    A comprehensive analysis on microstructure evolution of Mg-5.65Zn-0.66Zr alloy during hot deformation

    2021-05-21 03:32:08QianChengLiangChenJianweiTangGuoqunZhaoLuSunCunshengZhang
    Journal of Magnesium and Alloys 2021年2期

    Qian Cheng, Liang Chen, Jianwei Tang, Guoqun Zhao, Lu Sun, Cunsheng Zhang

    Key Laboratory for Liquid-Solid Structural Evolution and Processing of Materials (Ministry of Education), Shandong University, Jinan, Shandong 250061,PR China

    Received 6 October 2019; received in revised form 18 November 2019; accepted 2 January 2020

    Available online 29 September 2020

    Abstract

    Keywords: Hot compression; Microstructure; Recrystallization; Texture; Twinning.

    1. Introduction

    The consumption of Mg alloys is increasing in the field of automobile and aerospace industries due to the advantages of low density, high specifi strength and easy recycling [1-3].However, the poor formability of Mg alloys at room temperature caused by the hexagonal close-packed (HCP) crystal structure and limited slip systems restricts their widespread application. The thermo-mechanical processes such as hot extrusion, hot rolling and hot forging are usually employed to produce various of Mg components. The microstructure experiences significan evolution during the thermal-mechanical processes,and it is strongly affected by the temperature,strain and stain rate, which consequently affects the fina mechanical properties. Hence, the thermal deformation behaviors of Mg alloys have attracted much interests from researchers.

    In the past decades, lots of studies have been carried out to investigate the microstructure evolution of Mg alloys during hot deformation, and it was reported that the temperature, strain and stain rate greatly affected the occurrence of dynamic recovery, dynamic recrystallization (DRX), dynamic precipitation and twinning [4,5]. Wan et al. [6] studied the effects of pre-strain on twinning behaviors of an extruded Mg-Zr alloy, and found that the pre-strain was beneficia to promote the nucleation of twins inside grains. Yang et al.[7] studied the evolution of precipitates in ZK60 Mg alloy during hot deformation, and proposed that the high strain rate, high density dislocation, high shear stress and adiabatic temperature rise accelerated the precipitation and preliminary dissolution of the rod-like phases. Hadadzadeh et al. [8] developed the constitutive equation, strain hardening and strain rate sensitivity of ZK60 alloy based on the fl w behavior.Sanyal et al. [9] studied the effects of deformation temperature on DRX, texture and mechanical properties of Mg-Zn-Al alloy. Zhao et al. [10] clarifie the twinning behavior of hot extruded AZ31 hexagonal prisms during uniaxial compression.

    Twinning easily takes place at the initial deformation stage of Mg alloys due to the insufficien active slip systems in HCP structure [11], and it plays important roles in the deformation behavior. Twinning can compensate for the limited operative systems by reorienting grains,resulting in the rotation of basal planes from a hard slip to a soft direction, or the accommodation of strain along c-axis [12]. Moreover, twinning and DRX usually dominate the evolution of microstructure and texture during hot deformation of Mg alloys. As is known,three types of twins can be found in Mg alloys, and they are named as {10-12} extension twins with a characteristic misorientation of 86°<-12-10>, {10-11} contraction twins with 56° <-12-10>, and {10-11}-{10-12} double twins with 38°<-12-10>[13,14]. {10-12} extension twins are recognized to occur frequently during hot deformation of Mg alloys, and they greatly affect the texture evolution and indirectly facilitate the DRX behavior [13,15,16]. The effects of {10-12}extension twins on deformation of Mg alloys were summarized by Hong et al. [17] as follows: (1) accommodation of deformation, causing a low fl w stress and strain hardening rate; (2) Hall-Petch hardening by twinning-induced variation of grain size; (3) twining texture induced by the change in activities of slips.

    Besides, the non-basal slips also affect the deformation of Mg alloys. As is known, <a>or prismatic <a>slip are primary slip modes in HCP metals. However, these two slip systems only produce strain along <a>direction [18]. The activation of pyramidal <c+a>slip can enhance the deformation homogeneity by providing a strain component along <c>direction. The pyramidal slip has two modes: the first-orde{10-11}<11-2-3>mode and the second-order{-1-122}<11-23>mode. The pyramidal slip plays an essential role on the ductility of HCP metals. Kim et al. [19]. found that the pyramidal slip with both first-orde and second-order could be activated in Mg alloy, and the pyramidal dislocations formed at the boundaries of grains with [11-20] and [10-10] textures. Gallyev et al. [20] reported that the pyramidal slip was activated during high temperature deformation of Mg alloys due to the reduction of critical resolved shear stress (CRSS),which promoted the formation of high angle grain boundaries(HAGBs, >15o) and low temperature DRX. Zecevic et al.[21] studied the activity of first-orde and second-order pyramidal slips in Mg alloys, and proposed that the pyramidal slip led to the basal texture titling from normal direction.Kim et al. [22] found that the formation of shear bands was accelerated due to the DRX caused by the activation of <a>and <c+a>slips.

    Fig. 1. (a) Grain structure and orientation, and (b) second phase of the homogenized ZK60 alloy.

    Although some experimental works have been conducted to study the effects of temperature, strain and strain rate on the hot deformation behavior of Mg alloys,few of them could provide a comprehensive analysis on the microstructure evolution. In the present study, the hot compression tests were carried out by using a Mg-Zn-Zr alloy within the temperature range of 250-400 °C, strain rate range of 0.001-1 s-1, and various fina strain. The evolutions of microstructure without and with twining were respectively discussed. Moreover, The grain growth, DRX, twinning, texture and slip were investigated, and the relationships between them were clarified

    2. Experiment procedures

    The as-cast ZK60 Mg alloy with the chemical compositions of Mg-5.65Zn-0.66Zr (wt.%) was used as the raw material. The homogenization treatment was performed at 380 °C for 15 h, followed by air cooling. Fig. 1 shows the microstructure of homogenized ZK60 Mg alloy. An equiaxed grain structure with random distribution of orientation can be observed. The average grain size is calculated as around 26.5 μm. Moreover, small number of secondary particles locate on the grain boundaries. The particles are composed by Mg and Zn, and they should be Mg-Zn eutectic which were difficul to dissolve during homogenization. Then, the cylindrical samples with the diameter of 10 mm and the height of 15 mm were machined for hot compression test, which was carried out using a Gleeble-3500C thermo-simulation machine.In general,the hot forming processes of ZK60 alloy are performed within the temperature range of 250-400 °C, and a strain rate range of 0.001-1 s-1is usually applied [8,20,23].Therefore, the above ranges of temperature and strain rate were selected as the experimental conditions. The compression tests were divided into two groups. The firs group was conducted at the temperatures of 250 °C, 300 °C, 350 °C and 400 °C, and strain rates of 0.001 s-1, 0.01 s-1, 0.1 s-1and 1 s-1, with an identical true strain of 0.92. The second group was conducted at 300 °C and 350 °C, while the true strain varied from 0.09 to 1.6. The firs group was used to study the effects of temperature and strain rate on the microstructure evolution, while the second group focused on the effects of strain.

    Fig. 2. True stress-strain curves of ZK60 Mg alloy compressed at temperature range of 250-400 °C and with the strain rate of (a) 0.001 s-1, (b) 0.01 s-1,(c) 0.1 s-1, and (d) 1 s-1.

    The samples were immediately quenched into cooled water after compression tests. Then, the samples were sectioned along the compression direction (CD), and the microstructure in the center of the sectioned surface was examined.The samples for optical microscope (OM) observation were polished and then etched for 10 s using the mixture of 4.2 g picric acid,10 ml acetic acid, 10 ml distilled water, and 70 ml alcohol.Since the samples are axial axisymmetric, the other two observation directions were both set as transverse direction(TD)in electron back-scatter diffraction(EBSD)analysis.The samples for EBSD analysis were electro-polished in a solution of 800 ml ethanol,100 ml propanol,18.5 ml distilled water,75 g citric acid and 10 g hydroxyquinoline (ACII electrolyte) with the cooling of liquid nitrogen at 18 V for 40 s. Then, the EBSD analysis was conducted with a scanning step size of 1 μm, and the EBSD data was analyzed by HKL Channel 5 software.

    3. Results and discussion

    3.1. Flow stress behavior

    Fig. 2 shows the true stress-strain curves achieved from the hot compression tests of ZK60 alloy. As is seen, both the strain hardening and softening behavior can be observed.The fl w stress increases sharply and reaches a peak point at the initial stage, and then gradually decreases. The curves shown in Fig. 2 consist of work hardening and softening stages. The work hardening is mainly caused by dislocation,particle pipe-up and twining, and it is the main phenomenon at the initial deformation stage. With the increase of strain,the stored energy meets the requirement of CRSS.Then,DRX is initiated and the slope of stress-strain curves is decreased.It should be pointed out that the curves cannot reach a steady stage even at high strain level, which will be discussed in the latter section.

    Fig. 3. Optical microstructure of the compressed samples with a true strain of 0.92 and a reduction of 60%.

    Fig. 3 shows the optical microstructure of the compressed samples with a reduction of 60%, corresponding to a true strain of 0.92.As is seen,if the fina strain is fi ed at 0.92,the partial DRX occurs in all of the samples, and none of them achieves a complete DRXed grain structure. The fin DRXed grains locate along the boundaries of initial grains, leading to the formation of a necklace structure. Moreover, both the size and fraction of DRXed grains increase with the increase of deformation temperature. In contrast, the higher strain rate results in smaller size and fraction of DRXed grains. A deep analysis about the effects of deformation parameters on the grain structure will be discussed in the latter section.

    Fig. 4. Optical microstructure of the samples compressed with the strain of 0.032 and 0.23,and at the conditions of 350°C/0.001 s-1 and 350°C/0.1 s-1.

    3.2. Analysis of microstructure evolution without twinning

    To further study the microstructure evolution, the hot compression tests were conducted with various fina strain. This section aims to analyze the microstructure evolution without the formation of twins. The relatively high temperatures and low strain rates such as 350 °C/0.001 s-1and 350 °C/0.1 s-1were selected for examination, since the twins were difficul to form under these conditions. The true strain of 0.032,0.23, 0.33, 0.92 and 1.6 was selected from the curves of 350 °C/0.001 s-1and 350 °C/0.1 s-1for examination. The optical microstructures of samples with low strain levels such as 0.032 and 0.23 are firstl shown in Fig. 4. For both curves,almost no DRXed grain can be found when the strain is as low as 0.032, while some DRXed grains appear when the strain increases to 0.23. Although the twins can easily form during the work hardening stage of Mg alloys, they are not found in the samples shown in Fig. 4. It indicates that the deformation conditions of 350 °C/0.001 s-1and 350 °C/0.1 s-1cannot meet the values of CRSS of twins. Hence, the dominant deformation mechanism should be slip and DRX, which will be the main focus of this section.

    Fig. 5. EBSD maps of the samples compressed at 350 °C/0.001 s-1 with the strain of (a) 0.33, (b) 0.92, (c) 1.6, and at 350 °C/0.1 s-1 with the strain of (d) 0.33, (e) 0.92, (f) 1.6.

    The previous studies have reported the mechanisms of DRX in Mg alloys, such as the discontinuous DRX (DDRX),continuous DRX (CDRX), twinning induced DRX (TDRX)and particle-stimulated nucleation(PSN),and the DRX mechanisms were affected by the deformation conditions and the second phases [4,24,25]. It was reported that CDRX was the dominant mechanism during hot compression of ZK60 alloy [20,26]. Fig. 5 shows the EBSD maps at the conditions of 350 °C/0.001 s-1and 350 °C/0.1 s-1with the relatively high strain levels of 0.33, 0.92 and 1.6. It is obvious that large number of low angle grain boundaries (LAGBs, 2~15o)formed inside the deformed grains, which is an evidence of the CDRX. The continuously increase of DRX fraction with the increase of strain can be easily found in Fig. 5. As shown in Fig. 5(a) and 5(d), few DRXed grains can be observed at the strain of 0.33, which indicates the beginning of DRX,while more DRXed grains appear with the increase of strain.When the strain reaches 1.6, the DRX fraction of 0.001 s-1with 48.7% is higher than that of 0.1 s-1with 27.6%, as shown in Fig. 5(c) and (f). Moreover, most of the grains rotate during hot compression to form a preferred orientation that the c-axis tends to be parallel with CD. Besides, at the strain rate of 0.001 s-1and strain of 0.33, some of the grains have the size even larger than 100 μm, which is also much larger than the grain size of the homogenized billet, as shown in Fig. 5(a). It indicates that an obvious grain growth occurred at the strain rate of 0.001 s-1due to the long deformation time. In contrary, as shown in Fig. 5(d), the grain size with strain rate of 0.1 s-1and strain of 0.33 is similar with that of the homogenized billet. This phenomenon can be explained by the following two aspects. Firstly, the grain growth is related to the deformation time, and high strain rate brings short time for grain growth. Secondly, high strain rate produces more dislocations at grain boundaries, resulting in the strong pinning effects on the migration of grain boundary.

    Fig. 6. Size distribution of DRXed grains in samples compressed at (a) 350 °C/0.001 s-1 and (b) 350 °C/0.1 s-1.

    The grain orientation spread (GOS) angle with a threshold value of 5owas set to identify the DRXed grains [27], and the size distribution of the DRXed grains is shown in Fig. 6.As is seen from Fig. 6(a), the number fraction of grains less than 5 μm is 44.08% at the strain of 0.92, while it is 32.58%at the strain of 1.6. In contrary, the number fraction of grains with the size of 5-10 μm is 42.35% at the strain of 0.92,while it is 53.10% at the strain of 1.6. It indicates the growth of DRXed grains, which can be illustrated by a dynamic balance between the storage and annihilation of dislocations[28]. DRX is a discontinuous process that alternates between the storage of strain energy and the formation of recrystallized grains. Hence, the growth of DRXed grains might attribute to the fact that the storage energy is continuously consumed to a relatively low level, resulting in the absence of more DRXed grains. Then, with the increase of strain, the DRXed grains continuously swallowed the other fin grains, and the grain growth took place. Fig. 6(b) shows the samples compressed at a relatively high strain rate of 0.1 s-1. As is seen, the grain size distribution varied slightly with the increase of strain from 0.92 to 1.6, which indicates a steady state of DRX. One important reason for the steady DRX is the high deformation temperature, which is one of the most important factor on determining the size of DRXed grains. The deformation temperature is strongly affected by the level of strain rate. At low strain rate, there is sufficien time for samples to dissipate the deformation heat to environment, and the temperature is kept at a relatively stable level.At high strain rate,large amount of heat is generated due to the severe deformation, and it cannot dissipate during a short time, which results in an obvious temperature rise. In the present study, when the strain rate is 0.1 s-1, the whole compressing process is around 16 s, and the heat induced by plastic deformation cannot dissipate in such a short time. Hence, it can be regarded as a process of adiabatic compression, and the temperature of sample continuously increases with the increasing strain. The temperature rise can be estimated by the following formula [29,30]:

    where ΔT is the change of temperature, η with the value of 0.5 is the adiabatic correction factor,∫ε0 σdεis the area under the true stress-strain curve, ρ with the value of 1.8×10-6kg/mm3is the density, Cpwith the value of 1.3 kJ/kg·K is the specifi heat capacity, and β with the value of 0.95 is the fraction of mechanical work transformed to heat with the remaining fraction going to microstructure evolution. The calculated results about the temperature rise during the compression of 350 °C/0.1 s-1is shown in Fig. 7.It is obvious that the strain of 0.92 corresponds to a temperature rise of 14 °C, while the strain of 1.6 brings the temperature rise of 23 °C. With the increase of strain,more DRXed grains are formed due to the large amount of dislocation energy under the condition of high strain rate.However, high strain and high strain rate also causes an obvious temperature rise, which enhances the degree of grain growth. Hence, due to the combined aforementioned effects,a relatively steady distribution of grain size with the increase of strain is observed in Fig. 6(b).

    Fig. 7. Calculated temperature rise during the hot compression at 350 °C/0.1 s-1.

    Fig. 8 shows the (0001) and (10-10) pole figure of the samples compressed at the conditions of 350°C/0.001 s-1and 350 °C/0.1 s-1. It is obvious that both the strain and strain rate strongly affect the texture, and the texture becomes obvious with the increase of strain. More specificall , the grain orientation is more concentrated on CD, indicating the formation of basal texture. However, the texture intensity varies between the samples with different strain rates. With the increase of strain at 0.001 s-1, the texture intensity firstl increases and then decreases. In contrary, with the increase of strain at 0.1 s-1, the texture intensity continuously increases.Many reports indicated that the orientation of recrystallization grains was disordered, and the occurrence of recrystallization weakened the basal texture [31,32]. As discussed above, the low strain rate of 0.001 s-1facilitates the occurrence of DRX,while the high strain rate of 0.1 s-1reduces the DRX fraction. In order to verify this conclusion, the pole and inverse pole figure of the DRXed grains in Fig. 5(c) are taken out,and the results are shown in Fig. 9. It can be seen that the DRXed grains exhibit random orientations, and most of them deviate from CD, which can decrease the strength of basal texture.

    Fig. 8. (0001) and (10-10) pole figure with the strain of 0.33, 0.92 and 1.6 compressed at 350 °C/0.001 s-1 and 350 °C/0.1 s-1.

    Fig. 9. EBSD map, (0001) pole figur and inverse pole figur of the DRXed grains shown in Fig. 5(c).

    In addition, the split of basal texture is observed in all(0001) pole figures as shown in Fig. 8. This kind of phenomenon has been reported by previous studies that the split of basal texture occurred during hot compression and hot rolling processes [33,34]. In order to provide an in-depth discussion, three peaks close to CD are taken out from the(0001) pole figur with strain of 0.92 at the condition of 350 °C/0.001 s-1, and then the corresponding (0001) and(10-10) pole figure are shown in Fig. 10. It is seen that the strongest peak point of P1 corresponds to large unDRXed grains. The weakest point of P2 corresponds to the small deformed grains, while P3 corresponds to most of the DRXed grains. The pole figure of three peak points are belonged to {0001} or {0001}<11-20>basal texture. It is also seen from Fig. 8 that the {0001}<11-20>texture appears in the basal texture of {0001}. The possible reasons for the split of basal texture are attempted to explain as follows. Firstly, the addition of Zn and Zr elements can change the c/a value of HCP alloy. The value of c/a strongly affects the slip system.It was reported that the basal texture in both pure Zn and pure Zr would split during rolling, where Zn split along RD and Zr split along TD[35,36].These finding are similar with the results shown in Fig. 8, in which TD direction is split.Secondly, the pyramidal <c+a>slip might cause the split of basal texture. It was reported that the pyramidal slip caused the split of basal texture during rolling of ZK60 alloy, which was the main reason for the weakening of basal texture [37].Moreover, the combination of basal {0001}<11-20>slip and pyramidal {-1-122}<11-23>slip in Zn would result in the textures with basal poles titled away from CD towards the deformation direction [35]. The third reason is that the random orientation of DRXed grains weakens the basal texture.Hence, if another preferred orientation appears, the basal texture will be split.

    Fig. 10. (0001) and (10-10) pole figure of three peak points.

    Since the large unDRXed grains correspond to the deviated point with highest intensity in (0001) pole figures two typical unDRXed grains were selected from Fig. 5(e) and 5(f) to further study the influenc of pyramidal slip on basal texture. Fig. 11 shows the grain orientation, pole figure and Schmid factor (SF) maps of the unDRXed grains of G1 and G2, which correspond to the strain of 0.92 and 1.6, respectively. The SF values are classifie into high level (>0.3) and low level (<0.3). It is observed from the EBSD maps that both of these two grains consist of red and yellow regions.When the strain increases to 1.6, some purple regions appear in G2. Based on the inverse pole figure the yellow and purple regions approach the <10-10>and <11-20>directions,respectively. When the strain is as high as 1.6, the appearance of purple region implies that large unDRXed grains have a new tendency to deviate from CD,and the orientation of basal texture is further weakened.Moreover,it is observed that both the pyramidal <c+a>and prismatic <a>slips exhibit high SF values in G1 and G2. It means that the basal slip cannot meet the requirement of plastic deformation, and the pyramidal and prismatic slip systems should be activated. It has been mentioned that when compression reduction is increased,the contribution of basal and prismatic slips on deformation along CD becomes slight. Hence, the pyramidal slip must be activated to make a further deformation [35]. In addition, the occurrence of pyramidal slip is also related to the temperature. The CRSS of pyramidal slip decreases with the increase of temperature, resulting in the easy activation of slip system. It was reported that at high temperatures of 350 °C, the basal slip, pyramidal slip and non-basal cross slip could be found in the original grains of ZK60 alloy [20]. Moreover, it is found that the SF value of pyramidal <c+a>II slip expands to a broad range of 0.2-0.5 at high strain of 1.6, which implies that the pyramidal <c+a>II slip becomes more active.

    As discussed above, the pyramidal slip is an important factor on the split of basal texture. The mechanism can be explained by the rotation of grains during compression. It is well known that the slip plane of grain should rotate during hot compression. If there is only one grain, the grain will deform along the slip direction. However, the existence of surrounding grains or the grain itself restricts the radial deformation. As a result, when the grain is subjected to the force along CD direction, the grain rotation must occur to accommodate the deformation. When the pyramidal slip takes place, the rotation of c-axis can be offset, ensuring a continuous slip. Therefore, the direction of c-axis of the rotating grain deviates from CD. When the grain rotates to a certain angle from the basal plane,the new orientation has an adverse effect on the continuation of pyramidal slip. The orientation after rotation is similar with the state at the initial stage of compression, and then the basal slip will be activated again.As shown in Fig. 11, the change of SF values of basal slip from G1 (ε=0.92) to G2 (ε=1.6) can well explain this phenomenon, and it is reflecte that there is a close relationship between the basal slip and the pyramidal slip in grain rotation. Thus, it is assumed that these two slips at high strain condition will be active alternatively. When the basal slip is not easy to take place, the grain rotation occurs through pyramidal slip.When the grain begins to rotate,its orientation can meet the favorable condition of basal slip, and the basal slip will be activated. Moreover, the revolving of grain around c-axis can be observed, as indicated in the EBSD maps of Fig. 11. During hot compression process, the stress along TD can active the prismatic slip, which causes the grain rotation around c-axis. The combination of c-axis deviating from CD and grain revolving around c-axis causes the split of texture deviating from CD with certain angle. Hence, the pyramidal slip is likely to be an important factor for the split of basal texture.

    Fig. 11. EBSD analysis of the unDRXed grains G1 and G2. Basal <a>: {0001}<11-20>, Prismatic <a>: {10-10}<11-20>, Pyramidal <c+a>I: {10-11}<11-2-3>, Pyramidal <c+a>II: {-1-122}<11-23>.

    3.3. Analysis of microstructure evolution with twinning

    Due to the limited slip systems in Mg alloys, twinning has been theoretically and experimentally proven to be an important mechanism responsible for the plastic deformation[38]. Low temperature and high strain rate are usually beneficia for the formation of twins. Hence, in order to analyze the microstructure with the formation of twins, the curve of 300 °C/1 s-1was selected for examination. The hot compression tests were conducted with the strain of 0.09, 0.13 and 0.25. Fig. 12 shows the EBSD maps, twinning and distribution of misorientation angle.It is observed that plenty of twins and nearly no DRXed grain exist at the strain of 0.09. The fractions of DRX in Fig. 12(a)-(c) are calculated as 0.68%,2.29%, and 9.38%, which indicates that the fraction of DRX increases with the increasing strain. However, it is obviously observed from Fig. 12(d)-(i) that the number of twins decreases with the increasing strain. Moreover, the fraction of misorientation angle less than 10oalso increases, which is caused by slip. The peaks in Fig. 12(g)-(i) around 86° correspond to the {10-12} extension twins, and these peaks decrease with the increase of strain. When the strain reaches 0.25, most of the grains have been reoriented by the twins,and only few grains still retain the original orientations. It was reported that the plastic deformation of Mg alloys at low strain condition was dominated by twinning and grain rotation,which resulted in the twin platelets at grain cores and the distortion zones at grain boundaries [15-17]. When the strain rate becomes higher,twinning becomes more extensive due to the limited time in which the dislocation slip can occur [39].Different from the extruded Mg alloy with lots of extension{10-12} and contraction {10-10} twins [13], large number of extension twins and few contract twins are observed in the present study. Almost all of the {10-12} twins form in grains with <10-10>and <11-20>orientations, which agrees well with the study of Cho et al. [25]. Besides, the fraction of twins in grains with <11-20>orientation is higher than that in grains with <10-10>orientation, indicating that the propagation rate of twinning depends on the grain orientation.

    Fig. 12. EBSD maps, twinning, and distribution of misorientation angle in samples compressed at 300 °C/1 s-1 with the strain of (a) (d) (g) 0.09, (b) (e) (h)0.13 and (c) (f) (i) 0.25. The angular deviation used to identify the twin boundaries is within 5o of the ideal values.

    It is observed from the EBSD maps shown in Fig. 12 that the orientation of twins is almost parallel with CD, which implies that the twins contribute to the rotation of grains at the early deformation stage. Actually, during rolling or compression process,twins reorient the basal plane nearly perpendicular to loading direction,leading to a reorientation of the lattice of 86° [11]. Furthermore, with the increase of strain, lots of DRXed grains formed at the zones with twins, indicating that the twins should be related to the nucleation of recrystallization. In order to illustrate the effects of {10-12} twins, the relationships between twins, parent grains and DRXed grains are discussed. Three typical regions of R1, R2 and R3 are selected from Fig. 12(a), and the EBSD analysis is shown in Fig. 13. The {10-12} twins can be found in all of the grains,and the parent grains are greatly consumed by twins. The(0001) pole figure and inverse pole figure exhibit that the orientation of twins are nearly parallel with CD, which means that the twins contribute to the formation of basal texture at the early deformation stage.

    Fig. 14 shows the texture evolution with the increase of strain at the condition of 300 °C/1 s-1. The basal texture is clearly observed from the pole figure of all samples, and the intensity increases from 5.73 to 7.9 with increasing the strain from 0.09 to 0.25. However, comparing with Fig. 8 without twins,the basal texture forms earlier when the strain rate is as high as 1 s-1. This phenomenon can also be found by comparing Figs. 5 and 12. Fig. 5(a) shows that many grains with original orientation are remained at the strain of 0.33, while Fig.12(c)shows that only few grains with original orientation exist at the strain of 0.25. It indicates that the {10-12} twins contribute to the fast formation of basal texture. As shown in Fig.12(a),plenty of{10-12}extension twins form in the original grains with <10-10>and <11-20>orientations, leading to the rotation of these grains. Finally, the c-axis of theses grains rotate to an angle almost parallel with CD. Besides,the peak point in the pole figur of the sample compressed at 300 °C/1 s-1with strain of 0.13 was analyzed, as shown in Fig. 15. The deviation between the peak point and CD is around 19o, which is caused by the rotation of {10-12} twins.Moreover, the deviated peak point contains some integrated grains caused by basal slip. The above facts indicate that the formation of basal texture is attributed to the twins and basal slip.

    Fig. 13. (0001) pole f gures and inverse pole f gures of regions R1, R2 and R3.

    Fig. 14. (0001), (10-10) pole figure and inverse pole figure of samples compressed at 300 °C/1 s-1.

    Fig. 15. EBSD map, (0001) pole f gure and inverse pole f gure of peak point in sample compressed at 300 °C/1 s-1 with the strain of 0.13.

    In order to demonstrate the DRX induced by {10-12}twins, three typical regions of R1, R4 and R5 were selected from Fig. 12(a), 12(b) and 12(c) respectively for further analysis. The maps and distributions of SF for basal <a>, prismatic <a>, pyramidal <c+a>I and II slip systems are presented in Fig. 16. In these regions, the number of DRXed grains increases when the strain increases from 0.09 to 0.25,and almost all of them formed near the twin boundaries.Meanwhile, R4 and R5 have high-density LAGBs. These two factors indicate that the DRXed grains may form on the interaction boundaries of extension twins and slips [40]. It was reported that the formation of extension twins was closely related to the operative slips [41,42], and it affected the DRX behavior of Mg alloy during hot deformation process. As is seen from Fig. 16, the SF value of basal slip is low in the twining region, indicating that the basal slip is not active.However, the SF values of non-basal slips are very high in twining region, which means that the non-basal slips are active. Some researchers have studied the effects of non-basal slip on the DRX behavior of Mg alloys [42-44]. Lu et al.[42] found that <a>and <c>dislocations from the decomposition of <c+a>intersected with the twin boundaries,which was helpful on accumulating dislocations and formation of DRXed grains. Sanjari et al. [43] reported that the climb or cross-slip of dislocations could be facilitated by the activity of prismatic <a>slip at high temperature, which was necessary for the rearrangement of dislocations into cell and sub-grain boundaries. Yoo et al. [44] proposed that the<c+a>screw dislocations could cross slip from a prismatic plane to a pyramidal plane, and the rearrangement of dislocations caused the formation of network with LAGBs.Hence,in the present study, the twins with non-basal slips are regarded as important factors that facilitate the occurrence of DRX.

    Fig. 16. EBSD analysis of regions R1, R4 and R5.

    4. Conclusions

    The hot compression tests were conducted to study the microstructure evolution of ZK60 Mg alloy.Based on the OM images and EBSD analysis, the main conclusions are drawn as follows.

    (1) The fl w stress increases sharply to a peak point at the initial stage, and then gradually decreases. High temperature and low strain rate result in the decrease of fl w stress. The deformation parameters such as temperature, strain and strain rate significantl affect the microstructure features. Overall, high temperature, high strain and low strain rate increase the DRX fraction,although the complete DRX is not achieved in the present experiments. In addition, the low temperature and high strain rate are beneficia for the formation of twins.

    (2) The twins are not formed at the conditions of 350 °C/0.001 s-1and 350 °C/0.1 s-1. The growth of DRXed grains is obvious at low strain rate of 0.001 s-1,which should be caused by a dynamic balance between the storage and annihilation of dislocations. However,DRX tends to be steady at a high strain rate of 0.1 s-1,due to the combined effects of more deformation heat and fast accumulation of dislocation. The split of basal texture was observed in all samples. The pyramidal<c+a>slip with high SF value is active in large deformed grains,which corresponds to the peak split point in (0001) pole figure indicating the activity of pyramidal slip. The rotation of grains was proposed to explain the relationship between the pyramidal slip and the split of basal texture.

    (3) The {10-12} extension twins are formed during the compression at the condition of 300 °C/1 s-1, and the number of twins decreases with the increase of strain.The twins contribute greatly to the fast formation of basal texture and grain rotation at the early deformation stage. Moreover, the non-basal slips are active in twining region, which can facilitate the nucleation of DRX by climbing and intersecting of prismatic and pyramidal slips.

    Acknowledgments

    The authors would like to acknowledge the financia support from National Natural Science Foundation of China(51875317), Key Research and Development Program of Shandong Province (2019GGX104087), and National Natural Science Foundation of Shandong Province (ZR2019QEE030).

    1024手机看黄色片| 亚洲综合色惰| 日日夜夜操网爽| 人妻少妇偷人精品九色| 18禁在线播放成人免费| 精品久久久久久,| av在线亚洲专区| 中文字幕精品亚洲无线码一区| 成人国产麻豆网| 伊人久久精品亚洲午夜| 欧美极品一区二区三区四区| 日本欧美国产在线视频| 午夜亚洲福利在线播放| av天堂中文字幕网| 又爽又黄a免费视频| 久久国内精品自在自线图片| 成年女人永久免费观看视频| 成人国产麻豆网| 国产一区二区三区av在线 | 嫩草影视91久久| 日韩欧美在线二视频| 亚洲四区av| 中文在线观看免费www的网站| 香蕉av资源在线| 欧美精品啪啪一区二区三区| 久久精品国产鲁丝片午夜精品 | 国产精品久久电影中文字幕| 啪啪无遮挡十八禁网站| 丰满的人妻完整版| 国产极品精品免费视频能看的| 国产在线精品亚洲第一网站| 99久久无色码亚洲精品果冻| 日韩欧美精品免费久久| 日韩精品有码人妻一区| 国产毛片a区久久久久| 日本三级黄在线观看| 99精品久久久久人妻精品| 欧美性猛交黑人性爽| 婷婷色综合大香蕉| 日本黄大片高清| 婷婷亚洲欧美| 国产在线男女| 国内精品久久久久精免费| aaaaa片日本免费| 俄罗斯特黄特色一大片| 日韩欧美精品v在线| 国产老妇女一区| 18+在线观看网站| 欧美潮喷喷水| 国产大屁股一区二区在线视频| 熟女人妻精品中文字幕| 国内毛片毛片毛片毛片毛片| 18禁黄网站禁片免费观看直播| 亚洲国产高清在线一区二区三| .国产精品久久| 国产精品电影一区二区三区| 99热这里只有精品一区| 亚洲国产色片| 我要看日韩黄色一级片| 99久久精品热视频| 国产一区二区三区视频了| 国产伦精品一区二区三区四那| 俺也久久电影网| 日韩欧美三级三区| 亚洲精品在线观看二区| 看免费成人av毛片| 乱码一卡2卡4卡精品| 在线免费十八禁| 国内毛片毛片毛片毛片毛片| 亚洲18禁久久av| 欧美日韩精品成人综合77777| 老熟妇仑乱视频hdxx| 国产精品98久久久久久宅男小说| 日日摸夜夜添夜夜添小说| 又爽又黄a免费视频| 91麻豆av在线| 在线免费观看不下载黄p国产 | 亚洲国产精品久久男人天堂| 久久精品国产亚洲av天美| 亚洲国产精品成人综合色| 成年女人永久免费观看视频| 亚洲熟妇中文字幕五十中出| 国产不卡一卡二| 午夜福利在线在线| 日韩欧美国产一区二区入口| 国内精品美女久久久久久| 又黄又爽又免费观看的视频| 少妇的逼水好多| 国产 一区 欧美 日韩| 成人亚洲精品av一区二区| 久久久国产成人精品二区| 美女 人体艺术 gogo| 久9热在线精品视频| 日本一二三区视频观看| 俺也久久电影网| 日本欧美国产在线视频| 亚洲熟妇熟女久久| 日韩欧美国产在线观看| 在线看三级毛片| 好男人在线观看高清免费视频| 日韩av在线大香蕉| 欧美性猛交黑人性爽| 有码 亚洲区| АⅤ资源中文在线天堂| 99热只有精品国产| 深夜精品福利| 国产一区二区在线观看日韩| 国产午夜精品久久久久久一区二区三区 | 99久久精品国产国产毛片| 亚洲av成人av| 日日撸夜夜添| 国产伦精品一区二区三区视频9| 国产国拍精品亚洲av在线观看| 日本免费一区二区三区高清不卡| 成年版毛片免费区| 老司机深夜福利视频在线观看| 赤兔流量卡办理| 窝窝影院91人妻| 中文字幕人妻熟人妻熟丝袜美| 欧美另类亚洲清纯唯美| 成年免费大片在线观看| 好男人在线观看高清免费视频| 欧美成人一区二区免费高清观看| 18禁在线播放成人免费| 听说在线观看完整版免费高清| 免费高清视频大片| 精品午夜福利在线看| 国产蜜桃级精品一区二区三区| 欧美bdsm另类| 亚洲国产精品sss在线观看| 国产男靠女视频免费网站| 波多野结衣高清无吗| 精品一区二区三区人妻视频| 婷婷精品国产亚洲av| 亚洲va日本ⅴa欧美va伊人久久| .国产精品久久| 在线观看66精品国产| 网址你懂的国产日韩在线| h日本视频在线播放| 三级国产精品欧美在线观看| 不卡一级毛片| 日本免费一区二区三区高清不卡| 97碰自拍视频| 日本色播在线视频| 久久精品夜夜夜夜夜久久蜜豆| 欧美bdsm另类| 国产一区二区在线观看日韩| 国产精品av视频在线免费观看| 无遮挡黄片免费观看| 18禁黄网站禁片免费观看直播| 天堂动漫精品| 91久久精品国产一区二区三区| 校园人妻丝袜中文字幕| 两个人视频免费观看高清| 我要搜黄色片| 一边摸一边抽搐一进一小说| 在线观看午夜福利视频| 午夜激情福利司机影院| 精品人妻熟女av久视频| 蜜桃亚洲精品一区二区三区| 一级黄片播放器| 九九爱精品视频在线观看| 亚洲国产精品久久男人天堂| 精品久久久久久久久久久久久| 久久国产精品人妻蜜桃| 一进一出好大好爽视频| 国产主播在线观看一区二区| 精品国产三级普通话版| 婷婷六月久久综合丁香| 久久久久久伊人网av| 国产精品国产三级国产av玫瑰| 亚洲av免费在线观看| 国产91精品成人一区二区三区| 九九久久精品国产亚洲av麻豆| 天堂√8在线中文| eeuss影院久久| 国产伦精品一区二区三区视频9| 免费av毛片视频| 九九热线精品视视频播放| 国产成人福利小说| 少妇的逼好多水| 天堂√8在线中文| 国产精品精品国产色婷婷| 欧美成人性av电影在线观看| 简卡轻食公司| 一本久久中文字幕| 久久99热这里只有精品18| 国产精品免费一区二区三区在线| 天堂√8在线中文| 国产精品免费一区二区三区在线| 亚洲精品在线观看二区| 成人三级黄色视频| 日本 av在线| 国产成年人精品一区二区| 欧美日韩中文字幕国产精品一区二区三区| 午夜亚洲福利在线播放| 久久午夜福利片| 免费在线观看成人毛片| 日韩欧美国产在线观看| 婷婷亚洲欧美| 久久香蕉精品热| 日本黄色视频三级网站网址| 午夜免费成人在线视频| 精品国产三级普通话版| 日韩欧美三级三区| 乱人视频在线观看| 日韩亚洲欧美综合| 精品人妻一区二区三区麻豆 | 亚洲精品一区av在线观看| 少妇人妻一区二区三区视频| 亚洲精品在线观看二区| 18禁黄网站禁片免费观看直播| 亚洲美女视频黄频| 天堂√8在线中文| 欧美zozozo另类| 国产亚洲av嫩草精品影院| 别揉我奶头~嗯~啊~动态视频| 三级毛片av免费| 蜜桃亚洲精品一区二区三区| 国产色爽女视频免费观看| 91在线观看av| 小说图片视频综合网站| 欧美+亚洲+日韩+国产| av天堂在线播放| 97人妻精品一区二区三区麻豆| 十八禁网站免费在线| 亚洲精品国产成人久久av| 免费看美女性在线毛片视频| 毛片一级片免费看久久久久 | 一级av片app| aaaaa片日本免费| 国产精品永久免费网站| 国产精品人妻久久久久久| 看免费成人av毛片| av.在线天堂| 国产男靠女视频免费网站| 久久亚洲精品不卡| 美女黄网站色视频| 色哟哟·www| 日本 欧美在线| 51国产日韩欧美| 直男gayav资源| 18+在线观看网站| 国语自产精品视频在线第100页| 国内少妇人妻偷人精品xxx网站| 亚洲综合色惰| 嫩草影院新地址| 能在线免费观看的黄片| 天堂影院成人在线观看| 国产免费男女视频| 国产女主播在线喷水免费视频网站 | 精华霜和精华液先用哪个| 有码 亚洲区| 91久久精品国产一区二区三区| 亚洲五月天丁香| 亚洲欧美激情综合另类| 国产综合懂色| 成人永久免费在线观看视频| 99久久久亚洲精品蜜臀av| 午夜a级毛片| 黄色视频,在线免费观看| www.www免费av| 又爽又黄无遮挡网站| 美女被艹到高潮喷水动态| 波野结衣二区三区在线| 成人毛片a级毛片在线播放| 3wmmmm亚洲av在线观看| 丰满乱子伦码专区| 一区二区三区四区激情视频 | 欧美激情久久久久久爽电影| 99精品久久久久人妻精品| 成人二区视频| 亚洲av成人精品一区久久| .国产精品久久| 村上凉子中文字幕在线| 男女做爰动态图高潮gif福利片| 99在线人妻在线中文字幕| 天美传媒精品一区二区| 99精品久久久久人妻精品| 国产在线男女| 22中文网久久字幕| 日韩欧美一区二区三区在线观看| 亚洲五月天丁香| 99热6这里只有精品| 别揉我奶头 嗯啊视频| 国内精品一区二区在线观看| 久久99热这里只有精品18| 欧美xxxx黑人xx丫x性爽| 女的被弄到高潮叫床怎么办 | 亚洲 国产 在线| 国产主播在线观看一区二区| 成人特级av手机在线观看| 亚洲黑人精品在线| 97超级碰碰碰精品色视频在线观看| 精品久久久久久久久久免费视频| 日韩精品中文字幕看吧| 在线观看av片永久免费下载| 免费av毛片视频| 久久天躁狠狠躁夜夜2o2o| 非洲黑人性xxxx精品又粗又长| 国产精品一区二区免费欧美| 熟妇人妻久久中文字幕3abv| 国产三级中文精品| 波多野结衣高清作品| 精品免费久久久久久久清纯| 午夜福利视频1000在线观看| 精品久久久久久成人av| av在线亚洲专区| 色哟哟哟哟哟哟| 国产免费av片在线观看野外av| 少妇猛男粗大的猛烈进出视频 | a级一级毛片免费在线观看| 免费观看在线日韩| 精品一区二区免费观看| 亚洲七黄色美女视频| 少妇熟女aⅴ在线视频| 国产精品人妻久久久久久| 精品一区二区三区人妻视频| 精品一区二区三区人妻视频| 国产高潮美女av| 亚洲成人免费电影在线观看| 亚洲性久久影院| 日韩国内少妇激情av| 嫩草影视91久久| 精品一区二区免费观看| 桃红色精品国产亚洲av| 国产精品永久免费网站| 国产伦在线观看视频一区| 中文字幕av成人在线电影| 老熟妇仑乱视频hdxx| 国产精品亚洲一级av第二区| 午夜福利高清视频| 国产真实伦视频高清在线观看 | 国产单亲对白刺激| 午夜久久久久精精品| 国产大屁股一区二区在线视频| 久久久久久久久中文| 成人毛片a级毛片在线播放| 丰满人妻一区二区三区视频av| 一级毛片久久久久久久久女| 最近最新中文字幕大全电影3| 深夜a级毛片| 春色校园在线视频观看| 免费人成在线观看视频色| h日本视频在线播放| 欧美又色又爽又黄视频| 热99在线观看视频| 在线免费观看的www视频| 我要看日韩黄色一级片| 如何舔出高潮| 日本成人三级电影网站| 免费高清视频大片| 中文字幕精品亚洲无线码一区| 日本一本二区三区精品| 黄色欧美视频在线观看| 色尼玛亚洲综合影院| 日韩,欧美,国产一区二区三区 | 国产蜜桃级精品一区二区三区| 成人性生交大片免费视频hd| 亚洲av成人精品一区久久| 尾随美女入室| 日韩中文字幕欧美一区二区| 日韩一本色道免费dvd| 日韩精品有码人妻一区| 黄色视频,在线免费观看| 亚洲精品乱码久久久v下载方式| 91午夜精品亚洲一区二区三区 | 亚洲国产日韩欧美精品在线观看| 欧美区成人在线视频| 日韩精品青青久久久久久| 久久久成人免费电影| 免费大片18禁| xxxwww97欧美| 成人高潮视频无遮挡免费网站| 免费不卡的大黄色大毛片视频在线观看 | 国产精品亚洲一级av第二区| 亚洲成人中文字幕在线播放| 少妇被粗大猛烈的视频| 欧美zozozo另类| 国产精品一区二区免费欧美| 亚洲电影在线观看av| 国产91精品成人一区二区三区| 少妇猛男粗大的猛烈进出视频 | 丰满的人妻完整版| 久久99热6这里只有精品| 免费无遮挡裸体视频| 日韩中字成人| 最近视频中文字幕2019在线8| 一区二区三区四区激情视频 | 看十八女毛片水多多多| 亚洲成人中文字幕在线播放| 国产成人av教育| 91麻豆av在线| 亚洲精华国产精华液的使用体验 | 九九热线精品视视频播放| 日本一二三区视频观看| 久久久精品大字幕| 亚洲成人中文字幕在线播放| 精品日产1卡2卡| 2021天堂中文幕一二区在线观| 真人一进一出gif抽搐免费| 欧美激情久久久久久爽电影| 亚洲精品色激情综合| 给我免费播放毛片高清在线观看| 91麻豆av在线| 熟妇人妻久久中文字幕3abv| 嫩草影视91久久| 综合色av麻豆| 99热这里只有是精品在线观看| 老熟妇乱子伦视频在线观看| 国产高清有码在线观看视频| 免费av观看视频| 亚洲自偷自拍三级| 欧美中文日本在线观看视频| 亚洲精华国产精华液的使用体验 | 亚洲av第一区精品v没综合| 给我免费播放毛片高清在线观看| 99热这里只有是精品50| av天堂在线播放| 国产真实乱freesex| 成年版毛片免费区| 国国产精品蜜臀av免费| 国产精品久久久久久av不卡| 一级av片app| 老司机深夜福利视频在线观看| 婷婷精品国产亚洲av在线| 亚洲精品国产成人久久av| 欧美中文日本在线观看视频| 亚洲国产高清在线一区二区三| 99久久无色码亚洲精品果冻| 国产av麻豆久久久久久久| 国产私拍福利视频在线观看| 国产美女午夜福利| 日日摸夜夜添夜夜添av毛片 | 男女视频在线观看网站免费| 99久久成人亚洲精品观看| 一区二区三区激情视频| 十八禁网站免费在线| 无人区码免费观看不卡| 精品一区二区三区视频在线观看免费| 欧美性猛交╳xxx乱大交人| 黄色丝袜av网址大全| 亚洲成人免费电影在线观看| 久久中文看片网| 99九九线精品视频在线观看视频| 午夜福利18| 好男人在线观看高清免费视频| 国产精品美女特级片免费视频播放器| 乱人视频在线观看| 国产高清有码在线观看视频| av在线亚洲专区| 乱人视频在线观看| 一个人看的www免费观看视频| 免费观看的影片在线观看| 亚洲成人久久性| 美女 人体艺术 gogo| 波多野结衣高清无吗| 亚洲国产色片| 亚洲中文字幕一区二区三区有码在线看| 91久久精品国产一区二区成人| 国产伦精品一区二区三区四那| 自拍偷自拍亚洲精品老妇| 男插女下体视频免费在线播放| 国产精品99久久久久久久久| 天堂√8在线中文| 免费黄网站久久成人精品| 老熟妇仑乱视频hdxx| videossex国产| 亚洲最大成人中文| 最近视频中文字幕2019在线8| 两性午夜刺激爽爽歪歪视频在线观看| 国产精品国产三级国产av玫瑰| 国产精品久久电影中文字幕| 午夜免费成人在线视频| 国产人妻一区二区三区在| 国产黄片美女视频| 亚洲熟妇熟女久久| 性欧美人与动物交配| 一区二区三区高清视频在线| 美女xxoo啪啪120秒动态图| 国产成人a区在线观看| 亚洲av免费在线观看| 精品久久久久久久久久久久久| 欧美bdsm另类| 久久草成人影院| 亚洲成人久久性| 啪啪无遮挡十八禁网站| 免费在线观看日本一区| eeuss影院久久| 亚洲av免费高清在线观看| 国产伦在线观看视频一区| 亚洲熟妇熟女久久| 久久精品国产鲁丝片午夜精品 | 中国美女看黄片| 精品一区二区三区人妻视频| 又爽又黄无遮挡网站| 五月伊人婷婷丁香| 91精品国产九色| 婷婷精品国产亚洲av在线| 美女cb高潮喷水在线观看| 少妇高潮的动态图| 国产精品三级大全| 国产大屁股一区二区在线视频| 亚洲欧美日韩无卡精品| 久9热在线精品视频| 欧美最新免费一区二区三区| 超碰av人人做人人爽久久| 日日摸夜夜添夜夜添小说| 亚洲内射少妇av| 国产av一区在线观看免费| 搡老岳熟女国产| 欧美丝袜亚洲另类 | 乱系列少妇在线播放| 深夜a级毛片| 国产高清三级在线| 成年女人永久免费观看视频| 啦啦啦韩国在线观看视频| 床上黄色一级片| 大又大粗又爽又黄少妇毛片口| 久久久久久久久久黄片| 欧美另类亚洲清纯唯美| 久久欧美精品欧美久久欧美| 国模一区二区三区四区视频| 亚洲va日本ⅴa欧美va伊人久久| 成人特级av手机在线观看| 日韩欧美国产在线观看| 91麻豆精品激情在线观看国产| 精品99又大又爽又粗少妇毛片 | 国产精品一及| 乱码一卡2卡4卡精品| 日日撸夜夜添| 日韩欧美国产在线观看| 婷婷色综合大香蕉| 亚洲人成网站在线播| 美女大奶头视频| 蜜桃亚洲精品一区二区三区| 男人舔奶头视频| 午夜激情福利司机影院| 国产免费一级a男人的天堂| 久久久久九九精品影院| 99久久九九国产精品国产免费| 亚洲aⅴ乱码一区二区在线播放| 搞女人的毛片| 舔av片在线| 中文字幕高清在线视频| 淫秽高清视频在线观看| 欧美日韩综合久久久久久 | 18+在线观看网站| 超碰av人人做人人爽久久| 亚洲欧美日韩东京热| 欧美性猛交黑人性爽| 久久人妻av系列| 99热只有精品国产| 日本三级黄在线观看| 色噜噜av男人的天堂激情| 婷婷丁香在线五月| 国产精品无大码| 如何舔出高潮| 少妇丰满av| 成人亚洲精品av一区二区| 色噜噜av男人的天堂激情| 国产精品永久免费网站| a级毛片a级免费在线| 亚洲精华国产精华液的使用体验 | 人人妻人人看人人澡| 美女黄网站色视频| 中文字幕免费在线视频6| av在线观看视频网站免费| 精品一区二区三区视频在线| 国产精品综合久久久久久久免费| 别揉我奶头~嗯~啊~动态视频| 成人特级黄色片久久久久久久| 一边摸一边抽搐一进一小说| 两个人的视频大全免费| 欧美极品一区二区三区四区| 有码 亚洲区| 精品久久久久久久人妻蜜臀av| 日韩欧美免费精品| 欧美精品啪啪一区二区三区| 美女xxoo啪啪120秒动态图| 人人妻人人看人人澡| 亚洲内射少妇av| 黄色欧美视频在线观看| 精品午夜福利在线看| 成人美女网站在线观看视频| 国产黄a三级三级三级人| 看片在线看免费视频| 麻豆国产97在线/欧美| 看黄色毛片网站| 日韩欧美免费精品| 欧美三级亚洲精品| 国产v大片淫在线免费观看| 国国产精品蜜臀av免费| 少妇高潮的动态图| 男人的好看免费观看在线视频| 12—13女人毛片做爰片一| 免费在线观看成人毛片| 日本五十路高清| 99热这里只有是精品在线观看| 无遮挡黄片免费观看| 美女高潮的动态| 91av网一区二区| 老司机福利观看| 精品国产三级普通话版| 蜜桃久久精品国产亚洲av| 国产91精品成人一区二区三区| 日韩欧美在线二视频| 久久精品国产亚洲av香蕉五月| 天堂影院成人在线观看| 99在线人妻在线中文字幕| 国产精品国产高清国产av| 午夜激情欧美在线| 免费电影在线观看免费观看| 国产精品亚洲美女久久久| 午夜精品久久久久久毛片777|