    Research on the intermediate phase of 40CrMnSiB steel shell under different heat treatments

    2021-05-06 12:27:20WeibingLiZhichuangChenXiaomingWangWenbinLi
    Defence Technology 2021年3期

    Wei-bing Li,Zhi-chuang Chen,Xiao-ming Wang,Wen-bin Li

    ZNDY of Ministerial Key Laboratory,Nanjing University of Science and Technology,Nanjing,210094,China

    Keywords:Explosive mechanics Mid-explosion recovery experiment Explosion and fracture Heat treatment SEM(Scanning electron microscope)fracture analysis

    ABSTRACT

    1.Introduction

    The dynamic process of expansion and fracture of metal cylindrical shells under high-strain-rate loading has long been a focus of study[1,2].It has been found that the crack initiation and propagation of the metal casings under an explosive loading,are closely related to the mass distribution,the scattering velocity and angle of the fragments[3,4].As early as the 1940s,Mott et al.[5]proposed a theoretical calculation model for the fragment circumferential size based on stress wave theory and probability statistics.Later,Grady et al.[6]further considered that fracturing is not instantaneously completed and thus introduced the cohesive zone model,ultimately establishing a dynamic crushing theory based on energy.Stronge et al.[7]have studied the expansion and fracture characteristics of ST-series and HF-1 steel cylindrical shells after different heat treatment conditions.And the variation law of the fracture strain with the strain rate was obtained.Moreover,the validity of the two types of fracture criterion based on strain(strain rate independent)and energy(strain rate dependent)was compared and analyzed.To more thoroughly understand the mechanism of metal expansion and fracture,some studies have been conducted at the microscopic level.These studies have found that the dynamic response of the metal shell under a high strain rate is closely related to the microstructure of the shell material.For example,Beetle et al.[8],Sun et al.[9],Ren et al.[10]and Sunwoo et al.[11]have observed the fracture morphology characteristics of the casings via SEM and have deduced the metal shell fracture process and/or the material phase transition process.Jin et al.[12]have used high-speed photography and metallographic analysis to research the effect of different tempering conditions on the expansion and fracture characteristics of 45 steel casings under blast loading.Zhu et al.[13]have investigated the fracture mechanism of the 40CrMnSiB steel tempered with different temperatures through high-speed photography experiment and SEM analysis of the recovered fragments.It was found that steel tempered at higher temperatures delayed the generation of the cracks on the casing surface,the occurrence of fracturing and the leakage of the detonation product.However,the high-speed photographic images obtained could not clearly observe the specific distribution of the surface cracks.The microscopic fracture mechanism of the fragment also could not distinguish the difference in the axial direction.Therefore,further study is necessary for the high-strain-rate expansion deformation,crack initiation and fracture mechanism of the warhead.

    Currently,experimental studies of the expansion and fracture process of metal cylindrical shells under a high-strain-rate loading are mostly carried out by optical photography[14,15].Additionally,analyzing the recovered fragments is also a commonly used research method[16,17].Optical photographic technology cannot observe the internal crack initiation position,pattern,and propagation in the shell.Meanwhile,constrained by the optical vision boundaries and the image quality of photographic equipment,the resulting images cannot completely and accurately observe the propagation of the cracks in the entire cylindrical casing.Moreover,under the internal explosive loading,the metal shell will form many small fragments.Thus,it is not possible to completely patch these fragments together into the original shape of the cylindrical shell.And it is also impossible to obtain the axial and circumferential fracture parameters of the shell.According to Reference[18],as early as the 1950s,scholars in the former Soviet Union proposed the idea of applying a massive recovery device to terminate the expansion of the shell at a certain position.In this way,the shell wreckage exhibiting a relatively complete shape can be used to investigate the crack distribution characteristics and the fracture mechanism of the cylindrical shell under a high-strain-rate loading.However,few published test results have been reported in the published literature[19],and the relationship between the tempering temperature and the final fragment formation size needs further study.In order to better to describe the process of initiation cracking phase to the final fragmentation phase under high-strain-rate loading,it is necessary to study the fracture morphology of the metal casings at an intermediate phase.

    In this work,for the 40CrMnSiB steel at different tempering temperatures,a mid-explosion recovery experiment had been designed to recover the mid-state cylindrical shell with crack information.Then,the influence that the tempering temperature has on the fracture characteristics and the distribution of the crack propagation was studied.The variation law of important fracture parameters at different tempering temperatures such as the circumferential divide size was revealed.In addition,the influence of the axial position and tempering temperature on the microscopic fracture characteristics of the shell was discussed using SEM analysis.

    2.Experiment on mid-explosion recovery of metal cylindrical under internal explosive loading

    2.1.Experimental design

    A standard cylinder with a 50 mm inner diameter,an 80 mm length,and a 6 mm thickness was used as the structure of the casings.The CL-20-based pressed composite explosive with a length of 80 mm was employed for detonation,and the detonation point was located at one side of the center of the cylinder.In addition,two end covers constructed of 45# steel were connected to the shell by a screw threading.The specific structure of the warhead is shown in Fig.1.40CrMnSiB alloy steel was used as the casing material,which was tempered at 350 500 or 600°C after quenching at 860°C.Six experimental devices are prepared in the test,two for each tempering temperature.The performance parameters of the shell material under these three different tempering conditions are shown in Table 1.The characteristic parameters of the CL-20-based high-energy explosive are listed in Table 2.

    2.2.Experiment layout

    The experimental layout of the device used for the midexplosion recovery of the intermediate phase of expansion and fracture of the metal cylindrical casing is shown in Fig.2.To effectively compare and analyze the differences between the shell wreckages under the same constraints,the new and same recovery devices made of 60Mn2Si high-strength alloy steel were applied in each experiment.It is important in the design of the recovery device to determine the proper inner diameter of the device.Therefore,the initial inner diameter of the recovery device was confirmed with reference to the theory of Taylor[20].Therein,it is considered that the fracture radius(af)of the cylindrical shell under an explosive loading can be calculated as

    wherea0is the initial outer radius of the cylindrical casing(a0=31 mm);kis the adiabatic constant(k=3);PHis the denotation pressure of the Chapman-Jouguet detonation wave(PH=38.3×103MPa);andσsis the yield strength of the metal casing(σs=1080 MPa,where 40CrMnSiB steel tempered at 500°C was selected as the reference).According to the theory,the outer diameter of the casing at fracture is 97.75 mm.So,the initial inner diameter of the recovery device was chosen to be 100 mm.The warhead was placed at a fixed position in the center of the recovery device.The warhead and device together were placed in an explosion crater with a diameter of 400 mm and a depth of 500 mm.A polyfoam board was placed below the device as a buffer layer to unload the detonation product in the axial direction,and to subsequently reduce the shock effect of the detonation product on the bottom of the device.

    3.The effect of tempering temperature on fracture characteristics of 40CrMnSiB steel cylinder shell

    3.1.Experiment results

    Using the experimental scheme shown in Fig.2,the wreckage of the 40CrMnSiB steel cylindrical shells at the intermediate phase of the expansion and fracture was acquired,and are shown in Fig.3.In the experiment,it was observed that the inner diameter of the recovery device was slightly enlarged under the strong impact of the metal casing.Further,a number of cracks were observed on the inner wall surface of the device but no serious rupture occurred,as shown in Fig.4.These phenomena indicate that the casings did not expand outward substantially after impacting the inner wall of the recovery device.Therefore,the constraint on each of the casings recovered in this way can be considered to be identical.Disregarding the end covers,the recovery rate of the cylindrical shell is greater than 90%,basically achieving complete recovery.Analysis of the recovered wreckage shows that,under the same constraint condition,the degree of crushing of the shell tempered at 350°C is greater than the others.In contrast,the cylindrical shells tempered at 500 and 600°C,which possess high fracture toughness and higher dynamic plasticity,exhibited delayed cracking that resisted crack extension.Thus,the casings recovered by the device are still exhibiting the sliding phase at the moment of recovery.In terms of the overall structural integrity of the recovered shell wreckage,under the same internal explosive loading,the structural integrity of the shell tempered at 500°C is the best,and 350°C is the worst.This means that the complete fracture time of the shell tempered at 500°C was delayed and the corresponding fracture radius was larger.The detonation product can drive the shell tempered at 500°C more adequately before leaking from the cracks.Therefore,compared to the other two shells,the shell after tempering at 500°C has higher kinetic energy originated from detonation products.This conclusion is consistent with that gained in the previous ultra-high-speed photography experiments[9].

    Fig.1.Schematic(left)and photograph(right)of the warhead structure.

    Table 1Main parameters of the shell material used for simulation models[5].

    Table 2Parameters of high-power explosive CL-20.

    Fig.2.Schematic illustration of the experiment(left)and top-view photograph of the actual experiment in the explosion crater prior to detonation(right).

    3.2.Fracture pattern analysis

    Fig.3.Photographs of the wreckage recovered from the metal shells treated at tempering temperatures of(a)350,(b)500 and(c)600°C.

    Fig.4.Photograph of the recovery device after the strong impact of the metal shell showing a wide-angle top view(left)and a close-up top view of the inner wall(right).

    Tempering heat treatment changes the internal microstructure of the material,such as grain size,crystal defects,alloy element solubility,etc.,and initiates the solid phase transition of the material.These subtle changes in the microscopic scale will cause corresponding variations in the macroscopic mechanical properties of the material.Since the fracture separation of materials is a complex cross-scale problem,the variations in the microscopic scale will also have an important impact on the fracture characteristics of the material.Here,it is mainly reflected in the changes of the fracture behavior,fracture pattern and fracture size of the shells caused by the tempering temperatures.The macroscopic fracture characteristics of the shells developed with different tempering temperatures are analyzed,as shown in Figs.5-7.The macroscopic analysis of the wreckage of the shell tempered at 350°C is shown in Fig.5.Two kinds of fracture patterns were observed in the fragments:shear fracture and tensile-shear fracture.In addition,the fracture pattern was not consistent along the axial direction.Fig.5(a)shows that,from the detonation initiation end to the noninitiation end,the radial fracture patterns sequentially exhibited as a dual-directional shear fracture and tensile-shear fracture.The recovery results of the shells tempered at 500 and 600°C are shown in Figs.6 and 7,respectively.The fracture pattern of these shell is essentially a through-type shear fracture.However,owing to the strong restraint of the recovery device,the fracture surfaces have a certain degree of curvature.

    Moreover,the three different shells exhibited a similar phenomenon.It is that many cracks do not penetrate the entire wall thickness and the number of cracks on the inner wall exceed that of the outer wall.Under the explosive loading,the shear crack initiations at the inner wall of the shell and then extend along the shear band to the outer wall.At the same time,the shell on both sides of the crack near the inner wall enter the slide-separated state firstly to form fracture surface 1.According to the unloading wave theory of Mott,at the time of fracture,the unloading wave is released from the fracture and propagated into the shell on both sides of the fracture.The area propagated by the unloading wave is unloaded to the rigid state and the growth of the crack in this area is inhibited.Due to the mutual unloading effect between the cracks,a few cracks with earlier initiation time and higher propagation velocity dominate in the mutual shielding competition.These cracks extend to the outer wall to form sliding fracture surface 2.Finally,resulting in the number of cracks at the inner wall exceeded that at the outer wall,as shown in Fig.8.

    Fig.5.Photographic analysis of the recovered casing tempered at 350°C,showing(a)tensile-shear and dual-directional shear fracture,(b)unidirectional shear fracture and(c)the cracks in the inner surface.

    Fig.6.Photographic analysis of the recovered casing tempered at 500°C,showing the casing in the(a)lateral direction,(b)the interior view and(c)step plate.

    Fig.7.Photographic analysis of the recovered casing tempered at 600°C,showing the casing(a)interior view,(b)outer wall view and(c)a shear fracture.

    3.3.Fracture path analysis

    Fig.8.The fracture pattern of the expanding metal shell.

    Fragments are the final products of crack initiation,growth,and mutual convergence in three-dimensional space.There-fore,the fracture path of the cracks directly determines the shape and size of the final fragments.

    Many axial cracks can be found in the recovered shell wreckage which almost extends throughout the length of the shell.The propagation path of the crack in the axial direction can change several times,forming step plates at local positions,as shown in Fig.6(c).These long axial cracks do not extend from a single fracture source to the entire length of the shell but are instead formed by the convergence of the shear fracture cells that originated at different axial positions[21].Under the high strain rate loading,the fracture pattern of the shell in the radial direction is dominated by adiabatic shear fracture.Since the early fracture initiation in the upstream section has a great influence on the location of the fracture and the fracture pattern in the downstream section.Many long cracks that parallel axial direction are formed in the shell.However,the specific location of the shear fracture cell is also impacted by the microscopic defects of the material.So,the longitudinal propagation paths of these cracks constituted of the cells are not strictly parallel to the central axis of the shell.The faces of the fracture cells are not on the same plane,but each face roughly parallel to the axis,and there is a small circumferential spacing between the adjacent faces,as shown in Fig.9.After the shear fracture actuated,the medium surrounding the cells is unloaded and restored to a rigid state when these shear fracture cells propagated in the axial direction.The crack propagation energy is provided by the plastic deformation energy in the medium.The material in the rigid state cannot continue to provide energy for the crack propagation.Leading to the adjacent fracture cells cannot intrude into each other’s unloading area in the original propagation direction at the t3moment.However,owing to the weak region between the two crack tips,at the t4 moment,the stress field at the crack tip changes under the sustained action of the shells on both sides of the crack,resulting in circumferential tear behavior.The tearing along the circumferential direction finally achieves the mutual convergence of the fractured cells and forms a nearly vertical step-like fracture feature.

    3.4.Analysis of the influence of tempering temperature on fracture parameters

    The fracture parameters of the shell wreckage including the following aspects:the linear distance between adjacent shear fracture surfaces,Lt(i.e.,the circumferential divide size of the shell);the thickness of the recovered wreckage(δ);the number of circumferential divisions(Nc),which are illustrated in Fig.8.These parameters can be used to evaluate the performance of the warhead to form fragments in the circumferential direction.However,before measuring and analyzing these fracture parameters,it is necessary to investigate the effect that hard-recovery experiment may have on these parameters.According to the fracture morphology of the recovered shell wreckage,fracture surface 2 had slipped out of the shell outer wall to a large extent.Although the recovery device inevitably had a strong impact on the shell during the freezing process,the wall surface and the fracture surface on the outside of the shell can still be easily distinguished.The number of circumferential divisions can be determined,subsequently.Considering the changes of the shape and size of the outer wall surface of the shell caused by the strong impact.The linear distanceLsbetween two adjacent shear cracks on the inner wall surface was directly measured.Then,the circumferential divide sizeLtwas gained by the following equation:

    In order to study the changes of shell fracture parameters caused by different tempering temperatures,the region near the central position on the inner wall of the shell was selected as the statistical location(i.e.,the area between B and C in Fig.6(b)).Fifty cracks were selected in each shell,and the linear distances between the adjacent cracks on two different cross-sections were directly measured and recorded.Then the linear distance between adjacent shear fracture surfaces(Lt)was gained by the Eq.(2).Therefore,a total of 100 statistical samples were acquired in each of the shells,which are shown in Fig.10.Additionally,the average thickness(δave)and the number of circumferential divisions(Nc)of the recovered wreckage was also measured and calculated.These data are listed in Table 3 together with the average circumferential divide size(Lave).

    Combined with the data given in Fig.10 and Table 3,in the initial stage,the increasing tempering temperature(from 350°C to 500°C)significantly improves the dynamic plasticity and fracture toughness of the 40CrMnSiB steel.Thus,the shell easily enters a yield state under internal explosive loading.The expansion radius of the shell and the corresponding fracture characteristic parameter changes distinctly.Laveincreases from 3.18 mm to 3.56 mm(increased by 11.9%);δavedecreases from 3.79 mm to 3.44 mm(reduced by 9.2%),and the corresponding fracture strain(εf)increases from 0.37 to 0.43(whereinis the initial thickness of the casing);Ncdecreases from 84 to 73(decreased by 16.1%).However,when the tempering temperature further increased from 500°C to 600°C,the effect of the decrease in the dynamic strength of the material caused by the heat treatment will become obvious.And partially cancel out the influence caused by the improvement of the dynamic plasticity and fracture toughness.Finally,leading to an unobvious change of the fracture characteristic parameters.Laveincreases from 3.56 mm to 3.64 mm(increased by 2.2%);δaveincreases from 3.44 mm to 3.54 mm(increased by 2.9%),and the corresponding fracture strain(εf)decreases from 0.43 to 0.41;Ncincreased from 73 to 75.

    Fig.9.The representation of the growth and convergence of the adjacent shear fracture cells.

    Fig.10.Distribution of the circumferential divide size of the shells with different tempering temperatures.

    Table 3The fracture characteristic parameters of the shell wreckage.

    In order to theoretically predict the average circumferential size of the recovered fragments under high strain rate loading,based on the Mott unloading wave theory,Grady[14]further considers that the fracture is not instantaneously completed.The material fracture energy(Gc)that based on the cohesive force model is introduced to a one-dimensional ideal rigid-plastic rod.The characteristic time of the fracture is deduced,twice the Mott unloading wave propagation distance within this time is the average circumferential size of the fragments.The formula for predicting the average circumferential size of fragments at a high strain rate proposed by Grady is given as

    whereLGradyis the average circumferential size of the fragments;ρ is the material density;˙εis the average circumferential tensile strain rate at the fracture time;Gcis the fracture energy,for the shear fracture,it is given as[22].

    wherecis specific heat capacity;αis thermal softening coefficient;χis the thermal diffusion coefficient,χ=k/(ρc),kis the thermal conductivity;Yis the flow stress;˙γis the shear strain rate,which can use the circumferential tensile strain rate(˙ε)as an approximation[23].According to reference[24],at the fracture time,the circumferential tensile strain rate of the shells tempered at 350°C,500°C and 600°C is 4.94×104s-1,5.3×104s-1,5.25×104s-1,respectively.The relevant fracture energy parameters of 40CrMnSiB steel for different tempering states are shown in Table 4.The experimental and theoretical values of the average circumferential divide size are plotted in Fig.11.

    From the data in Fig.11,when the tempering temperature increases,the predicted value of the average circumferential divide size based on the Grady model is gradually reduced,while the experimental value is gradually increased.In addition,for the casing tempered at 350°C,the difference between the theoretical values and experimental values is the largest,reaching 25.0%.As the tempering temperature increases from 350°C to 500°C,the fracture energy of the material decreases continuously.The theoretical solution of the circumferential size of the fragments based on the fracture energy also decreases accordingly.Owing to the complexity of the material fracture problem,the circumferential size of the fragments cannot be described simply by the fracture energy.It is also necessary to give a certain explanation from the microscale for the actual fracture problem.

    After quenching at 860°C,the microstructure of 40CrMnSiB steel consisted of quenched-martensite and a small amount of retained austenite.The martensitic phase transition temperature of 40CrMnSiB steel isMs=362°C.Therefore,at the tempering temperature of 350°C,only austenite transformed,the content of martensite almost unchanged,and the final microstructure is tempered-martensite.Martensite has high strength but poor toughness,making the material more prone to brittle fracture under high strain rate loading.This fracture property is somewhat different from the cohesive fracture model,resulting in a larger difference in the result.When the tempering temperature increased to 500°C and 600°C,the martensite gradually decomposed and finally formed tempered troostite composed of ferrite matrix and fine-grained cementite.Although the strength of ferrite matrix is low,its toughness is good,and plastic deformation is easy to occur.Under high strain rate loading,the ductile fracture is more likely to happen,which is consistent with the cohesive force fracture model used by Grady calculation model well.

    4.Observation and analysis of microstructure of recovered shell wreckage

    4.1.Microscopic fracture mechanism of fractures at different axial positions

    To study the microscopic fracture mechanisms at different axial positions,the shell wreckage tempered at 350°C was selected as the research object.The fracture surfaces at the detonation initiation end(Fig.12)and that near the middle(Fig.13)were observed carefully by a FEI Quanta 250FEG SEM equipped with an EDS system.Fig.12 shows that the fracture surfaces near the initiation end have distinctly different fracture characteristics at different locations.The area near the outer wall(area A in Fig.12(a)and(b))andthe area near the inner wall(area B in Figs.10(a),Fig.12(c))were magnified and characterized.The fracture surface in Fig.12(c)does not exhibit the typical dimples caused by shear fracturing,but instead presents a flow-like structural feature with obvious directionality.Under the great pressure impact of the detonation products,the shear cracks near the inner wall are guided by adiabatic shear bands during fracture.Accompanied by the formation of these adiabatic shear bands,severe plastic deformation occurs in the in-band organization and generates the temperature effect.The material in the band is softened but still maintaining a“weak continuous”state.Subsequently,the relative movement of the shells on both sides of the shear band eventually leads to the generation of cracks that then extend along the shear band.Therefore,the direction of the flow structure is related to the relative movement direction of the casing in the relative sliding state.Further observation reveals that the direction of the flow-like structure is not always in the radial direction of the cylindrical casing.Signifying that,in the relative sliding state,the relative movement of the casing near the detonation position is not only along the radial direction.In particular,the closer the casing is to the inner wall,the greater the axial motion component of the relative motion.Fig.12(b)shows a number of scratches whose extension direction are parallel to the radial direction of the casing.These occur because the fracturing in the vicinity of area A in Fig.12(a)is formed after the shell collides with the recovery device.During the collision process,the strong interaction between the shell material on both sides of the fracture caused the fracture surface to be severely squeezed and scraped,ultimately forming scratches.

    Table 4Relevant parameters of shear fracture energy.

    Fig.11.The comparison of the average circumferential divide size between experiment and Grady model.

    Fig.12.SEM images of the fracture near the initiation end showing(a)a wide-angle view and(b,c)a higher-definition view of the areas marked in(a)as(b)area A and(c)area B.

    Fig.13.SEM images of the fracture near the middle of the casing showing a wide-angle view(left),and a higher-definition view of the area marked C(middle)and marked D(right).

    Fig.13 shows the fracture surface observed near the middle of the shell.Two types of steps in the radial and longitudinal directions could be observed in Fig.13(a).To study the formation mechanism of these two steps,the fracture surface of two areas(marked C and D in Fig.13(a))was further magnified for characterization in Fig.13(b)and(c),respectively.The fracture morphology in Fig.13(b)appears as mostly an uncharacteristic flat surface,also known as a flat or extended area,which is a typical feature of a sliding separation fracture.Fig.13(c),however,exhibits flow-like structural features whose direction is approximately parallel to the radial direction(i.e.,going from the inner wall to the outer wall),whereby it is inferred that the fracture initiation point is near the inner wall.Contrasting Fig.13(b)and(c),the microscopic fracture characteristics of the upper and lower sides(i.e.,areas C and D in Fig.13(a))of the radial step differ significantly.This reflects the microscale nature of the axial cracks being made up of many tiny crack cells that are relatively independent.Expansion of a crack always follows the principle of least energy consumption,and the formation of the steps requires the consumption of additional energy.So the height of these radial steps gradually decreased along the radial direction until disappeared,and eventually formed larger longitudinal crack cells.To investigate the formation mechanism of a longitudinal step,the flow-like structural features of the left and right sides of the longitudinal step in Fig.13(c)were studied.No difference is apparent between the two flow-like structures in this direction from the inner wall to the outer wall.Therefore,the possibility can be eliminated that two cracks extending from opposite directions converge to form the step.The longitudinal steps were instead caused by a change of the crack propagation path,which originated near the inner wall.The propagation path of the crack always follows the shear band,and the specific choice also follows the principle of least energy consumption.

    The fracture morphologies of the two axial positions of the initiation end(Fig.12)and the middle position(Fig.13)were compared and analyzed.The fracture surface at the initiation end of the shell has a distinct tearing feature,and the flow-like structure near the inner wall is approximately along the longitudinal direction.Nevertheless,the direction of the flow-like structure near the middle of the shell exhibits a substantial radial direction.From these microscopic fracture characteristics,affected by the axial sparse wave,the fracture behavior of the shell at the initiation position is different from that of the middle position.Near the middle position of the casing,the shear crack cells form at the area near the inner wall and extend radially.Meanwhile,these crack cells gradually converge in the axial direction and ultimately run through the entire wall thickness.In contrast,the fracture at the detonation initiation end is formed by tearing along the crack,which occurs a distance from the initiation position and propagates along the axis direction.

    4.2.Comparison of SEM images of the shell wreckage tempered at different temperatures

    Fig.14 shows higher-resolution SEM images of the wreckage of shells tempered under three different temperatures.The flowstructure characteristics are more obvious in the fracture surface of the shell tempered at 350°C.The temperature of the internal organization of the adiabatic shear band is related to the flow stress of the material.In this relation,a greater flow stress in the material induces more plastic deformation work performed by the local deformation of the band and a higher amount of generated heat[18].After 350°C tempering,the strength of the material is higher than that of the other two materials,and therefore more heat is generated during the formation of the shear bands.Correspondingly,more serious melting occurs in the microstructure at the fracture surface,resulting in more prominent flow characteristics.In addition,there are a large number of spherical particles coated with bright contrast matter(i.e.,white color in Fig.14)on the fracture surface.Energy dispersive X-ray spectral analysis concludes that these spherical particles are likely alloy carbides precipitated from the carbon-rich quench-induced martensite created in the tempering process,wherein the specific composition is shown in Table 5.Owing to the natural oxidation of the sample placed in the air for a long time,the oxygen element content of the alloying carbides is abnormally high.The precipitation of alloy carbides is positively correlated with the tempering temperature,so the number of carbide particles in the shell after tempering at 600°C is the largest,as shown in Fig.14(c).Alloying carbides precipitated during the tempering process can improve the strength of the steel by means of dispersion strengthening.However,it cannot completely offset the reduction in the strength caused by the decomposition of the quenched martensite.Therefore,the strength of 40CrMnSiB steel decreases gradually as the tempering temperature is increased.

    5.Conclusions

    (1)In this paper,a mid-explosion recovery experiment for 40CrMnSiB steel cylindrical shells with different tempering temperatures under an internal explosive loading was designed.The mid-state morphology of the shells was successfully obtained.It is found that the recovered shell wreckage after tempering at 500°C has the best overall structural integrity.This means that after tempering at 500°C,the shell can obtain higher energy from the detonation products,and the fragmentation performance is better,which can provide references and guidance for the selection of shell materials for fragment warhead.

    Fig.14.SEM images showing microscopic fractures of the shell after a tempering temperature of(a)350,(b)500 and(c)600°C.

    Table 5Chemical elements of the spherical phase.

    (2)The radial fracture patterns of the three shells are dominated by adiabatic shear fractures,and meanwhile,accompanied by some tensile-shear fracture.The process of converging adjacent two shear fracture cells to form a step-like fracture characteristic is revealed.The effect of tempering temperature on the fracture characteristic parameters of shell wreckage including the circumferential divide size,the thickness,and the number of circumferential divisions was obtained.When the tempering temperature increased from 350°C to 500°C,the circumferential divide size increased by 11.9%,the average thickness decreased by 9.2%,and the number of circumferential divisions decreased by 16.1%.When the tempering temperature continued to increase to 600°C,the corresponding fracture feature parameters did not change significantly.

    (3)The SEM investigation of the fracture morphology of the 40CrMnSiB steel shell with different tempering temperatures was conducted.With increasing tempering temperature,the flow-like structure characteristics of the fracture surface was less obvious and the amount of alloying carbide that precipitated during the tempering process increased.This increased carbide precipitation resulted in an increased number of spherical carbide particles scattered around the fracture surface.Comparing the microscopic fracture characteristics of different axial positions of the shell tempered at 350°C,it is found that the fracturing near the middle position comprises a plurality of radial shear fracture units.In contrast,the fracture at the initiation end was formed by tearing along the crack,which originated at a distance from the initiation end and propagated along the axis direction.

    Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgment

    The work presented in this paper has been funded by the National Natural Science Foundation of China(Grant No.11972018),and sponsored by the Defense Pre-Research Joint Foundation of Chinese Ordnance Industry(Grant No.6141B012858).

    精品国内亚洲2022精品成人| 免费人成在线观看视频色| 国产久久久一区二区三区| 黑人欧美特级aaaaaa片| 手机成人av网站| 国产男靠女视频免费网站| 日本 av在线| 亚洲av一区综合| 成年人黄色毛片网站| 夜夜夜夜夜久久久久| 99久久成人亚洲精品观看| 日韩国内少妇激情av| 1000部很黄的大片| АⅤ资源中文在线天堂| 精品熟女少妇八av免费久了| 中文字幕久久专区| 国产高清视频在线播放一区| 少妇的逼好多水| 嫩草影院入口| svipshipincom国产片| 两性午夜刺激爽爽歪歪视频在线观看| 国产真实伦视频高清在线观看 | 97人妻精品一区二区三区麻豆| 有码 亚洲区| 一本一本综合久久| 淫妇啪啪啪对白视频| 成年版毛片免费区| 国产伦精品一区二区三区视频9 | 在线国产一区二区在线| 欧美一区二区精品小视频在线| 亚洲,欧美精品.| 久久精品91无色码中文字幕| 日本在线视频免费播放| 国产乱人伦免费视频| 丁香欧美五月| 精品免费久久久久久久清纯| 99久国产av精品| 麻豆一二三区av精品| 亚洲电影在线观看av| 国产欧美日韩一区二区三| 51午夜福利影视在线观看| 国产成人av教育| 欧美潮喷喷水| 91久久精品电影网| 亚洲熟妇中文字幕五十中出| 国产精品熟女久久久久浪| 午夜精品国产一区二区电影 | 黄色日韩在线| 哪个播放器可以免费观看大片| 狂野欧美激情性xxxx在线观看| 成人av在线播放网站| 最近最新中文字幕大全电影3| 国产精品.久久久| 亚洲精品成人久久久久久| 免费看美女性在线毛片视频| 建设人人有责人人尽责人人享有的 | 高清午夜精品一区二区三区| 日韩大片免费观看网站| 好男人在线观看高清免费视频| 十八禁国产超污无遮挡网站| 中文天堂在线官网| 国产高清国产精品国产三级 | 大香蕉97超碰在线| 国产成人精品一,二区| 在线天堂最新版资源| 国产成人91sexporn| 国产成人a∨麻豆精品| 欧美高清性xxxxhd video| 看免费成人av毛片| 久久精品夜夜夜夜夜久久蜜豆| 综合色丁香网| 久热久热在线精品观看| 久久久久久久久久久免费av| 国产精品一及| 简卡轻食公司| 欧美激情国产日韩精品一区| 成人国产麻豆网| 日日干狠狠操夜夜爽| 久久草成人影院| 搞女人的毛片| 亚洲国产av新网站| 国产在视频线精品| 中文字幕久久专区| 91aial.com中文字幕在线观看| 欧美日韩视频高清一区二区三区二| 啦啦啦啦在线视频资源| 一个人看的www免费观看视频| 国产精品av视频在线免费观看| 久久韩国三级中文字幕| av在线老鸭窝| 日韩欧美 国产精品| 又粗又硬又长又爽又黄的视频| 性色avwww在线观看| 午夜久久久久精精品| 天堂中文最新版在线下载 | 国产亚洲一区二区精品| 久久久欧美国产精品| 纵有疾风起免费观看全集完整版 | 亚洲国产精品国产精品| 亚洲电影在线观看av| 久久久久久久久久黄片| 国产精品美女特级片免费视频播放器| 久久久欧美国产精品| 亚洲精品亚洲一区二区| 丝袜美腿在线中文| 99热这里只有是精品50| 只有这里有精品99| 少妇猛男粗大的猛烈进出视频 | .国产精品久久| 亚洲av成人精品一二三区| 亚洲高清免费不卡视频| 成人一区二区视频在线观看| 男女边摸边吃奶| 麻豆国产97在线/欧美| 熟女人妻精品中文字幕| 内射极品少妇av片p| 亚洲自拍偷在线| 国产av国产精品国产| 日本三级黄在线观看| 在线a可以看的网站| 亚洲欧美成人综合另类久久久| 毛片一级片免费看久久久久| 国产成人a区在线观看| 在线观看av片永久免费下载| 超碰av人人做人人爽久久| 少妇熟女欧美另类| 亚洲色图av天堂| 九九久久精品国产亚洲av麻豆| 成人无遮挡网站| 午夜久久久久精精品| 永久免费av网站大全| 91久久精品国产一区二区三区| 女人被狂操c到高潮| 国产精品99久久久久久久久| 国产精品av视频在线免费观看| 婷婷色综合www| 国产探花在线观看一区二区| 精品人妻视频免费看| 69人妻影院| 99久久人妻综合| 国产一级毛片七仙女欲春2| 91久久精品国产一区二区三区| 干丝袜人妻中文字幕| 亚洲欧美日韩东京热| 国产伦精品一区二区三区视频9| 国内精品宾馆在线| 国产淫语在线视频| 亚洲自拍偷在线| 大片免费播放器 马上看| 丝瓜视频免费看黄片| 欧美xxⅹ黑人| 搡老妇女老女人老熟妇| 又黄又爽又刺激的免费视频.| 日韩av不卡免费在线播放| 18禁在线播放成人免费| 久久人人爽人人片av| 精品人妻一区二区三区麻豆| av网站免费在线观看视频 | 成人性生交大片免费视频hd| 伊人久久精品亚洲午夜| 丰满人妻一区二区三区视频av| 五月天丁香电影| 午夜视频国产福利| 久久这里只有精品中国| 麻豆成人午夜福利视频| www.av在线官网国产| 美女国产视频在线观看| 成人鲁丝片一二三区免费| 人人妻人人澡人人爽人人夜夜 | 久久久久久久国产电影| 永久网站在线| 啦啦啦中文免费视频观看日本| 直男gayav资源| 国产成人精品久久久久久| 国产精品爽爽va在线观看网站| 如何舔出高潮| 欧美xxⅹ黑人| 欧美激情在线99| 高清在线视频一区二区三区| 亚洲av中文av极速乱| 91在线精品国自产拍蜜月| 日韩欧美国产在线观看| 人人妻人人澡欧美一区二区| 午夜老司机福利剧场| av专区在线播放| 婷婷色综合大香蕉| 久久久久精品性色| 欧美不卡视频在线免费观看| 一级片'在线观看视频| 三级国产精品片| 亚洲成色77777| 国产av不卡久久| a级毛色黄片| 免费av不卡在线播放| 国产av不卡久久| 女人被狂操c到高潮| 老司机影院毛片| 床上黄色一级片| 91精品国产九色| 国产精品久久久久久久电影| 综合色丁香网| 免费人成在线观看视频色| 精品人妻视频免费看| 一本久久精品| 亚洲国产日韩欧美精品在线观看| 七月丁香在线播放| 国产精品伦人一区二区| 国产高潮美女av| 综合色丁香网| 午夜免费观看性视频| 看非洲黑人一级黄片| 亚洲av免费高清在线观看| 中文字幕av在线有码专区| 黄片wwwwww| 国产亚洲精品久久久com| 国产精品不卡视频一区二区| 亚洲av.av天堂| 最近2019中文字幕mv第一页| 人体艺术视频欧美日本| 欧美一区二区亚洲| 精品国内亚洲2022精品成人| 在线观看一区二区三区| 99热全是精品| 亚洲av日韩在线播放| 欧美性猛交╳xxx乱大交人| av黄色大香蕉| 日韩欧美精品v在线| 国产在视频线精品| 大香蕉久久网| 最近视频中文字幕2019在线8| 国产91av在线免费观看| 只有这里有精品99| 国产精品久久久久久精品电影小说 | 啦啦啦啦在线视频资源| 国产乱人视频| 好男人在线观看高清免费视频| 国产精品99久久久久久久久| 又粗又硬又长又爽又黄的视频| 蜜桃亚洲精品一区二区三区| 国产高潮美女av| 一夜夜www| 免费av不卡在线播放| 国产精品三级大全| 天堂影院成人在线观看| 看非洲黑人一级黄片| 久99久视频精品免费| 国产精品1区2区在线观看.| 综合色av麻豆| 直男gayav资源| 亚洲精品aⅴ在线观看| 亚洲欧美日韩卡通动漫| 日日摸夜夜添夜夜添av毛片| 亚洲av成人av| 中文在线观看免费www的网站| 日产精品乱码卡一卡2卡三| 婷婷色综合www| 精品少妇黑人巨大在线播放| a级毛片免费高清观看在线播放| 久久精品国产鲁丝片午夜精品| 亚洲精品乱码久久久久久按摩| 嫩草影院入口| 麻豆成人av视频| 中文精品一卡2卡3卡4更新| 久久草成人影院| 麻豆久久精品国产亚洲av| 国产免费视频播放在线视频 | 日日干狠狠操夜夜爽| 亚洲三级黄色毛片| 美女黄网站色视频| 久久久久久久久久久丰满| 国产极品天堂在线| 日本欧美国产在线视频| 久久久久久久久久久免费av| 最近视频中文字幕2019在线8| 丝袜喷水一区| 99热网站在线观看| 国产精品国产三级国产专区5o| 欧美三级亚洲精品| 色播亚洲综合网| 联通29元200g的流量卡| 美女黄网站色视频| 18禁动态无遮挡网站| 寂寞人妻少妇视频99o| 91精品伊人久久大香线蕉| 尾随美女入室| 国产av不卡久久| 蜜桃久久精品国产亚洲av| 91午夜精品亚洲一区二区三区| 色播亚洲综合网| 看黄色毛片网站| 97超视频在线观看视频| 丝瓜视频免费看黄片| 国产av在哪里看| 久久久久九九精品影院| 国产白丝娇喘喷水9色精品| 欧美一区二区亚洲| 日韩在线高清观看一区二区三区| 国产精品三级大全| 青春草视频在线免费观看| 一级毛片 在线播放| 晚上一个人看的免费电影| 亚洲精品日韩在线中文字幕| 成年人午夜在线观看视频 | 日本爱情动作片www.在线观看| 久久精品熟女亚洲av麻豆精品 | 久久久久久久国产电影| 日本色播在线视频| 超碰97精品在线观看| 边亲边吃奶的免费视频| 亚洲va在线va天堂va国产| 少妇熟女aⅴ在线视频| 国产一区二区亚洲精品在线观看| 免费观看精品视频网站| 国产欧美另类精品又又久久亚洲欧美| videos熟女内射| 婷婷色综合大香蕉| 久热久热在线精品观看| 国产精品福利在线免费观看| 99热全是精品| 国产乱人视频| 乱系列少妇在线播放| 国产精品久久久久久久电影| 久久韩国三级中文字幕| 少妇高潮的动态图| 少妇裸体淫交视频免费看高清| 久久这里有精品视频免费| 国产 亚洲一区二区三区 | 免费在线观看成人毛片| 身体一侧抽搐| 亚洲四区av| 白带黄色成豆腐渣| 啦啦啦中文免费视频观看日本| 中文资源天堂在线| av在线天堂中文字幕| 国产在线男女| 97在线视频观看| 免费少妇av软件| 七月丁香在线播放| 国产精品麻豆人妻色哟哟久久 | 精品国内亚洲2022精品成人| 国产成人精品婷婷| 男女那种视频在线观看| 高清日韩中文字幕在线| 国产大屁股一区二区在线视频| av国产免费在线观看| 非洲黑人性xxxx精品又粗又长| 人妻夜夜爽99麻豆av| 一本久久精品| 美女脱内裤让男人舔精品视频| 国产精品久久久久久av不卡| 18+在线观看网站| 国产一区二区亚洲精品在线观看| 午夜免费男女啪啪视频观看| 我要看日韩黄色一级片| 久久亚洲国产成人精品v| 亚洲最大成人av| 亚洲人成网站在线观看播放| 淫秽高清视频在线观看| av在线亚洲专区| 最近视频中文字幕2019在线8| 免费av观看视频| 国产亚洲最大av| 波多野结衣巨乳人妻| 一级毛片电影观看| 91精品一卡2卡3卡4卡| 男女国产视频网站| 中文资源天堂在线| 欧美一区二区亚洲| 成人高潮视频无遮挡免费网站| 视频中文字幕在线观看| 国产一区二区三区综合在线观看 | 搡老乐熟女国产| 午夜视频国产福利| 18禁在线播放成人免费| 人妻制服诱惑在线中文字幕| 亚洲国产精品成人综合色| 看免费成人av毛片| 18禁在线无遮挡免费观看视频| 亚洲色图av天堂| 男女视频在线观看网站免费| 三级男女做爰猛烈吃奶摸视频| 欧美成人a在线观看| .国产精品久久| 丰满少妇做爰视频| 亚洲第一区二区三区不卡| 国内精品宾馆在线| 国产乱人视频| 成人鲁丝片一二三区免费| 亚洲国产精品sss在线观看| 极品教师在线视频| 久久久成人免费电影| 天堂影院成人在线观看| 国产亚洲91精品色在线| 少妇的逼水好多| 亚洲精品国产成人久久av| 亚洲国产日韩欧美精品在线观看| 最近中文字幕高清免费大全6| 成人高潮视频无遮挡免费网站| 亚洲国产精品成人综合色| .国产精品久久| 亚洲va在线va天堂va国产| 日本-黄色视频高清免费观看| 国产精品熟女久久久久浪| 1000部很黄的大片| 秋霞在线观看毛片| 免费观看a级毛片全部| 亚洲av电影不卡..在线观看| 高清日韩中文字幕在线| 联通29元200g的流量卡| 久久久精品欧美日韩精品| 伦精品一区二区三区| 日本爱情动作片www.在线观看| 岛国毛片在线播放| 最近手机中文字幕大全| 国内少妇人妻偷人精品xxx网站| 99热6这里只有精品| 日产精品乱码卡一卡2卡三| 麻豆av噜噜一区二区三区| 国产 一区精品| 18禁动态无遮挡网站| 精品久久久久久电影网| 国产色婷婷99| 噜噜噜噜噜久久久久久91| 91狼人影院| 久久97久久精品| 久久热精品热| 久久精品夜色国产| 街头女战士在线观看网站| 国产精品伦人一区二区| 色综合亚洲欧美另类图片| 国产精品麻豆人妻色哟哟久久 | 成人高潮视频无遮挡免费网站| av卡一久久| 美女脱内裤让男人舔精品视频| 一个人观看的视频www高清免费观看| av天堂中文字幕网| 毛片女人毛片| 日韩av不卡免费在线播放| 啦啦啦啦在线视频资源| 亚洲国产av新网站| 成人综合一区亚洲| av在线天堂中文字幕| www.av在线官网国产| 国模一区二区三区四区视频| 成人毛片a级毛片在线播放| 亚洲精品第二区| 国产午夜精品久久久久久一区二区三区| 午夜福利成人在线免费观看| 国产精品国产三级国产av玫瑰| 国产探花在线观看一区二区| 久久综合国产亚洲精品| 亚洲色图av天堂| 禁无遮挡网站| 国产极品天堂在线| 亚洲久久久久久中文字幕| 美女国产视频在线观看| 久久这里有精品视频免费| av在线天堂中文字幕| 99久久九九国产精品国产免费| 最近手机中文字幕大全| 男人舔奶头视频| 欧美 日韩 精品 国产| 久久久久久久久大av| 欧美潮喷喷水| 最近中文字幕高清免费大全6| av天堂中文字幕网| 乱系列少妇在线播放| 亚洲成人精品中文字幕电影| 精品人妻一区二区三区麻豆| 国产精品日韩av在线免费观看| 亚洲,欧美,日韩| 美女内射精品一级片tv| 我的老师免费观看完整版| 建设人人有责人人尽责人人享有的 | 日本一本二区三区精品| 嫩草影院精品99| 岛国毛片在线播放| 国产精品嫩草影院av在线观看| 国产爱豆传媒在线观看| 欧美日韩亚洲高清精品| 国产精品久久久久久久久免| 天堂中文最新版在线下载 | 亚洲精品一区蜜桃| 亚洲内射少妇av| 99re6热这里在线精品视频| 欧美xxxx黑人xx丫x性爽| 国产精品综合久久久久久久免费| 久热久热在线精品观看| 亚洲精品色激情综合| 欧美高清成人免费视频www| 欧美zozozo另类| 国产成人精品久久久久久| 青春草国产在线视频| 久久久久精品久久久久真实原创| 黄色欧美视频在线观看| 少妇裸体淫交视频免费看高清| 最近中文字幕2019免费版| 最近2019中文字幕mv第一页| 日韩精品有码人妻一区| 国产欧美日韩精品一区二区| 两个人视频免费观看高清| 天堂中文最新版在线下载 | 老师上课跳d突然被开到最大视频| 有码 亚洲区| 少妇熟女aⅴ在线视频| 免费观看的影片在线观看| 国产亚洲5aaaaa淫片| 久久精品国产鲁丝片午夜精品| 亚洲欧洲日产国产| 伦理电影大哥的女人| 国产淫片久久久久久久久| 日韩欧美精品v在线| 国产亚洲av片在线观看秒播厂 | 国产成人精品一,二区| 免费大片18禁| 国产有黄有色有爽视频| 久久99热6这里只有精品| 久久久久久久久大av| 国产精品人妻久久久久久| 美女内射精品一级片tv| 亚洲精品视频女| 欧美成人午夜免费资源| 色综合站精品国产| .国产精品久久| 少妇人妻精品综合一区二区| 亚洲av成人精品一二三区| 久久这里有精品视频免费| 一二三四中文在线观看免费高清| 边亲边吃奶的免费视频| 亚洲av电影不卡..在线观看| 麻豆国产97在线/欧美| 国产精品一区二区三区四区免费观看| 男人爽女人下面视频在线观看| 亚洲精品日韩av片在线观看| 国产精品麻豆人妻色哟哟久久 | 国产熟女欧美一区二区| 国产亚洲一区二区精品| 日韩欧美三级三区| 国产探花极品一区二区| 久久久久网色| 男女下面进入的视频免费午夜| 秋霞伦理黄片| 大片免费播放器 马上看| 亚洲精品自拍成人| 伊人久久国产一区二区| 97在线视频观看| 国产精品1区2区在线观看.| 少妇人妻精品综合一区二区| 久久久久久伊人网av| 免费看不卡的av| 一区二区三区乱码不卡18| 亚洲av中文av极速乱| 精品人妻一区二区三区麻豆| 偷拍熟女少妇极品色| 国产午夜福利久久久久久| 国产精品久久久久久久久免| 亚洲内射少妇av| h日本视频在线播放| 国产中年淑女户外野战色| 日韩制服骚丝袜av| 中国美白少妇内射xxxbb| 亚洲精品国产av成人精品| 欧美日韩在线观看h| 成人综合一区亚洲| 在线观看免费高清a一片| 日韩av在线免费看完整版不卡| 直男gayav资源| 国产精品精品国产色婷婷| 国产精品久久久久久久电影| 亚洲精品456在线播放app| 一边亲一边摸免费视频| 日韩国内少妇激情av| 亚洲欧美中文字幕日韩二区| 99久久精品热视频| 亚洲无线观看免费| 亚洲精品日本国产第一区| 日韩中字成人| 80岁老熟妇乱子伦牲交| 亚洲va在线va天堂va国产| 国产 一区精品| 成人一区二区视频在线观看| 亚洲高清免费不卡视频| 国产精品福利在线免费观看| 夜夜爽夜夜爽视频| 毛片一级片免费看久久久久| 日产精品乱码卡一卡2卡三| 国产成人a区在线观看| 亚洲aⅴ乱码一区二区在线播放| 男人舔奶头视频| 日本一本二区三区精品| 69av精品久久久久久| 亚洲精品视频女| 男女那种视频在线观看| 亚洲aⅴ乱码一区二区在线播放| 午夜日本视频在线| 免费黄频网站在线观看国产| 成人午夜高清在线视频| 国产黄色免费在线视频| 一级爰片在线观看| 久久97久久精品| freevideosex欧美| 免费少妇av软件| 六月丁香七月| 亚洲精品,欧美精品| 青春草视频在线免费观看| 好男人视频免费观看在线| 国产真实伦视频高清在线观看| 午夜免费观看性视频| 久久久久九九精品影院| 国产一区二区在线观看日韩| 欧美高清成人免费视频www| 午夜精品在线福利| 草草在线视频免费看| 久久久久免费精品人妻一区二区| 在线 av 中文字幕|