看的视频| 亚洲欧美一区二区三区黑人| 精品欧美一区二区三区在线| 一级a爱视频在线免费观看| 丰满的人妻完整版| 美女 人体艺术 gogo| 精品卡一卡二卡四卡免费| 无遮挡黄片免费观看| 久久久精品欧美日韩精品| 亚洲男人的天堂狠狠| 日本黄色视频三级网站网址| 久久久久久久午夜电影 | 亚洲精品在线美女| 五月开心婷婷网| 成年女人毛片免费观看观看9| 激情在线观看视频在线高清| 一区福利在线观看| 99国产精品一区二区蜜桃av| 欧美中文综合在线视频| 99久久久亚洲精品蜜臀av| 男女床上黄色一级片免费看| 久久香蕉激情| 久久热在线av| 夜夜看夜夜爽夜夜摸 | 日本免费a在线| 成人亚洲精品av一区二区 | 欧美日韩亚洲综合一区二区三区_| aaaaa片日本免费| 9191精品国产免费久久| 国产高清激情床上av| 一级作爱视频免费观看| 不卡av一区二区三区| 男女床上黄色一级片免费看| 欧美人与性动交α欧美精品济南到| 亚洲欧美激情综合另类| 无限看片的www在线观看| 久久精品aⅴ一区二区三区四区| 日韩大码丰满熟妇| 精品久久久久久成人av| 日韩精品中文字幕看吧| av中文乱码字幕在线| 人人妻人人爽人人添夜夜欢视频| 精品国产一区二区久久| 两性午夜刺激爽爽歪歪视频在线观看 | √禁漫天堂资源中文www| 大型黄色视频在线免费观看| 亚洲av熟女| 亚洲色图综合在线观看| 啦啦啦免费观看视频1| 中亚洲国语对白在线视频| 9色porny在线观看| 嫩草影视91久久| 久久久久久久久久久久大奶| 怎么达到女性高潮| 神马国产精品三级电影在线观看 | 中文亚洲av片在线观看爽| 两个人免费观看高清视频| 中国美女看黄片| 天堂影院成人在线观看| 亚洲人成网站在线播放欧美日韩| 国产伦人伦偷精品视频| 精品午夜福利视频在线观看一区| 欧美成人午夜精品| 岛国视频午夜一区免费看| 国产精品偷伦视频观看了| 精品第一国产精品| 精品国产超薄肉色丝袜足j| 久久人妻熟女aⅴ| 精品第一国产精品| 在线视频色国产色| 国产黄色免费在线视频| 看免费av毛片| 一区福利在线观看| 成年人黄色毛片网站| 一边摸一边抽搐一进一出视频| 女性生殖器流出的白浆| 大码成人一级视频| 免费在线观看影片大全网站| 久久久久久久精品吃奶| 国产成人av激情在线播放| 午夜免费成人在线视频| 日韩av在线大香蕉| 女人爽到高潮嗷嗷叫在线视频| 亚洲,欧美精品.| 久久久久国产一级毛片高清牌| 国产一区二区三区视频了| 满18在线观看网站| av国产精品久久久久影院| 午夜a级毛片| av片东京热男人的天堂| 久热爱精品视频在线9| 精品免费久久久久久久清纯| 亚洲在线自拍视频| 国产亚洲精品第一综合不卡| 国产伦人伦偷精品视频| 人人澡人人妻人| 在线永久观看黄色视频| 免费在线观看亚洲国产| 色婷婷久久久亚洲欧美| 免费av毛片视频| x7x7x7水蜜桃| 欧美成人午夜精品| 精品久久久久久久毛片微露脸| 两个人看的免费小视频| 久久久久久亚洲精品国产蜜桃av| 亚洲精品国产一区二区精华液| 国产高清视频在线播放一区| 免费女性裸体啪啪无遮挡网站| 夜夜躁狠狠躁天天躁| 免费看a级黄色片| 久久性视频一级片| 欧美乱码精品一区二区三区| 十八禁网站免费在线| 精品欧美一区二区三区在线| 亚洲一区二区三区色噜噜 | 在线观看午夜福利视频| 男男h啪啪无遮挡| 亚洲视频免费观看视频| 老司机午夜十八禁免费视频| 在线观看免费视频日本深夜| 91av网站免费观看| 精品国内亚洲2022精品成人| 岛国视频午夜一区免费看| 两人在一起打扑克的视频| 夜夜看夜夜爽夜夜摸 | 99在线视频只有这里精品首页| 色婷婷久久久亚洲欧美| 中文字幕另类日韩欧美亚洲嫩草| 91精品国产国语对白视频| 丰满的人妻完整版| 免费不卡黄色视频| 国产乱人伦免费视频| 国产精品爽爽va在线观看网站 | 黄色成人免费大全| 91成年电影在线观看| 中文字幕最新亚洲高清| 精品国产一区二区三区四区第35| 操美女的视频在线观看| 日韩中文字幕欧美一区二区| 交换朋友夫妻互换小说| 可以在线观看毛片的网站| 丁香欧美五月| 十八禁人妻一区二区| 国产精品99久久99久久久不卡| 国产精品免费一区二区三区在线| 久久精品国产99精品国产亚洲性色 | 久久中文字幕一级| 成人影院久久| 国产又爽黄色视频| 午夜精品久久久久久毛片777| 国产精品乱码一区二三区的特点 | 1024香蕉在线观看| 操美女的视频在线观看| 久久婷婷成人综合色麻豆| 日本a在线网址| 啦啦啦在线免费观看视频4| 午夜福利欧美成人| 成熟少妇高潮喷水视频| 一进一出抽搐gif免费好疼 | 国产成+人综合+亚洲专区| 在线天堂中文资源库| 日本三级黄在线观看| 日本欧美视频一区| 欧美丝袜亚洲另类 | 亚洲 国产 在线| 真人一进一出gif抽搐免费| 一边摸一边做爽爽视频免费| 交换朋友夫妻互换小说| 国产伦一二天堂av在线观看| 国产一卡二卡三卡精品| www.精华液| av在线播放免费不卡| 性欧美人与动物交配| 涩涩av久久男人的天堂| 制服诱惑二区| 777久久人妻少妇嫩草av网站| 亚洲性夜色夜夜综合| 久久 成人 亚洲| 久久香蕉国产精品| 日本vs欧美在线观看视频| 一边摸一边做爽爽视频免费| 人成视频在线观看免费观看| netflix在线观看网站| 深夜精品福利| 精品一区二区三区av网在线观看| 18禁国产床啪视频网站| 日本三级黄在线观看| 亚洲第一av免费看| 极品人妻少妇av视频| 久久精品91蜜桃| 露出奶头的视频| 一级毛片高清免费大全| 久久精品影院6| 亚洲avbb在线观看| 国产成人系列免费观看| 精品久久久久久电影网| 欧美+亚洲+日韩+国产| 久久性视频一级片| 国产乱人伦免费视频| 中亚洲国语对白在线视频| 亚洲欧美精品综合一区二区三区| 人成视频在线观看免费观看| 免费在线观看视频国产中文字幕亚洲| 欧美激情极品国产一区二区三区| 国产激情欧美一区二区| 亚洲免费av在线视频| 亚洲精品国产色婷婷电影| av超薄肉色丝袜交足视频| 老熟妇仑乱视频hdxx| 少妇粗大呻吟视频| 精品国产亚洲在线| 日韩欧美免费精品| 国产精品久久电影中文字幕| 亚洲中文字幕日韩| 欧美在线一区亚洲| 久久青草综合色| 午夜91福利影院| 中文字幕人妻熟女乱码| 欧美丝袜亚洲另类 | 欧美乱色亚洲激情| 亚洲av成人不卡在线观看播放网| 91av网站免费观看| 免费在线观看视频国产中文字幕亚洲| 国产欧美日韩一区二区三| 国产av一区在线观看免费| 黄色女人牲交| 亚洲精品国产色婷婷电影| 亚洲av美国av| 午夜免费鲁丝| 成年人免费黄色播放视频| 久久 成人 亚洲| av视频免费观看在线观看| 成人国语在线视频| 免费少妇av软件| 国产成人欧美在线观看| 免费看a级黄色片| 欧美日韩视频精品一区| 国产精品乱码一区二三区的特点 | 一级,二级,三级黄色视频| 黑人巨大精品欧美一区二区mp4| 亚洲精华国产精华精| av电影中文网址| 亚洲男人天堂网一区| 国产高清国产精品国产三级| 亚洲成av片中文字幕在线观看| 一级毛片精品| 99精国产麻豆久久婷婷| 一本综合久久免费| 日本精品一区二区三区蜜桃| 中出人妻视频一区二区| 在线永久观看黄色视频| 一级毛片女人18水好多| 90打野战视频偷拍视频| 99国产精品99久久久久| 免费高清在线观看日韩| 午夜免费鲁丝| 1024香蕉在线观看| 可以免费在线观看a视频的电影网站| 热re99久久精品国产66热6|