    Transverse relaxation characteristic and stress relaxation model considering molecular chains of HTPB coating based on pre-strained thermal aging

    2021-05-06 12:00:58YongqingDuJinZhengGuiboYuJinzhungZhi
    Defence Technology 2021年3期

    Yong-qing Du ,Jin Zheng ,**,Gui-bo Yu ,Jin-zhung Zhi

    a Shijiazhuang Campus,Army Engineering University,Shijiazhuang,050003,China

    b Intelligent Manufacturing Institute,Hebei College of Industry and Technology,Shijiazhuang,050003,China

    Keywords:HTPB Pre-strain aging Transverse relaxation characteristic Molecular chain Stress relaxation model

    ABSTRACT In order to accurately describe the transverse relaxation characteristic and stress relaxation modulus of HTPB coating during pre-strain thermal aging process,a one month thermal aging test was carried out at 70 °C with pre-strain of 0%,3%,6% and 9%,respectively.The low-field 1H NMR and stress relaxation modulus tests were carried out for HTPB coating at different aging stages.The stress relaxation model considering the molecular chains was proposed according to the changes of crosslinking chain and dangling chain of HTPB coating during pre-strain aging.The results showed that with the increase of aging time,the decay rate of transverse relaxation curve became faster,the transverse relaxation time decreased,the value of combined parameter qMrl increased,the proportion of crosslinking chain decreased,while the proportion of dangling chain increased.Moreover,the stress relaxation modulus increased,the crosslinking network structure of HTPB coating became denser and the degree of crosslinking increased.At the initial aging stage,the pre-strain will destroy the crosslinking network structure of HTPB coating to a certain extent.With the increase of aging time,the effect of pre-strain will gradually weaken and the influence of aging on materials will gradually increase.The correlations between the stress relaxation model considering the molecular chains and the test results were more than 0.9950,which can accurately describe the stress relaxation modulus of HTPB coating during the pre-strain thermal aging process.

    1.Introduction

    HTPB coating is an important part of solid rocket motor,which excellent mechanical performance is the key to ensure the combat effectiveness of solid rocket motor[1,2].The thermal oxidative aging is the most common factor affecting the properties of materials[3,4],during which process the microstructure of the material will generally undergo the interruption of macromolecular chains and crosslinking reaction[5].On the one hand,the proportion of dangling chain increases due to the chain scission of the polymer network in the presence of high temperature and oxygen;on the other hand,the extra crosslinking reaction caused by macromolecular free radicals or double bonds will take place in the internal material,finally forming a denser crosslinking network in the long aging time[6].The increase of crosslinking density in the aging process greatly weakens the deformation ability of the material and makes it more inclined to rigid body.At the same time,the chain scission reaction and random crosslinking reaction of polymer chains make the regularity of the crosslinking network worse,and the stress transfer ability gradually weakened,which further affecting the mechanical properties of the material[7].

    NMR technology has been widely used in the measurement of polymer microstructure and aging.This method has the advantages of non-destructive and fast,and can determine the different relaxation mechanisms and rates related to molecular motion in polymers.It is very sensitive to the changes of molecular chain structure and relaxation time of different types of polymer chain caused by crosslinking or chain scission during aging[8,9].Allen et al.[10]tested the aging properties of SBR under the conditions of heat and ultraviolet light,and revealed the molecular structure change and aging mechanism of SBR by means of NMR and IR.Daniel et al.[11]conducted the thermal oxygen aging test of HTPB at 80°C and found that the transverse relaxation time of HTPB can reflect the thermal oxygen aging change of materials sensitively.Jabez et al.[12]found that the change of molecular weight distribution of HTPB in the process of manufacturing and storage can be effectively characterized by transverse relaxation time.

    HTPB coating has typical viscoelastic mechanical characteristic.Under static or dynamic load,HTPB coating will appear creep,stress relaxation and other phenomena,which is related to the molecular chain structure of HTPB coating[13].Chi et al.[14]found that aging has a significant impact on the elastic part of the relaxation modulus of HTPB coating,but has a small impact on the viscous part,so they ignored the impact of the viscous part on the stress relaxation modulus of HTPB coating,and established a stress relaxation model with aging effect.Mojtaba et al.[15]studied the effect of hydrothermal aging on stress relaxation of materials,and predicted the long-term stress relaxation behavior using Kohlrausch-Williams-Watts(KWW)expression.Rui et al.[16]considered the effect of physical aging and obtained a scheme to simplify stress relaxation data.Liang et al.[17]proposed a new stress relaxation empirical model based on the relaxation function of the dual variable parameter Maxwell model.Zheng et al.[18]proposed a modified standard linear solid state(SLS)model to describe the compressive stress relaxation behavior of materials.This model not only made up for the deficiency of the empirical model,but also considered the change of the intrinsic viscosity of the material in the process of thermal oxygen aging.The above researches are mainly based on macro mechanics,without considering the change of molecular chain structure in the aging process.Marina et al.[19]verified the correctness of the proposed micro molecular chain motion mechanism through experiments,which showed that the viscoelastic behavior can be accurately described by considering the influence of different time scales of molecular chain motion on the relaxation process.Therefore,it is feasible and valuable to establish the stress relaxation model by considering the change of molecular chain.

    In this paper,a one month pre-strain thermally-accelerated aging test was carried out on HTPB coating.The transverse relaxation characteristic of HTPB coating during aging was tested and analyzed by low-field1H NMR.The stress relaxation modulus of HTPB coating at different aging stages was measured,and a stress relaxation model was proposed considering the change of molecular chains.

    2.Materials and methods

    2.1.Materials

    The HTPB coating used in the test is provided by the stateoperated No.845 factory in Xi’an,China,and the size and specific composition are referred to Ref.[20],which are shown as follows.

    According to the manufacturing process of the No.845 factory,the HTPB is used as adhesive,the TDI is used as the curing agent,the diisooctyl sebacate is used as the plasticizer,the zinc oxide is used as the reinforcing,active and vulcanizing agent,the silicon dioxide is used to improve the performance of ablation and corrosion resistance,and the molecular sieve is used as the catalytic agent and adsorbent(Fig.1).

    2.2.Aging test

    Fig.1.Sample of HTPB coating.

    The thermally-accelerated aging test of HTPB coating was conducted in the type DU288 oil bath thermostat.The test temperature was 70°C±1°C and the humidity in the thermostat was kept less than 50% by using silica desiccant.The samples of HTPB coating were stretched to the pre-strain of 0%,3%,6% and 9%,respectively for aging test.After aging for 3 d,6 d,12 d,20 d,and 30 d,the samples of HTPB coating were taken out and natural cooled to room temperature in a vacuum drying oven for 24 h.

    2.3.Transverse relaxation characteristic test

    The transverse relaxation characteristic of HTPB coating was measured by low-field1H NMR.The test temperature was 90°C.The HTPB coating samples were cut into rectangular strips of 10 mm×6 mm×2 mm and preheated at 90°C for 30 min before the transverse relaxation characteristic test.The transverse relaxation of the hydrogen protons of the HTPB coating tested by lowfield1H NMR is caused by the intramolecular and intermolecular hydrogen proton dipole interactions.At the NMR test temperature,the dipole interactions are considered to be the effect of the average of the thermal molecular motions.Since the hydrogen protons are used as probes for the NMR measurements,the transverse relaxation of the HTPB coating can be explained by the single chain model(XLD model)[21-23].

    2.4.Stress relaxation modulus test

    The stress relaxation modulus of HTPB coating was tested in Instron 5982.The test was conducted at room temperature of 25°C±2°C and using silica desiccant to keep the humidity of the test environment less than 50%.The stress relaxation modulus of HTPB coating samples aged at different stages were tested according to method 413.4 in GJB 770B-2005[24](see Fig.1).

    3.Results and discussion

    3.1.Effect of pre-strain aging on transverse relaxation characteristic

    3.1.1.Analysis of transverse relaxation curve

    The internal molecular chain scission and crosslinking reaction will occur at the same time during the whole aging process[25].In order to explore the changes of different types of molecular structure in HTPB coating during aging,the low-field1H NMR test was carried out[26,27],and the decay curves of transverse relaxation with relaxation time of HTPB coating were obtained as shown in Fig.2.

    Fig.2.The decay curves of transverse relaxation of HTPB coating.

    The decay of transverse relaxation is related to the low frequency motion of the polymer chain,which is very sensitive to the change of the crosslinking network structure during aging.The higher the crosslinking density,the shorter the transverse relaxation time,and the faster the decay of the transverse relaxation curve with the relaxation time[28,29].It can be seen from Fig.2 that with the increase of aging time and decrease of pre-strain,the decay rate of transverse relaxation curve of HTPB coating became faster,which demonstrated that the crosslinking density of HTPB coating increased gradually during pre-strain aging,and the crosslinking network of material was denser.

    The transverse relaxation decay curve of HTPB coating was fitted with the modified single chain model(XLD model)[21-23]:

    whereM(t)/M(0)is the change of transverse relaxation with time after normalization;M(0)is the initial and reference point;M(t)is the transverse relaxation value at relaxation timet;Ais the proportion of crosslinking chain signal in the total signal,%;(1-A)is the proportion of dangling chain signal in the total signal,%;T2is the transverse relaxation time,ms;qis the dipolar interaction,which is the ratio factor between the second moment higher than the glass transition temperature and the rigid second moment;Mrlis the dipole moment in the rigid lattice molecule,m/s2;qMrlis the average residual part of the second moment of the two pole interaction,m/s2;A0has no practical physical significance.The analysis of the fitting parameters was shown in the following section.

    3.1.2.The value of T2

    Daniel et al.[11]tested the1H NMR relaxation properties of HTPB polyurethane elastomers aged at 80°C,and found that the oxidative aging of HTPB polyurethane elastomers at high temperature resulted in additional crosslinking and densification of materials,resulting in loss of elasticity and deterioration of material properties.The transverse relaxation timeT2has a high sensitivity to thermal aging,and with the increase of thermal aging time,the transverse relaxation timeT2decreased approximately linearly.The aging properties of HTPB polyurethane elastomers can be effectively analyzed by using the transverse relaxation time as a parameter.Daniel’s study considered the thermal oxygen aging,but did not add the factor of pre-strain.Jabez et al.[12]found that the transverse relaxation timeT2obtained by1H NMR can sensitively capture the small changes in molecular weight and molecular weight distribution of HTPB prepolymer,and can be effectively applied to the manufacturing and storage process of HTPB prepolymer.Jabez’s study confirmed the sensitivity of the transverse relaxation time in capturing the microstructure changes of HTPB prepolymer,which provided a theoretical basis for this study.

    Fig.3.The variation of transverse relaxation time with pre-strain aging time.

    The transverse relaxation timeT2of HTPB coating with different pre-strain aging time is shown in Fig.3.It can be seen from Fig.3 that under different pre-strain conditions,the transverse relaxation time of HTPB coating decreased with the aging time.This was mainly because that the crosslinking network of the material became closer and the degree of crosslinking increased with the increase of aging time[30].At the same aging time,the pre-strain had a great influence on the material before aging for 12d.The transverse relaxation time of HTPB coating increased with the increase of pre-strain,which indicated that the pre-strain would destroy the crosslinking network of the material and reduce the crosslinking degree of the material[31].When the aging time was more than 12d,the influence of pre-strain on the material decreased gradually due to the stress relaxation phenomenon[13].The variation trend of the transverse relaxation time of HTPB coating with the increase of pre-strain was less monotonous than that when the aging time was less than 12d,which was mainly related to the joint action of oxidative crosslinking and degradative chain scission of HTPB coating aging[32,33].

    3.1.3.The value of qMrl

    The combined parameterqMrlis used to calculate the crosslinking density of HTPB coating.The higher theqMrlvalue,the higher the crosslinking density of the corresponding material[6].The variation ofqMrlwith pre-strain aging time is shown in Fig.4.

    Fig.4.The variation of qMrl with pre-strain aging time.

    The value ofqMrlof HTPB coating increased with aging time,which indicated that the crosslinking density of the material increased with aging time.At the same aging time,the value ofqMrlof HTPB coating decreased with the increase of pre-strain,which demonstrated that the existence of pre-strain will reduce the crosslinking density of the material.When the pre-strain was 3%,theqMrlof HTPB coating decreased slightly;while the pre-strains were 6% and 9%,theqMrlof HTPB coating decreased significantly,which indicated that the large strain had a serious destructive effect on the crosslinking structure,and then affected the mechanical properties of the material[34-36].

    3.1.4.Crosslinking chain and dangling chain

    The change curves of the proportion of crosslinking chain in HTPB coating with the pre-strain aging is shown in Fig.5.

    Under the aging condition of 0% pre-strain,the proportion of crosslinking chain of HTPB coating decreased with the increase of aging time,and the proportion of dangling chain increased gradually.The crosslinking density of HTPB coating was the result of the interaction between the crosslinking chain and the dangling chain[37].It can be seen from the test results that the role of the crosslinking chain was gradually weakened in the aging process,while the role of the dangling chain was gradually enhanced.By the time of aging for 30d,the proportion of the dangling chain has exceeded 50%.The change of the proportion of crosslinking chain and dangling chain was mainly due to the effect of degradative chain scission during the aging process[32,33].

    Under the condition of pre-strain aging,the changes of crosslinking chain and dangling chain of HTPB coating were different from that under the condition of 0% pre-strain aging.Under the condition of 3% pre-strain aging,the decrease of the proportion of crosslinking chain and the increase of the proportion of dangling chain were not obvious when the aging time was less than 12d.Compared with the aging condition of 0% pre-strain at the same aging time,the proportion of crosslinking chain of the HTPB coating under 3%pre-strain aging was slightly higher,and the proportion of dangling chain was slightly lower.This was mainly due to the rearrangement orientation of the molecular chain of HTPB coating under the condition of low strain stretching.At the same time,the crystallization in the material due to stretching played the role of physical crosslinking point and prevented the molecular chain from disentangling and inhibited the reduction of crosslinking chain[38-41].With the increase of aging time,the effect of pre-strain gradually weakened,and the interaction between oxidative crosslinking and degradative chain scission resulted in the decrease of the proportion of crosslinking chain and the increase of the proportion of dangling chain.

    Fig.5.Change curves of the proportion of crosslinking chain with pre-strain aging.

    Compared with the aging of 0% and 3% pre-strains,the proportion of the crosslinking chain decreased rapidly and the proportion of the dangling chain increased significantly in aging for 3d when the pre-strains were 6% and 9%,which were mainly due to the larger strain effect leading to the molecular chain disentanglement,crystal distortion and even damage[38,42].With the increase of aging time,the proportion of crosslinking chain and dangling chain of HTPB coating changed into platform area,the proportion of crosslinking chain decreased slowly,and the proportion of dangling chain increased slowly,which were mainly due to the pre-strain effect and the combined effect of oxidative crosslinking and degradative chain scission in the aging process.

    It can be seen from the above analysis that with the increase of aging time,the random occurrence of crosslinking reaction inside the material will obviously increase the heterogeneity of the material.The network crosslinking of HTPB coating resulted in the increase of crosslinking point and crosslinking density.Under the combined effects of pre-strain,oxidative crosslinking and degradative chain scission,the proportion of crosslinking chain of HTPB coating decreased gradually,while the proportion of dangling chain increased.

    3.2.Stress relaxation model considering molecular chains

    Chi et al.[14]tested the stress relaxation modulus of HTPB coating aged at 75°C for different time.It was found that the relaxation modulus of the coating increased after aging,but the effect of aging on the relaxation modulus of the coating was timedependent,and the change range of short-term relaxation modulus was very small.With the increase of stress relaxation loading time,the effect of aging on the relaxation modulus increased.At the same time,there was a good quantitative relationship between the elastic modulus and the gel fraction of the coating.Mojtaba et al.[15]studied the effect of thermal oxidative aging and hygrothermal aging on the relaxation behavior of polycarbonate blends.It was found that the thermal aging resulted in the increase of material modulus,while the moisture absorption had the opposite effect.With the increase of water content,the stiffness of the material decreased,and the modulus decreased with the relaxation of the material.Rui et al.[16]also concluded that thermal oxidative aging can increase the stress relaxation modulus of materials.Liang et al.[17]carried out a long-term stress relaxation test of glass fiber reinforced polymer composite and controlled the initial deflection of 10%,15% and 20%,respectively.It was found that the stress relaxation modulus of the material increased with the increase of the initial deflection.

    Based on the previous studies,the stress relaxation tests were carried out on HTPB coating at different pre-strain aging stages,and the stress relaxation curves are shown in Fig.6.

    With the increase of aging time and decrease of pre-strain,the stress relaxation modulus of HTPB coating increased gradually,which is same with the research of Layton[43].The results showed that with the increase of crosslinking degree,the crosslinking network became denser,and the stress relaxation modulus of HTPB coating increased gradually.At the same time,the increase of the viscous part of HTPB coating during the aging process,such as the dangling chain,will lead to the release of more stress during the relaxation process,which was also the reason for the increase of stress relaxation modulus of HTPB coating[6].

    During the aging process,the stress relaxation modulus of HTPB coating can be divided into elastic part and viscous part,namely:

    whereEis the stress relaxation modulus at different aging time,MPa;is the elastic part of the stress relaxation modulus,that is,elastic modulus,MPa;is the viscous part of the stress relaxation modulus,that is,viscous modulus,MPa.

    According to the statistical theory of polymer[44],the elastic modulus of the material is directly proportional to the crosslinking density:

    whereEε0is the elastic modulus without aging,MPa;kεis the aging reaction rate constant of elastic modulus;νais the crosslinking density at different aging time,10-4mol/cm3;ν0is the crosslinking density without aging,10-4mol/cm3.The test results of the crosslinking density of HTPB coating in this paper were shown in Ref.[20].

    The viscous part of stress relaxation modulus of HTPB coating was mainly attributed to physical entanglement and dangling chain.Assuming that the changes of physical entanglement and dangling chain in HTPB coating during aging were from the extra crosslinking and the chain scission of polymer chain,and the chain scission or crosslinking reaction conforms to the first-order reaction kinetics[45],the evolution of viscous modulus can be expressed as follows:

    Fig.6.Stress relaxation curves of HTPB coating under pre-strain aging.

    whereEc0is the contribution of crosslinking chain to the viscous modulus without aging,MPa;Ed0is the contribution of dangling chain to the viscous modulus without aging,MPa;τc0andτd0are relaxation time without aging,s;fc0is the proportion of crosslinking chain of HTPB coating without aging,%;fd0is the proportion of dangling chain of HTPB coating without aging,%;fcais the proportion of crosslinking chain of HTPB coating at different aging time,which is obtained from Fig.5 in Section 3.1.4,%;fdais the proportion of dangling chain of HTPB coating at different aging time,andfda=1-fca,%;kc,kd,kτc,kτdare aging reaction rate constant.

    For the stress relaxation test results of HTPB coating without aging and with pre-strain aging,the Levenberg-Marquardt method[46]was used for nonlinear fitting.The fitting curves are shown in Fig.6 and the parameter fitting results are shown in Table 1~Table 5.

    From Tables 2-5,it can be seen that under the condition of 0%pre-strain aging,the parameterkεincreased with the increase of aging time.In general,the parameterkcwas smaller than the parameterkdin the aging process,which indicated that the changing rate of elastic modulus increased gradually,and the increasing rate of the dangling chain was larger than that of the crosslinking chain.Under the condition of 3%,6%and 9%pre-strainaging,the parameterkεdecreased first and then increased with the increase of aging time.Generally,the parameterkcwas larger than the parameterkdfirst and then smaller than the parameterkd.This is mainly due to the influence of pre-strain at the initial aging stage.During the aging process,the influence of pre-strain was gradually weakened,and the role of oxidative crosslinking and degradation chain scission was gradually highlighted.

    Table 1Fitting results of HTPB coating without aging.

    Under 0%pre-strain aging,the parameterkτcdecreased with the increase of aging time,while the parameterkτdincreased gradually,indicating that the influence of the crosslinking chain on the relaxation property of the material decreased and that of the dangling chain increased gradually.Under the condition of 3%,6%and 9%pre-strain aging,the interaction among pre-strain,oxidative crosslinking and degradative chain scission competed with each other,which resulted in the change of parameterskτcandkτdwith aging time were not monotonous,but the parameterskτcwere larger than the parameterskτd,indicating that the influence of the dangling chain on the relaxation modulus during the pre-strain aging process occupied the leading role.

    It can be seen from the fitting curves and fitting results that the correlation coefficients between model fitting curves and test results were all greater than 0.9950,the average relative errors were all less than 3.5523%,which verified that the stress relaxation model considering the molecular chains proposed in this paper can accurately describe the test results of stress relaxation modulus of HTPB coating.

    Table 2Fitting results of stress relaxation model of 0% pre-strain aging.

    Table 3Fitting results of stress relaxation model of 3% pre-strain aging.

    Table 4Fitting results of stress relaxation model of 6% pre-strain aging.

    Table 5Fitting results of stress relaxation model of 9% pre-strain aging.

    4.Conclusions

    In this paper,the pre-strain thermal aging test of HTPB coating was carried out,the transverse relaxation characteristic of HTPB coating during pre-strain aging were analyzed,and a stress relaxation model considering the molecular chains was proposed.The specific conclusions are as follows:

    (1)With the increase of pre-strain aging time,the decay rate of transverse relaxation curves of HTPB coating became faster,the transverse relaxation timeT2was gradually reduced,the combined parameterqMrlrepresenting the crosslinking density increased with aging time while the proportion of crosslinking chain was gradually decreased.It is the contribution of the increment of physical crosslinking density;

    (2)Before aging for 12 d,with the increase of pre-strain,the transverse relaxation timeT2was increased,the proportion of crosslinking chain increased first and then decreased,while the proportion of dangling chain decreased first and then increased.When the aging time was more than 12 d,the variation trends of the transverse relaxation time,the proportion of crosslinking chain and the proportion of dangling chain were less monotonous than those when the aging time was less than 12 d.Meanwhile,the combined parameterqMrldecreased with the increase of pre-strain.The existence of pre-strain at the early stage of aging will destroy the crosslinking network structure of HTPB coating to some extent,and reduce the crosslinking degree of materials.With the increase of aging time,the influence of pre-strain on the performance of HTPB coating was gradually weakened due to the phenomenon of stress relaxation,and the influence of oxidative crosslinking and degradative chain scission in the aging process was gradually strengthened;

    (3)According to the change of crosslinking chain and dangling chain in the pre-strain aging process of HTPB coating,a stress relaxation model considering the molecular chains was proposed.The model can accurately describe the stress relaxation modulus of HTPB coating during pre-strain aging,and the correlation coefficients between model fitting curves and test results were all greater than 0.9950,the average relative errors were all less than 3.5523%.Declaration of competing interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgements

    This work was supported by the National Defense Pre-Research Projects[grant number ZS2015070132A12002].

    精品久久久噜噜| 国产一区二区在线观看日韩| 久久精品综合一区二区三区| 午夜激情欧美在线| 少妇的逼水好多| 又紧又爽又黄一区二区| 五月伊人婷婷丁香| 91久久精品国产一区二区成人| 97超级碰碰碰精品色视频在线观看| 亚洲人成网站高清观看| 成年女人看的毛片在线观看| 亚洲18禁久久av| 日韩高清综合在线| 国产精品久久久久久久久免| 欧美激情国产日韩精品一区| 国产av在哪里看| 欧美黑人欧美精品刺激| 在线免费十八禁| 国产高清三级在线| 不卡一级毛片| 久久久久久国产a免费观看| 日本欧美国产在线视频| 国产在线精品亚洲第一网站| 久久精品91蜜桃| 免费av毛片视频| 免费人成视频x8x8入口观看| 高清在线国产一区| 又紧又爽又黄一区二区| 天堂动漫精品| 午夜激情欧美在线| 人人妻人人看人人澡| 亚洲成人久久性| 日本精品一区二区三区蜜桃| 能在线免费观看的黄片| 欧美潮喷喷水| 午夜福利在线在线| 国产高清有码在线观看视频| 亚洲美女搞黄在线观看 | 人人妻人人看人人澡| 午夜福利高清视频| 国产精品爽爽va在线观看网站| 精品人妻熟女av久视频| 亚洲国产日韩欧美精品在线观看| 免费看a级黄色片| 乱人视频在线观看| 老司机午夜福利在线观看视频| 色5月婷婷丁香| av在线观看视频网站免费| 国产精品爽爽va在线观看网站| 热99re8久久精品国产| 啦啦啦韩国在线观看视频| 999久久久精品免费观看国产| 精品乱码久久久久久99久播| 午夜爱爱视频在线播放| 国产亚洲精品av在线| 男女啪啪激烈高潮av片| 亚洲av一区综合| 成年免费大片在线观看| 搞女人的毛片| 久久99热这里只有精品18| 一个人观看的视频www高清免费观看| 如何舔出高潮| 熟女电影av网| 国产av不卡久久| 免费观看的影片在线观看| 亚洲av成人精品一区久久| 亚洲中文字幕日韩| 成人特级av手机在线观看| 日日摸夜夜添夜夜添小说| 一进一出抽搐gif免费好疼| 久久人人爽人人爽人人片va| 亚洲欧美日韩高清专用| 国产v大片淫在线免费观看| 色av中文字幕| or卡值多少钱| 欧美一区二区亚洲| 一区二区三区四区激情视频 | 精品一区二区三区av网在线观看| 亚洲中文字幕一区二区三区有码在线看| 久久精品国产亚洲网站| 特级一级黄色大片| www.色视频.com| 欧美成人一区二区免费高清观看| 亚洲三级黄色毛片| 午夜福利18| 天美传媒精品一区二区| 国产v大片淫在线免费观看| 少妇高潮的动态图| 亚洲av免费在线观看| 亚洲最大成人手机在线| 亚洲三级黄色毛片| 亚洲专区中文字幕在线| 日本爱情动作片www.在线观看 | 国产精品一区二区三区四区免费观看 | 97碰自拍视频| 一级毛片久久久久久久久女| 欧美3d第一页| 女同久久另类99精品国产91| 亚洲国产欧美人成| 欧美极品一区二区三区四区| 麻豆久久精品国产亚洲av| 国产精品日韩av在线免费观看| 中文字幕精品亚洲无线码一区| 18+在线观看网站| 深夜a级毛片| 久久6这里有精品| 亚洲第一电影网av| 成年女人看的毛片在线观看| 国产精品女同一区二区软件 | 老司机午夜福利在线观看视频| 婷婷亚洲欧美| 亚洲av成人av| 国产单亲对白刺激| 国产熟女欧美一区二区| 亚州av有码| 在线免费十八禁| 91在线观看av| 丰满的人妻完整版| 亚洲人与动物交配视频| 看十八女毛片水多多多| 国产一区二区在线av高清观看| 韩国av在线不卡| 日本熟妇午夜| 亚洲国产欧洲综合997久久,| 极品教师在线视频| 99久久久亚洲精品蜜臀av| 淫秽高清视频在线观看| 国产久久久一区二区三区| 国产精品亚洲一级av第二区| 久久人人爽人人爽人人片va| 人妻久久中文字幕网| h日本视频在线播放| 亚洲一级一片aⅴ在线观看| 午夜精品在线福利| 国产色爽女视频免费观看| 黄色配什么色好看| 婷婷六月久久综合丁香| 国产精品精品国产色婷婷| 啦啦啦啦在线视频资源| 变态另类成人亚洲欧美熟女| 少妇的逼好多水| 很黄的视频免费| 亚洲欧美日韩东京热| 黄色女人牲交| 精品无人区乱码1区二区| 国产免费男女视频| 美女高潮喷水抽搐中文字幕| 干丝袜人妻中文字幕| 国产精品98久久久久久宅男小说| 长腿黑丝高跟| 女的被弄到高潮叫床怎么办 | 无人区码免费观看不卡| av天堂中文字幕网| 少妇的逼好多水| 国产精品伦人一区二区| 色哟哟哟哟哟哟| 亚洲狠狠婷婷综合久久图片| 免费黄网站久久成人精品| 国产极品精品免费视频能看的| 亚洲精品国产成人久久av| 国产v大片淫在线免费观看| 亚洲人成网站在线播放欧美日韩| 嫩草影院精品99| 亚洲男人的天堂狠狠| 午夜福利在线观看免费完整高清在 | 老熟妇仑乱视频hdxx| 在线观看美女被高潮喷水网站| 亚洲精品乱码久久久v下载方式| 精品一区二区三区视频在线观看免费| 黄色视频,在线免费观看| 中文字幕免费在线视频6| 全区人妻精品视频| 亚洲狠狠婷婷综合久久图片| 十八禁国产超污无遮挡网站| 成人三级黄色视频| 麻豆国产av国片精品| 亚洲性久久影院| 国产蜜桃级精品一区二区三区| 久久久国产成人免费| 欧美+日韩+精品| 久久久久久久久大av| 午夜激情福利司机影院| 麻豆成人av在线观看| a级毛片免费高清观看在线播放| 欧美成人免费av一区二区三区| 在线天堂最新版资源| 欧美一区二区国产精品久久精品| 日韩欧美国产在线观看| 日本与韩国留学比较| 一区二区三区免费毛片| 伦精品一区二区三区| 国产私拍福利视频在线观看| 又爽又黄无遮挡网站| 动漫黄色视频在线观看| av视频在线观看入口| 大又大粗又爽又黄少妇毛片口| 亚洲美女黄片视频| 高清毛片免费观看视频网站| 欧美高清成人免费视频www| 日韩精品有码人妻一区| 国产日本99.免费观看| 白带黄色成豆腐渣| 舔av片在线| 99久久成人亚洲精品观看| 亚洲av中文av极速乱 | 国产高潮美女av| 国产伦人伦偷精品视频| 日本一本二区三区精品| 国产主播在线观看一区二区| 干丝袜人妻中文字幕| 日本黄色视频三级网站网址| 欧美在线一区亚洲| 中文资源天堂在线| 99在线人妻在线中文字幕| 亚洲精品456在线播放app | 亚洲成a人片在线一区二区| 99视频精品全部免费 在线| 亚洲精品国产成人久久av| 直男gayav资源| 亚洲av中文av极速乱 | 99国产极品粉嫩在线观看| 日韩欧美精品免费久久| 老司机深夜福利视频在线观看| 国产精品无大码| 成年人黄色毛片网站| 亚洲最大成人中文| 丰满乱子伦码专区| 精品一区二区三区av网在线观看| 久久精品国产亚洲av香蕉五月| 狂野欧美白嫩少妇大欣赏| 波野结衣二区三区在线| 最近视频中文字幕2019在线8| 黄色丝袜av网址大全| 大型黄色视频在线免费观看| 免费观看的影片在线观看| 亚洲va日本ⅴa欧美va伊人久久| 久久精品影院6| 亚洲男人的天堂狠狠| 嫩草影视91久久| 欧美xxxx黑人xx丫x性爽| 欧美高清成人免费视频www| 美女黄网站色视频| 直男gayav资源| 2021天堂中文幕一二区在线观| 禁无遮挡网站| 国产精品国产高清国产av| 欧美日韩中文字幕国产精品一区二区三区| 日本一本二区三区精品| 国产免费av片在线观看野外av| xxxwww97欧美| 欧美+亚洲+日韩+国产| 男人的好看免费观看在线视频| 不卡视频在线观看欧美| 国产一区二区三区在线臀色熟女| 啦啦啦韩国在线观看视频| 99久久精品热视频| 精品久久久久久成人av| 亚洲欧美日韩无卡精品| 三级毛片av免费| 在线观看免费视频日本深夜| 91久久精品国产一区二区成人| 可以在线观看毛片的网站| 中文字幕av成人在线电影| 久久6这里有精品| 天堂网av新在线| 日韩欧美 国产精品| av视频在线观看入口| 18+在线观看网站| 亚洲自偷自拍三级| 亚洲天堂国产精品一区在线| 热99在线观看视频| 男人狂女人下面高潮的视频| 99国产极品粉嫩在线观看| 久久午夜亚洲精品久久| 久久精品91蜜桃| 少妇猛男粗大的猛烈进出视频 | av专区在线播放| 亚洲av.av天堂| 蜜桃亚洲精品一区二区三区| 村上凉子中文字幕在线| 国产人妻一区二区三区在| 熟女电影av网| 日韩高清综合在线| 一级黄色大片毛片| 啪啪无遮挡十八禁网站| 色综合色国产| av在线天堂中文字幕| 日日夜夜操网爽| 久久久成人免费电影| 桃色一区二区三区在线观看| 此物有八面人人有两片| 精品人妻熟女av久视频| 欧美一区二区精品小视频在线| 高清毛片免费观看视频网站| 国产老妇女一区| 日本a在线网址| 在线国产一区二区在线| 丰满乱子伦码专区| 麻豆一二三区av精品| 日韩欧美三级三区| 久久国产精品人妻蜜桃| 97超视频在线观看视频| 久久人妻av系列| 久久精品久久久久久噜噜老黄 | 亚州av有码| 色尼玛亚洲综合影院| 久久国产乱子免费精品| 久久久久国内视频| 日韩一区二区视频免费看| 麻豆一二三区av精品| 亚洲无线观看免费| 免费不卡的大黄色大毛片视频在线观看 | 一级黄色大片毛片| 美女黄网站色视频| 97热精品久久久久久| 欧美+日韩+精品| 天堂√8在线中文| 中文字幕免费在线视频6| 91午夜精品亚洲一区二区三区 | 亚洲中文字幕日韩| 欧美性感艳星| 亚洲三级黄色毛片| 少妇被粗大猛烈的视频| 99riav亚洲国产免费| 欧美人与善性xxx| 国产精品一区二区三区四区久久| 久久99热6这里只有精品| 三级男女做爰猛烈吃奶摸视频| 国产精品日韩av在线免费观看| 最新在线观看一区二区三区| 波野结衣二区三区在线| 99在线人妻在线中文字幕| 国产v大片淫在线免费观看| 亚洲人成网站在线播放欧美日韩| 琪琪午夜伦伦电影理论片6080| 久久精品国产99精品国产亚洲性色| 亚洲人成网站在线播放欧美日韩| 嫩草影院入口| 亚洲最大成人中文| 日韩av在线大香蕉| 白带黄色成豆腐渣| 欧美xxxx黑人xx丫x性爽| 白带黄色成豆腐渣| 中国美女看黄片| 又黄又爽又免费观看的视频| 啪啪无遮挡十八禁网站| 亚洲专区国产一区二区| 日韩高清综合在线| 午夜福利在线观看免费完整高清在 | eeuss影院久久| 久久久国产成人精品二区| 欧美日本亚洲视频在线播放| 又爽又黄无遮挡网站| 国产三级在线视频| 国产精品伦人一区二区| 男人舔女人下体高潮全视频| 九九爱精品视频在线观看| 黄片wwwwww| 久久草成人影院| 久久国产乱子免费精品| 成熟少妇高潮喷水视频| 国产伦精品一区二区三区视频9| 精品日产1卡2卡| 亚洲精品日韩av片在线观看| 精品99又大又爽又粗少妇毛片 | av在线老鸭窝| 天堂√8在线中文| 99热精品在线国产| 久久精品综合一区二区三区| 中国美白少妇内射xxxbb| 俄罗斯特黄特色一大片| 日韩,欧美,国产一区二区三区 | 一区二区三区激情视频| 好男人在线观看高清免费视频| 国产一区二区三区视频了| 久久6这里有精品| 国产精品一区二区三区四区免费观看 | 美女cb高潮喷水在线观看| 成人特级黄色片久久久久久久| 一本久久中文字幕| av.在线天堂| 99久久精品国产国产毛片| 亚洲国产高清在线一区二区三| 免费观看的影片在线观看| 欧美潮喷喷水| 噜噜噜噜噜久久久久久91| 午夜日韩欧美国产| 国产精品女同一区二区软件 | 午夜福利视频1000在线观看| 午夜福利在线观看免费完整高清在 | 88av欧美| 99久久精品一区二区三区| 九九热线精品视视频播放| 日韩在线高清观看一区二区三区 | 日日夜夜操网爽| 男女边吃奶边做爰视频| 日韩在线高清观看一区二区三区 | 真人做人爱边吃奶动态| 免费看美女性在线毛片视频| 国产精品不卡视频一区二区| 日本免费a在线| 久久久久国产精品人妻aⅴ院| 岛国在线免费视频观看| 女同久久另类99精品国产91| 久9热在线精品视频| 国产极品精品免费视频能看的| 欧美色视频一区免费| 12—13女人毛片做爰片一| 日韩 亚洲 欧美在线| 欧美+亚洲+日韩+国产| 国产日本99.免费观看| 国产一区二区三区av在线 | 亚洲一区高清亚洲精品| 国产不卡一卡二| 欧洲精品卡2卡3卡4卡5卡区| 亚洲av美国av| 午夜视频国产福利| 日本免费a在线| 99久久九九国产精品国产免费| videossex国产| 在线天堂最新版资源| 欧美色视频一区免费| 大型黄色视频在线免费观看| 亚洲精品456在线播放app | 日韩一区二区视频免费看| 噜噜噜噜噜久久久久久91| 熟妇人妻久久中文字幕3abv| 精品久久久久久久末码| 999久久久精品免费观看国产| 久99久视频精品免费| 亚洲精品一区av在线观看| 国产精品久久久久久久久免| 一进一出好大好爽视频| 可以在线观看毛片的网站| 我要看日韩黄色一级片| 伦理电影大哥的女人| www.www免费av| 日本黄大片高清| 国产成人av教育| 国产午夜精品久久久久久一区二区三区 | 午夜爱爱视频在线播放| 午夜福利18| 亚洲人成网站在线播| 国产私拍福利视频在线观看| a级一级毛片免费在线观看| 国内毛片毛片毛片毛片毛片| .国产精品久久| 国内精品宾馆在线| 99国产极品粉嫩在线观看| 99久国产av精品| 久久久久久伊人网av| 欧美一级a爱片免费观看看| 男女边吃奶边做爰视频| 不卡视频在线观看欧美| 久久久久九九精品影院| 亚洲精品亚洲一区二区| 欧美极品一区二区三区四区| 深夜精品福利| 国内精品久久久久精免费| 丰满人妻一区二区三区视频av| 美女被艹到高潮喷水动态| 欧美性感艳星| 国产高清不卡午夜福利| 国产精品美女特级片免费视频播放器| 97人妻精品一区二区三区麻豆| 国产av一区在线观看免费| 国产国拍精品亚洲av在线观看| a级一级毛片免费在线观看| 欧美日韩乱码在线| 九九在线视频观看精品| 午夜激情欧美在线| 男女下面进入的视频免费午夜| 高清在线国产一区| 久久久久久国产a免费观看| 久久精品国产亚洲av涩爱 | 亚洲七黄色美女视频| 九九在线视频观看精品| 少妇人妻精品综合一区二区 | 黄色日韩在线| 国产淫片久久久久久久久| 久久人人精品亚洲av| 中文字幕免费在线视频6| 亚洲精品色激情综合| 亚洲成av人片在线播放无| 免费搜索国产男女视频| 91久久精品电影网| 亚洲欧美精品综合久久99| 国产精品国产三级国产av玫瑰| 午夜免费男女啪啪视频观看 | 国产精品永久免费网站| 国产成人福利小说| 少妇熟女aⅴ在线视频| 最后的刺客免费高清国语| 男女啪啪激烈高潮av片| 亚洲男人的天堂狠狠| 免费高清视频大片| 免费看光身美女| 男插女下体视频免费在线播放| 日韩欧美国产一区二区入口| 日本三级黄在线观看| 有码 亚洲区| 成人高潮视频无遮挡免费网站| 久久久久国内视频| 久久久午夜欧美精品| 久久精品国产亚洲av天美| 精品久久国产蜜桃| 99久久九九国产精品国产免费| 真人一进一出gif抽搐免费| 国产av在哪里看| 99久久成人亚洲精品观看| 亚洲av日韩精品久久久久久密| 黄色一级大片看看| 国产真实乱freesex| www日本黄色视频网| 又黄又爽又刺激的免费视频.| 综合色av麻豆| 一个人看的www免费观看视频| 好男人在线观看高清免费视频| 国产一区二区三区av在线 | 欧美国产日韩亚洲一区| 色综合站精品国产| 国产乱人伦免费视频| 可以在线观看的亚洲视频| 在线观看一区二区三区| 日日摸夜夜添夜夜添小说| 亚洲欧美日韩卡通动漫| ponron亚洲| 99热这里只有精品一区| 琪琪午夜伦伦电影理论片6080| 99久久九九国产精品国产免费| 别揉我奶头~嗯~啊~动态视频| 欧美日韩精品成人综合77777| 黄色欧美视频在线观看| 国产高清有码在线观看视频| 12—13女人毛片做爰片一| 成熟少妇高潮喷水视频| 女生性感内裤真人,穿戴方法视频| 婷婷亚洲欧美| 18禁黄网站禁片午夜丰满| 成人国产麻豆网| 麻豆一二三区av精品| 欧美成人a在线观看| 亚洲精品亚洲一区二区| 级片在线观看| 超碰av人人做人人爽久久| 永久网站在线| 老司机福利观看| 色哟哟·www| 一个人看的www免费观看视频| 无人区码免费观看不卡| 久久久久久伊人网av| 久久久久免费精品人妻一区二区| 99久久精品国产国产毛片| 美女大奶头视频| 啦啦啦韩国在线观看视频| 免费搜索国产男女视频| 久久欧美精品欧美久久欧美| 国产aⅴ精品一区二区三区波| 欧美一区二区亚洲| 欧美日韩黄片免| 老司机福利观看| 久久久久久国产a免费观看| 免费av不卡在线播放| 韩国av在线不卡| 日韩欧美三级三区| 亚洲最大成人中文| 久99久视频精品免费| 九九久久精品国产亚洲av麻豆| netflix在线观看网站| 禁无遮挡网站| eeuss影院久久| 赤兔流量卡办理| 久久久久九九精品影院| 91av网一区二区| 国产成人a区在线观看| 天堂√8在线中文| 18+在线观看网站| 国产三级在线视频| 春色校园在线视频观看| 99视频精品全部免费 在线| 久久久色成人| 国产乱人视频| 欧美3d第一页| 国产私拍福利视频在线观看| 国产激情偷乱视频一区二区| 69av精品久久久久久| 成人特级黄色片久久久久久久| 免费在线观看成人毛片| 日韩人妻高清精品专区| 成年人黄色毛片网站| 91午夜精品亚洲一区二区三区 | 国产亚洲精品久久久久久毛片| 午夜爱爱视频在线播放| av天堂在线播放| 美女高潮的动态| 男女做爰动态图高潮gif福利片| 中文字幕人妻熟人妻熟丝袜美| 天堂动漫精品| 久久久久国产精品人妻aⅴ院| 午夜激情福利司机影院| 深夜精品福利| 老司机深夜福利视频在线观看| 能在线免费观看的黄片| 国产91精品成人一区二区三区| 内射极品少妇av片p| 国产美女午夜福利| 他把我摸到了高潮在线观看| 日韩国内少妇激情av| 午夜激情福利司机影院| 国产精品人妻久久久影院| h日本视频在线播放| 久久久国产成人精品二区| 国产一区二区亚洲精品在线观看| 亚洲中文字幕日韩| 精品99又大又爽又粗少妇毛片 |