    Reduction of the residual stresses in cold expanded thick-walled cylinders by plastic compression

    2016-12-27 01:08:16SKVORTSOVBOZNAKKIMYuARLYAPOVDMITRIEV
    Defence Technology 2016年6期

    V.F.SKVORTSOV,A.O.BOZNAK,A.B.KIM,A.Yu ARLYAPOV,A.I.DMITRIEV,b,*

    aDepartment of Automated Engineering Technology,Tomsk Polytechnic University,Lenin Av.30,Tomsk,Russia

    bInstitute of Strength Physics and Materials Science SB RAS,Akademicheski 2/4,Tomsk,Russia

    Reduction of the residual stresses in cold expanded thick-walled cylinders by plastic compression

    V.F.SKVORTSOVa,A.O.BOZNAKa,A.B.KIMa,A.Yu ARLYAPOVa,A.I.DMITRIEVa,b,*

    aDepartment of Automated Engineering Technology,Tomsk Polytechnic University,Lenin Av.30,Tomsk,Russia

    bInstitute of Strength Physics and Materials Science SB RAS,Akademicheski 2/4,Tomsk,Russia

    We suppose that in order to maintain high accuracy of holes and to lower residual stresses after cold expansion of thick-walled cylinders,which undergo cross-section plastic deformation,it is necessary to perform axial plastic compression and subsequent cold expansion with small interferences.To test this hypothesis,we studied hoop,radial and axial residual stresses in cylinders made of carbon steel AISI 1050 with hole diameter of 5 mm,outer diameter of 15 mm and length of 30 mm by Sachs method as well as accuracy of expanded holes.It is found that double cold expansion with total interference equal to 5.1%generates hoop residual stresses with largest absolute value equal to 284 MPa and ensures high holes accuracy(IT7).After plastic compression with strain equal to 0.5 and 1%the mentioned stresses reduced to 120 and 75 MPa respectively, and accuracy of the holes reduced as well.Subsequent cold expansion with small interference equal to 0.9%helps to restore holes accuracy(IT7) gained by double cold expansion and ensure that absolute value of hoop residual stresses(177 MPa)is lower compared to double cold expansion. ?2016 The Authors.Production and hosting by Elsevier B.V.on behalf of China Ordnance Society.This is an open access article under the CC BY-NC-ND license(http://creativecommons.org/licenses/by-nc-nd/4.0/).

    Thick-walled cylinders;Cold expansion;Plastic compression;Residual stresses

    1.Introduction

    Thick-walled cylinders(cylinders with an outer diameter D at least twice the size of the inner diameter d)constitute a large group of parts with precise small diameter holes(d≤10 mm). These parts include,for example,micro hydraulic and pneumatic cylinders,various bushings,guides,tubes,rolling bearing rings,etc.Improvement of surface finish[1,2]and accuracy of small diameter holes[3–5]is an actual task and requires the development of new methods of processing and cold expansion is one of the most effective methods of finishing and hardening of holes in such parts[4,5].Cold expansion is the process of pushing an oversized tapered pin or mandrel through the hole. Along with high productivity,cold expansion helps to increase accuracy up to IT6–IT8,improve surface roughness to Ra 0.1–0.3 μm,considerably work-harden surface layer and generate favorable compressive residual stresses[4–7].Besides precise hole processing[4,5],cold expansion is used to raise fatigue strength of parts with fastener holes[8–12].

    However,residual stresses generated during cold expansion of parts such as thick-walled cylinders can be undesirably high in some cases.If subsequent machining removes considerable allowances,workpiece undergoes substantial deformations and its accuracy decreases due to redistribution of residual stresses [7,13].Thisisalso possible dueto relaxation ofresidualstresses during product operation[14].In connection with the stated above it is of interest to investigate methods to reduce these stresses.

    Vishnyakov[15]points out that one of the effective ways to influence value and distribution of residual stresses can be plastic stretching or compression with small(from 1 to 2%) strains.Yang et al.[16]performed finite element method simulation of quench residual stress reduction through cold stretching process and demonstrated effectiveness of the given method to reduce residual stresses.Ko? et al.[13]showed that compression of Al 7050 blocks with strain from 1 to 4% reduced the residual stresses more than by 90%.Proskuryakov [4]suggested a method to reduce residual stresses in tubular samples after cold expansion.The method consists of pressingthe samples onto a special mandrel with interference from 0.1 to 5%and subsequent plastic upsetting to axial strain in the range from 0.3 to 3.5%.The author also notes that this method can lead to decrease in accuracy of the sample hole.

    Based on the review of studies[4,13,15,16],we can assume that one of the methods to manage residual stresses is axial plastic compression with low strains applied after cold expansion with high interferences and followed by cold expansion with small(approximately 1%of hole diameter)interference. It should be expected that residual stresses,generated after cold expansion with high interferences,have to drop during the compression[6,17].However,a certain decrease in accuracy of a hole caused by cold expansion is inevitable.Subsequent cold expansion with small interference,when semi-elastic deformation takes place(the external surface of the cylinder remains in elastic state i.e.deformation of the external surface is smaller than 0.2%),helps to restore the accuracy.Additionally,as shown in Refs.[4,7],it helps to generate significantly lower residual stresses compared to cold expansion with high interferences,when cross-sectional deformation takes place (deformation of the external surface exceeds 0.2%).

    The aim of this work is to experimentally investigate capabilities of plastic compression to reduce residual stresses in cold expanded thick-walled cylinders.

    2.Experimental procedure

    The experiments were aimed at determining residual stresses and carrying out accuracy analysis of holes subjected to double cold expansion,to double cold expansion followed by plastic compression with strain equal to 0.5 and 1%,and to cold expansion performed after plastic compression.

    2.1.Test specimens

    Experiments were carried out on samples made of carbon steelAISI 1050 with dimensions shown in Fig.1.Samples were machined on a lathe DMG Mori CTX 310 ecoline,holes were drilled and reamed.

    The total amount of samples was 25.They were divided into 5 lots.Samples from the first lot were cold expanded with high interferences.Samples from the second and the third lots were subjected to cold expansion with high interferences and plastic compression.Samples from the fourth and the fifth lots were subjected to cold expansion with high interferences, plastic compression and subsequent cold expansion with small interference.

    Fig.1.Dimensions of the samples(mm).

    Fig.2.Direct cold expansion.

    2.2.Cold expansion

    Direct cold expansion was used in this study(Fig.2).To achieve the double cold expansion,two tapered pins were forced through the hole in the same direction.The total interference for the two passes was 5.1%.It was defined by the following equation

    wheredprepresents the diameter of the cylindrical part of the pin and d represents the specimen hole diameter.Subsequent cold expansion was performed with small interference equal to 0.9%.

    The tapered pins used for cold expansion(Fig.3)were made of WC-8%Co(92%of tungsten carbide and 8%of cobalt)by Mion Company(Tomsk,Russia)with dimensions shown in Fig.4.Oil fluid MR-7 was used as a lubricant.Tests were performed on the universal testing machine IR5082-500.Cold expansion speed was equal to 0.008 m/s.Sample was held in the device shown in Fig.2.

    Fig.3.Tapered pins.

    Fig.4.Dimensions of the tapered pins(mm).

    2.3.Plastic compression

    Plastic compression with strain equal to 0.5 and 1%was performed on the universal testing machine IR5082-500.To ensure proper position of the samples during compression,their faces were preliminarily ground to remove any bulges left after cold expansion.Mixture of oil fluid MR-7 with molybdenum disulfide powder was applied to the faces of the samples to reduce friction.Sample was held in the device shown in Fig.5.

    2.4.Measurement of residual stresses

    Residual stresses were found by Sachs method[18–20].This method consists of independent successive removal of layers of metal from the inner or outer surface of the samples and measurement of resulted hoop and axial strains.We chose this method because it is a well-established technique to study distribution of residual stresses in cylindrical components that have rotational symmetry.This method has no limitations with regard to the depth of stress measurements and helps to measure the stresses throughout the entire thickness of the cylinder wall. Moreover,the method helps to define all three components of residual stress simultaneously.In addition,the given method is sufficiently accurate(nominal accuracy for steel is 45 MPa).

    Fig.5.Plastic compression.

    Fig.6.Measuring devices:(a)ultra-optimeter;(b)Mikrokator.

    According to this method,0.7 mm thick layers of metal were incrementally removed from the surface of the sample hole on a CNC wire-EDM machine model DK 7725;resulted changes in outer diameter and length were measured.External surface diameters were measured on the ultra-optimeter“Carl Zeiss Jena”(Fig.6(a))with an accuracy of readings equal to 0.0002 mm.The length of samples was measured using a Mikrokator 05IGP(Fig.6(b))with accuracy of readings equal to 0.0005 mm fixed in a stand.Outer diameter of the samples was measured in two longitudinal sections and in three crosssections(in the middle and at a distance of 2 mm from the sample faces,as shown in Fig.7(a)).Diameter of the sample external surface was taken as the average of the measured values.Length of the sample was measured as shown in Fig.7(b),and was considered equal to the average of the two extreme values of the measured lengths.

    External surface and faces of the samples were fine ground after plastic compression.This technique was used to ensure high accuracy of measurements of a sample length and diameter after boring.Since cold expansion leads to form distortion of the cylinder external surface and formation of bulges of metal displaced from the hole,it is impossible to perform accurate measurements without additional machining.Apparently,fine grinding affects residual stresses generated after cold expansion,but considering the fact that cold expansion creates residual stresses in the entire volume of material and grinding (depth of cut is smaller than 0.01 mm)affects stresses only in surface layer,influence of grinding on the residual stress distribution can be considered negligible.

    Fig.7.Scheme of measurement:(a)outer diameter of the sample;(b)height.

    Fig.8.Dependence of change of outer diameter 1 and length 2 of the cold expanded with high interference samples on the internal surface radius.Here and below,dotted lines show internal and external surfaces of the samples.

    Fig.8 shows an example of change of outer diameter ΔD and length ΔL of the samples during incremental boring,95 per cent confidence intervals are also given.These results are intermediate outcomes and are used to calculate hoop and axial strain after cutting.Similar dependences were obtained in each experiment and then were approximated with straight lines and second-degree polynomials,in which equations were then used to calculate residual stresses.

    Residual stresses were calculated using formulas proposed by I.A.Birger for the classic Sachs method[15]

    whereRis the radius of the sample external surface,mm;ris the radius of the internal surface of the sample(cutting radius), mm;is the hoop strain on outer radius as a result of cutting internal surface to the radius r;is the axial strain on outer radius as a result of cutting internal surface to the radiusr.

    Young’s modulusE=210 GPa and Poisson’s ratio ν=0.3 were used in calculations.

    Fig.9.Curves for hoop 1,radial 2 and axial 3 residual stresses in the samples double cold expanded with total interference equal to 5.1%.

    2.5.Assessment of hole accuracy

    Sample hole diameter was measured with a dial bore gauge“Carl Zeiss Jena”with accuracy of readings equal to 0.002 mm. Measurements were performed in two longitudinal sections and in three cross-sections(in the middle and at a distance of 2 mm from the sample faces).Accuracy of holes was evaluated by the scatter of diameters as a difference between maximum and minimum diameters in the lot.

    3.Results and discussion

    Distribution of hoop σθ,radial σrand axial σzresidual stresses along the radiusrof the samples(stress curves)double cold expanded with a total interference equal to 5.1%is shown in Fig.9.This interference causes plastic–elastic hoop residual strain on the outer surface equal to 0.0047.

    It can be seen that hoop and axial residual stresses are compressive in the zone adjacent to the hole and are balanced by corresponding tensile residual stresses in the external surface.Radial residual stresses on the hole surface and external surface are equal to zero,and are compressive in the rest of the part material.The largest in absolute value stresses are the hoop residual stresses,which are equal to-284 MPa near the hole surface.Dispersion of the sample hole diameters decreased from 0.042 mm to 0.009 mm(diameter after drilling followed by reaming was 5.018+0.042 mm,diameter after cold expansion was 5.254+0.009 mm).

    Plastic compression of the samples performed after double cold expansion with total interference equal to 5.1%leads to a sharp decrease in hoop and radial residual stresses absolute value(Fig.10).To a large degree,shape of the residual stresses curves remains unchanged.When the compression strain is 0.5%hoop residual stresses reduce in absolute value from -284 MPa(Fig.9)to-120 MPa(Fig.10(a)),and radial residual stresses from-85 MPa(Fig.9)to-21 MPa(Fig.10(a)). Increase in compression strain to 1%(Fig.10(b))leads to decrease in hoop residual stresses to-75 MPa,and decrease in radial residual stresses to-12 MPa.

    Fig.10.Curves for hoop 1,radial 2 and axial 3 residual stresses in the samples after cold expansion with interference equal to 5.1%and plastic compression with strain 0.5%(a)and 1%(b).

    The process of cold expansion generates deformations that are not uniform throughout the part and,as a result,leads to development of residual stresses.The reduction of residual stress level is achieved due to the fact that during plastic compression the uniaxial loading of a sample takes place,and after unloading elastic deformations will be uniform in magnitude and type.

    At the same time,plastic compression leads to a distinct increase in axial residual stresses.The maximum value of these stresses after double cold expansion with a total interference equal to 5.1%is-51 MPa(Fig.9),and after plastic compression with strains equal to 0.5 and 1%,increase to-99 MPa (Fig.10(a))and-73 MPa(Fig.10(b))respectively.This increase is probably due to non-uniform deformation of samples during compression caused by friction on the faces.

    The same reason leads to decrease in accuracy of the sample hole diameter during compression.When compression strain is 0.5 and 1%,dispersion of the sample hole diameter increases from 0.009 mm to 0.012 mm and 0.015 mm respectively(hole diameter after compression with 0.5%strain is 5.254+0.012mm, after compression with 1%strain is 5.251+0.015mm).

    Curves for residual stresses generated after subsequent cold expansion of plastically compressed samples with interference equal to 0.9%are shown in Fig.11.This interference causes elastic hoop residual strain on the sample outer surface,which is equal to 0.00034.It can be seen that residual stresses are almost independent of the degree of plastic deformation during compression.The largest in absolute value hoop residual stresses is equal to-178 MPa,and is 38%smaller than hoop residual stresses in samples after double cold expansion with total interference equal to 5.1%(Fig.9).Radial residual stresses increase to their initial values(-84 MPa),and axial residual stresses increase to-149 MPa.Dispersion of the sample hole diameters after subsequent cold expansion was 0.008 mm(hole diameter was 5.27+0.008mm).

    Fig.11.Curves for hoop 1,radial 2 and axial 3 residual stresses in the samples after double cold expansion with total interference equal to 5.1%,plastic compression with strain 0.5%(a)and 1%(b)and subsequent cold expansion with interference equal to 0.9%.

    Table 1 Summarized experimental data.

    The experimental data(Table 1)show that plastic compression helps to reduce residual stresses in the thick-walled cylinders cold expanded with high interferences.We can suggest that the most efficient method is to apply double cold expansion with high interferences along with axial compression with strain equal to 0.5%.This technique helps to reduce absolute value of hoop residual stresses by 58%,and decrease radial stresses by 75%.Dispersion of the sample hole diameters slightly increases(decrease of accuracy is smaller than one quality grade).

    Further increase of deformation leads to a more substantial decrease in residual stresses along with decrease in hole accuracy.Subsequent cold expansion with small interference restores accuracy gained by double cold expansion and ensures lower hoop residual stresses,but makes manufacturing process more complex(requires additional operation).

    4.Conclusions

    The main results can be formulated as following:

    1)Double cold expansion of holes in thick-walled cylinders made of carbon steel AISI 1050(hole diameter is 5 mm, outer diameter is 15 mm,length is 30 mm)with total interference equal to 5.1%helps to limit dispersion of the hole diameter within 0.009 mm(IT7).Along with it, residual stresses are generated in the bulk of the cylinders.The largest in absolute value stresses near the hole surface are the hoop residual stresses,which are equal to -284 MPa,radial residual stresses are-85 MPa,and axial residual stresses are-51 MPa.

    2)Plastic compression of the cylinders with 0.5%strain reduced absolute value of hoop residual stresses by 58% (to-120 MPa),and decreased radial stresses by 75%(to -21 MPa).Axial residual stresses increased to-99 MPa, and dispersion of hole diameters increased to 0.012 mm, what corresponds to IT7(decrease of accuracy is smaller than one quality grade).

    3)With increase in compression strain to 1%,hoop residual stresses decrease in absolute value by 74%(to-75 MPa), and radial stresses decrease by 86%(to-12 MPa).Axial residual stresses increase to-73 MPa,and dispersion of hole diameters increases to 0.015 mm,what corresponds to IT8(decrease of accuracy is one quality grade).

    4)After subsequent cold expansion of plastically com

    pressed samples with interference equal to 0.9%, hoop residual stresses are equal to-178 MPa,and are 38%smaller than hoop residual stresses in samples after double cold expansion with total interference equal to 5.1%.Axial residual stresses increase to-143 MPa,and radial residual stresses increase to their initial values. Dispersion of the sample hole diameters decreases to 0.008 mm,what corresponds to IT7(accuracy gained by double cold expansion is completely restored).

    5)Based on the experimental data we can suggest that double cold expansion performed with high interference along with axial plastic compression with a strain smaller than 0.5%is the most reasonable.This helps to significantly reduce hoop and radial residual stresses,while the accuracy decrease is smaller than one quality grade.

    We expect that this technique can be further developed by selection of a proper lubricant in order to reduce friction force on the faces of the cylinders during plastic compression.This may help to ensure more uniform deformation and as a result a smaller decrease in accuracy of holes.We plan to test the technique using finite element method and propose recommendations for optimum cold expansion parameters(interference, axial plastic strain during compression).It is also needed to assess feasibility of reducing residual stresses in cold expanded thick-walled cylinders by subsequent plastic stretching with small strains,and also combine cold expansion and plastic stretching into one process.This investigation is going to be carried out using not only real cold expansion process,but finite element method as well.

    Acknowledgments

    The authors gratefully acknowledge the guidance and role of the late Professor Vladimir Skvortsov during the conceptual stage of this study.The authors also wish to thank Lyudmila Petrova for invaluable metrological support.A.I.D.also thanks RFBR grant no.15-08-01511a.

    [1]Luo F,Cockburn A,Sparkes M,Lupoi R,Chen Z,O’Neill W,et al. Performance characterization of Ni60-WC coating on steel processed with supersonic laser deposition.Defence Technol 2015;11:35–47.

    [2]Wang T,Xie LJ,Wang XB,Shang TY.2D and 3D milled surface roughness of high volume fraction SiCp/Al composites.Defence Technol 2015;11:104–9.

    [3]Endo H,Murahashi T,Marui E.Accuracy estimation of drilled holes with small diameter and influence of drill parameter on the machining accuracy when drilling in mild steel sheet.Int J Mach Tools Manuf 2007;47:175–81.

    [4]Proskuryakov YG.Holes cold expansion.Moscow:Mashgiz;1961.

    [5]Skvortsov VF,Arlyapov AY,Okhotin IS,Kim AB.Mandrelling with high allowances as a method of finishing treatment of small diameter deep holes.Proceedings of 7th International Forum on Strategic Technology, IFOST 2012;7:1–5.

    [6]Skvortsov VF,Arlyapov AY,Boznak AO,Kim AB.Residual stresses in compression and tension mandrelling thick-walled cylinders.Proceedings of 2014 International Conference on Mechanical Engineering, Automation and Control Systems,MEACS 2014;1:1–4.

    [7]Skvortsov VF,Boznak AO,Kim AB,Arlyapov AY.Influence of thick-walled cylinders length on the residual stresses generated during the single-cycle mandrelling.IOP Conference Series:Materials Science and Engineering 2015;91:1–5.

    [8]Chakherlou TN,Alvandi-Tabrizi Y,Kiani A.On the fatigue behavior of cold expanded fastener holes subjected to bolt tightening.Int J Fatigue 2011;33:800–10.

    [9]De Matos PFP,McEvily AJ,Moreira PMGP,de Castro PMST.Analysis of the effect of cold-working of rivet holes on the fatigue life of an aluminum alloy.Int J Fatigue 2007;29:575–86.

    [10]Fu Y,Ge E,Su H,Xu J,Li R.Cold expansion technology of connection holes in aircraft structures:a review and prospect.Chinese J Aeronaut 2015;28:961–73.

    [11]Maximov JT,Duncheva GV,Amudjev IM.A novel method and tool which enhance the fatigue life of structural components with fastener holes.Eng Fail Anal 2013;31:132–43.

    [12]Nigrelli V,Pasta S.Finite-element simulation of residual stress induced by split-sleeve cold-expansion process of holes.J Mater Process Technol 2008;205:290–6.

    [13]Ko? M,Culp J,Altan T.Prediction of residual stresses in quenched aluminum blocks and their reduction through cold working processes. J Mater Process Technol 2006;174:342–54.

    [14]Zhuang WZ,Halford GR.Investigation of residual stress relaxation under cyclic load.Int J Fatigue 2001;23:31–7.

    [15]Vishnyakov YD,Piskarev VD.Control of residual stresses in metals and alloys.Moscow:Metallurgiya;1989.

    [16]Yang X,Zhu J,Nong Z,Lai Z,He D.FEM Simulation of quenching process in A357 aluminum alloy cylindrical bars and reduction of quench residual stress through cold stretching process.Comput Mater Sci 2013;69:396–413.

    [17]Birger IA.Residual stresses.Moscow:Mashgiz;1963.

    [18]Chen J,Terasaki T,Akiyama T,Kishitake K.New concept of equivalent inherent strain for measuring axisymmetric residual stresses.J Manuf Sci Eng 2000;122:304–9.

    [19]Garcia-Granada AA,Lacarac VD,Smith DJ,Pavier MJ.A new procedure based on Sachs’boring for measuring non-axisymmetric residual stresses: experimental application.Int J Mech Sci 2001;43:2753–68.

    [20]Sachs G.The determination of residual stresses in rods and tubes. Z Metallkunde 1927;19:352–7.

    Received 27 April 2016;revised 8 August 2016;accepted 12 August 2016 Available online 1 September 2016

    Peer review under responsibility of China Ordnance Society.

    *Corresponding author.Tel.:+73822286972.

    E-mail address:dmitr@ispms.ru(A.I.DMITRIEV).

    http://dx.doi.org/10.1016/j.dt.2016.08.002

    2214-9147/?2016 The Authors.Production and hosting by Elsevier B.V.on behalf of China Ordnance Society.This is an open access article under the CC BY-NC-ND license(http://creativecommons.org/licenses/by-nc-nd/4.0/).

    麻豆久久精品国产亚洲av| av国产久精品久网站免费入址| 最近中文字幕2019免费版| 天堂网av新在线| 一本久久精品| 1000部很黄的大片| 蜜桃亚洲精品一区二区三区| 日本免费a在线| 99在线人妻在线中文字幕| 欧美区成人在线视频| 国产伦精品一区二区三区四那| 成人性生交大片免费视频hd| 99九九线精品视频在线观看视频| 26uuu在线亚洲综合色| 午夜福利在线在线| 亚洲第一区二区三区不卡| 国产精品乱码一区二三区的特点| 国产午夜精品一二区理论片| 最近最新中文字幕大全电影3| 一级二级三级毛片免费看| 成人国产麻豆网| 中文天堂在线官网| 搞女人的毛片| 蜜桃久久精品国产亚洲av| 18禁动态无遮挡网站| 禁无遮挡网站| 听说在线观看完整版免费高清| 亚洲精品成人久久久久久| 少妇人妻一区二区三区视频| 午夜福利在线在线| 国产女主播在线喷水免费视频网站 | 亚洲欧美日韩东京热| 麻豆成人av视频| 日韩视频在线欧美| 建设人人有责人人尽责人人享有的 | 欧美成人免费av一区二区三区| 丝袜美腿在线中文| 麻豆国产97在线/欧美| www.色视频.com| 自拍偷自拍亚洲精品老妇| 91久久精品电影网| 午夜福利在线在线| ponron亚洲| 国产极品精品免费视频能看的| 久久久久久久久久黄片| 欧美高清性xxxxhd video| 一二三四中文在线观看免费高清| 亚洲av成人av| 日本与韩国留学比较| 亚洲电影在线观看av| 亚洲经典国产精华液单| 少妇熟女aⅴ在线视频| 联通29元200g的流量卡| 精品久久久久久久人妻蜜臀av| 观看免费一级毛片| av线在线观看网站| 午夜激情欧美在线| 亚洲最大成人手机在线| 国产精品久久久久久av不卡| 嫩草影院新地址| 国产成人精品婷婷| 97超视频在线观看视频| 精华霜和精华液先用哪个| 国产免费一级a男人的天堂| 老司机影院毛片| 赤兔流量卡办理| 亚洲天堂国产精品一区在线| 欧美成人免费av一区二区三区| 中文字幕制服av| 桃色一区二区三区在线观看| 国产美女午夜福利| 久久久久网色| 99久国产av精品国产电影| 两个人视频免费观看高清| 高清av免费在线| 变态另类丝袜制服| 亚洲av福利一区| 久久久成人免费电影| 欧美日韩精品成人综合77777| 久久这里只有精品中国| 美女国产视频在线观看| 国产三级在线视频| 日韩欧美 国产精品| 欧美激情国产日韩精品一区| 久久久久久久久中文| 尤物成人国产欧美一区二区三区| 热99re8久久精品国产| 简卡轻食公司| 三级国产精品片| 国产人妻一区二区三区在| 国产亚洲精品久久久com| 超碰97精品在线观看| 丰满少妇做爰视频| 中国国产av一级| 亚洲18禁久久av| 七月丁香在线播放| 亚洲精品aⅴ在线观看| 你懂的网址亚洲精品在线观看 | 国产私拍福利视频在线观看| 亚洲国产精品sss在线观看| 黄片无遮挡物在线观看| 国产一区二区三区av在线| ponron亚洲| 在线观看av片永久免费下载| 精品人妻偷拍中文字幕| 日韩精品青青久久久久久| 日韩av不卡免费在线播放| 亚洲精品亚洲一区二区| 汤姆久久久久久久影院中文字幕 | 内地一区二区视频在线| 亚洲国产精品久久男人天堂| 如何舔出高潮| 国产成人aa在线观看| 欧美色视频一区免费| 丰满少妇做爰视频| 色播亚洲综合网| 69人妻影院| 三级经典国产精品| 国产91av在线免费观看| 国产v大片淫在线免费观看| 一级av片app| 中文字幕制服av| 欧美成人午夜免费资源| 国产 一区 欧美 日韩| 看黄色毛片网站| 中文资源天堂在线| 免费看光身美女| 国产精品.久久久| 人人妻人人澡人人爽人人夜夜 | 亚洲av一区综合| 69人妻影院| 美女cb高潮喷水在线观看| 能在线免费观看的黄片| 久久精品夜色国产| 亚洲一区高清亚洲精品| 一卡2卡三卡四卡精品乱码亚洲| 99久久成人亚洲精品观看| 国产精品永久免费网站| 国产91av在线免费观看| av线在线观看网站| 欧美97在线视频| 久久久久免费精品人妻一区二区| 久久久久久久久久成人| 国产白丝娇喘喷水9色精品| 插逼视频在线观看| av福利片在线观看| 在线a可以看的网站| 国产午夜精品论理片| 91精品一卡2卡3卡4卡| 日韩一区二区视频免费看| 亚洲av中文字字幕乱码综合| 特级一级黄色大片| av天堂中文字幕网| 亚洲欧美精品自产自拍| 亚洲欧洲国产日韩| 一个人免费在线观看电影| 91精品伊人久久大香线蕉| 午夜福利视频1000在线观看| 麻豆av噜噜一区二区三区| 人妻少妇偷人精品九色| 春色校园在线视频观看| 国产在视频线精品| 日韩亚洲欧美综合| 精品欧美国产一区二区三| 热99re8久久精品国产| 国产av一区在线观看免费| 国产淫语在线视频| 麻豆成人av视频| 夫妻性生交免费视频一级片| 三级国产精品欧美在线观看| 久久热精品热| 亚洲成人精品中文字幕电影| www.色视频.com| 国产精品,欧美在线| 听说在线观看完整版免费高清| 国产精品女同一区二区软件| 69人妻影院| 午夜福利视频1000在线观看| 国产成人aa在线观看| 麻豆精品久久久久久蜜桃| 日本三级黄在线观看| 大又大粗又爽又黄少妇毛片口| www.av在线官网国产| av在线蜜桃| 亚洲成人精品中文字幕电影| 亚洲欧洲国产日韩| 国产一区二区亚洲精品在线观看| 日日干狠狠操夜夜爽| 色噜噜av男人的天堂激情| av国产免费在线观看| 亚洲国产精品专区欧美| 国产av不卡久久| 亚洲欧美日韩卡通动漫| 成人av在线播放网站| 免费在线观看成人毛片| 国产精品久久电影中文字幕| 免费人成在线观看视频色| 少妇熟女aⅴ在线视频| 亚洲欧美精品自产自拍| 久久这里只有精品中国| 一个人观看的视频www高清免费观看| 精品人妻熟女av久视频| videos熟女内射| 亚洲在久久综合| 国产av码专区亚洲av| 中文字幕av成人在线电影| 亚洲精品成人久久久久久| 免费av毛片视频| 乱人视频在线观看| 日韩av在线大香蕉| 国产真实乱freesex| 国产av一区在线观看免费| 国产伦在线观看视频一区| 久久精品人妻少妇| www.色视频.com| 99在线人妻在线中文字幕| 日日摸夜夜添夜夜爱| 能在线免费观看的黄片| 成人美女网站在线观看视频| 人人妻人人看人人澡| 免费无遮挡裸体视频| 国产老妇女一区| 亚洲精品自拍成人| 日韩精品有码人妻一区| 国产高清国产精品国产三级 | 在现免费观看毛片| 真实男女啪啪啪动态图| 人妻夜夜爽99麻豆av| 国产成人91sexporn| 中文字幕熟女人妻在线| 亚洲国产精品成人久久小说| 九九爱精品视频在线观看| 啦啦啦韩国在线观看视频| 国产白丝娇喘喷水9色精品| 国产三级在线视频| 五月玫瑰六月丁香| 免费观看人在逋| 免费黄色在线免费观看| 国产综合懂色| 免费av观看视频| 人体艺术视频欧美日本| 久久99热这里只有精品18| 欧美性猛交╳xxx乱大交人| 国产精品久久久久久av不卡| 午夜老司机福利剧场| 国模一区二区三区四区视频| 久久人人爽人人片av| 久久人人爽人人片av| 欧美成人精品欧美一级黄| 天堂av国产一区二区熟女人妻| 国产探花极品一区二区| 人妻夜夜爽99麻豆av| 美女国产视频在线观看| 嫩草影院新地址| 日韩一区二区三区影片| 欧美97在线视频| 网址你懂的国产日韩在线| 中文字幕av成人在线电影| 我的女老师完整版在线观看| 一个人观看的视频www高清免费观看| 日韩一区二区三区影片| 午夜视频国产福利| 日本免费在线观看一区| 国产精品福利在线免费观看| 免费不卡的大黄色大毛片视频在线观看 | 成人综合一区亚洲| 色综合色国产| 亚洲av中文av极速乱| 久久精品夜夜夜夜夜久久蜜豆| 亚洲内射少妇av| 最近手机中文字幕大全| 亚洲图色成人| 大香蕉久久网| 欧美日韩精品成人综合77777| 男女国产视频网站| 国产亚洲精品久久久com| 级片在线观看| 亚洲成色77777| 久久亚洲精品不卡| 亚洲av一区综合| 久久久久性生活片| 看片在线看免费视频| 中文亚洲av片在线观看爽| 亚洲av.av天堂| 69人妻影院| 国产精品一二三区在线看| 欧美丝袜亚洲另类| 免费观看精品视频网站| 99久久九九国产精品国产免费| 日本与韩国留学比较| 中文精品一卡2卡3卡4更新| 日韩高清综合在线| 色尼玛亚洲综合影院| 一级黄色大片毛片| 欧美日韩精品成人综合77777| 日本av手机在线免费观看| 久99久视频精品免费| 国产色婷婷99| 亚洲欧美精品自产自拍| 美女黄网站色视频| 99久久无色码亚洲精品果冻| 亚洲人成网站在线播| 久久精品国产亚洲av涩爱| 亚洲av日韩在线播放| 精品人妻视频免费看| 国产一区二区亚洲精品在线观看| 男插女下体视频免费在线播放| 一级av片app| 亚洲无线观看免费| 日本色播在线视频| 日日摸夜夜添夜夜爱| 一级爰片在线观看| 日韩av在线免费看完整版不卡| 国产视频首页在线观看| 国产精品蜜桃在线观看| 国产黄片美女视频| 亚洲精品色激情综合| 久99久视频精品免费| 麻豆成人av视频| 菩萨蛮人人尽说江南好唐韦庄 | 极品教师在线视频| 九九在线视频观看精品| 亚洲欧洲日产国产| 国产单亲对白刺激| 亚洲成人av在线免费| 综合色av麻豆| 国产综合懂色| 村上凉子中文字幕在线| 亚洲欧美清纯卡通| 精品久久久久久久人妻蜜臀av| 婷婷六月久久综合丁香| 久久人人爽人人片av| 最近中文字幕2019免费版| 变态另类丝袜制服| 日本黄色片子视频| 国语自产精品视频在线第100页| 亚洲av免费在线观看| 在现免费观看毛片| 国产又色又爽无遮挡免| 91午夜精品亚洲一区二区三区| 18禁在线播放成人免费| 免费看av在线观看网站| 内射极品少妇av片p| 国产精品无大码| 一夜夜www| 国产亚洲av片在线观看秒播厂 | 超碰97精品在线观看| 99久国产av精品| 国产成人精品久久久久久| 一夜夜www| 亚洲av中文字字幕乱码综合| 国产精品国产三级国产av玫瑰| 国产亚洲一区二区精品| 在线a可以看的网站| 青春草亚洲视频在线观看| 午夜久久久久精精品| 日本午夜av视频| 人妻少妇偷人精品九色| 黄色配什么色好看| 国产av不卡久久| 久久国产乱子免费精品| 18禁在线播放成人免费| 男人狂女人下面高潮的视频| 午夜免费男女啪啪视频观看| 欧美日韩精品成人综合77777| 日本免费a在线| 亚洲av电影不卡..在线观看| 国产精品一区二区在线观看99 | 十八禁国产超污无遮挡网站| 插逼视频在线观看| 综合色av麻豆| 欧美成人免费av一区二区三区| 亚洲中文字幕日韩| 丰满乱子伦码专区| 亚洲人成网站在线播| 成年女人看的毛片在线观看| 国产黄a三级三级三级人| 麻豆精品久久久久久蜜桃| 女人久久www免费人成看片 | 桃色一区二区三区在线观看| 国产精品国产高清国产av| 亚洲精品日韩av片在线观看| 免费搜索国产男女视频| a级一级毛片免费在线观看| 亚洲成人中文字幕在线播放| 亚洲精品影视一区二区三区av| 蜜桃久久精品国产亚洲av| 亚洲国产高清在线一区二区三| 亚洲国产欧美在线一区| 国产人妻一区二区三区在| 国产伦理片在线播放av一区| 精品人妻视频免费看| 日本欧美国产在线视频| 麻豆一二三区av精品| 国产午夜精品久久久久久一区二区三区| 乱人视频在线观看| 在线播放国产精品三级| 国产极品精品免费视频能看的| 一级毛片电影观看 | 成人综合一区亚洲| 亚洲精品,欧美精品| 欧美成人一区二区免费高清观看| 国产 一区 欧美 日韩| 国产精品综合久久久久久久免费| 国产精品精品国产色婷婷| 国产久久久一区二区三区| 91午夜精品亚洲一区二区三区| 久久99热这里只频精品6学生 | 看免费成人av毛片| 亚洲自偷自拍三级| 一级黄片播放器| 在线a可以看的网站| 最近中文字幕高清免费大全6| 精品国内亚洲2022精品成人| 婷婷色综合大香蕉| 最近手机中文字幕大全| 久久这里有精品视频免费| 亚洲乱码一区二区免费版| 搡老妇女老女人老熟妇| 一级爰片在线观看| 欧美日本亚洲视频在线播放| 91精品伊人久久大香线蕉| 国产一区有黄有色的免费视频 | 国产激情偷乱视频一区二区| 久久精品久久久久久噜噜老黄 | 国产精品一区二区三区四区免费观看| av又黄又爽大尺度在线免费看 | 青春草视频在线免费观看| 国产av在哪里看| 亚洲国产精品成人综合色| 黄色欧美视频在线观看| 国产精品福利在线免费观看| 一边摸一边抽搐一进一小说| 国产激情偷乱视频一区二区| av免费观看日本| 亚洲综合精品二区| 午夜免费男女啪啪视频观看| 白带黄色成豆腐渣| 国产伦精品一区二区三区视频9| 午夜爱爱视频在线播放| 白带黄色成豆腐渣| 一级毛片电影观看 | 在线a可以看的网站| 有码 亚洲区| 尤物成人国产欧美一区二区三区| 免费看a级黄色片| 2021少妇久久久久久久久久久| 免费看光身美女| 欧美一区二区国产精品久久精品| 亚洲不卡免费看| 久久久午夜欧美精品| 最近中文字幕高清免费大全6| 日本一本二区三区精品| av免费观看日本| 久久久久性生活片| 国产黄片美女视频| 我要看日韩黄色一级片| 夜夜爽夜夜爽视频| 久久久久久久久大av| 特大巨黑吊av在线直播| 三级国产精品欧美在线观看| av国产久精品久网站免费入址| 国产探花极品一区二区| 国产精品三级大全| 久久精品国产鲁丝片午夜精品| 日产精品乱码卡一卡2卡三| 成人性生交大片免费视频hd| 天堂中文最新版在线下载 | 精品久久久噜噜| 国产精品久久久久久精品电影| 成人二区视频| 91午夜精品亚洲一区二区三区| 毛片女人毛片| 亚洲av二区三区四区| 丝袜美腿在线中文| 99在线视频只有这里精品首页| 2021少妇久久久久久久久久久| 国产黄片美女视频| 免费搜索国产男女视频| 欧美不卡视频在线免费观看| 久久99热这里只频精品6学生 | 国产熟女欧美一区二区| 日韩欧美精品免费久久| 小说图片视频综合网站| 97热精品久久久久久| 免费av不卡在线播放| 精品久久久久久久末码| 夫妻性生交免费视频一级片| 天天躁日日操中文字幕| 波野结衣二区三区在线| 亚洲高清免费不卡视频| 人人妻人人澡人人爽人人夜夜 | 国产精品精品国产色婷婷| 欧美高清成人免费视频www| 噜噜噜噜噜久久久久久91| 国产精品人妻久久久久久| 激情 狠狠 欧美| 91狼人影院| 国产黄片视频在线免费观看| av专区在线播放| 国产精品乱码一区二三区的特点| 久久久久久国产a免费观看| 可以在线观看毛片的网站| 亚洲av.av天堂| 亚洲国产精品国产精品| 99久久精品热视频| 美女高潮的动态| 午夜福利高清视频| 亚洲四区av| 永久免费av网站大全| 亚洲成人久久爱视频| 亚洲真实伦在线观看| 51国产日韩欧美| 天天躁夜夜躁狠狠久久av| 精品人妻熟女av久视频| 两个人的视频大全免费| 久久久久网色| 欧美一区二区精品小视频在线| 国产成人aa在线观看| 日韩av在线免费看完整版不卡| 桃色一区二区三区在线观看| av免费观看日本| 久久久久久久国产电影| 欧美日韩在线观看h| 久99久视频精品免费| 三级国产精品欧美在线观看| 亚洲精品影视一区二区三区av| 亚洲av二区三区四区| 日本一二三区视频观看| 身体一侧抽搐| 好男人在线观看高清免费视频| 国产午夜福利久久久久久| 午夜精品在线福利| 寂寞人妻少妇视频99o| 亚洲人与动物交配视频| 久久99精品国语久久久| 国产精品一二三区在线看| 我的老师免费观看完整版| 最近手机中文字幕大全| 熟女电影av网| 久久午夜福利片| 一级黄色大片毛片| av国产久精品久网站免费入址| 国产老妇女一区| 最后的刺客免费高清国语| av福利片在线观看| 精品国产一区二区三区久久久樱花 | 91精品国产九色| 久久99精品国语久久久| 简卡轻食公司| 大话2 男鬼变身卡| 在现免费观看毛片| 成人毛片60女人毛片免费| 欧美色视频一区免费| 日韩一本色道免费dvd| 国产精品国产三级国产专区5o | av女优亚洲男人天堂| 国产女主播在线喷水免费视频网站 | 免费看a级黄色片| 色视频www国产| 自拍偷自拍亚洲精品老妇| 人妻系列 视频| 人妻夜夜爽99麻豆av| 午夜福利在线观看吧| 国产精品乱码一区二三区的特点| 99在线人妻在线中文字幕| 夜夜爽夜夜爽视频| 中文精品一卡2卡3卡4更新| 秋霞伦理黄片| 国产亚洲最大av| 国产成人午夜福利电影在线观看| 久久精品影院6| 国产淫语在线视频| 久久人人爽人人爽人人片va| 成人一区二区视频在线观看| 亚洲av福利一区| 午夜精品一区二区三区免费看| 一本—道久久a久久精品蜜桃钙片 精品乱码久久久久久99久播 | 精品久久久久久久人妻蜜臀av| 久久人人爽人人爽人人片va| 亚洲无线观看免费| АⅤ资源中文在线天堂| 成人欧美大片| 久久久精品欧美日韩精品| 亚洲精华国产精华液的使用体验| 中国国产av一级| 国产探花极品一区二区| 欧美激情在线99| 三级男女做爰猛烈吃奶摸视频| 欧美成人一区二区免费高清观看| 国产精品久久久久久久电影| 简卡轻食公司| 午夜日本视频在线| 一级av片app| 亚洲伊人久久精品综合 | 人人妻人人看人人澡| 综合色丁香网| 国产精品一区二区三区四区免费观看| 91久久精品国产一区二区成人| av福利片在线观看| 99久久精品国产国产毛片| 亚洲精品aⅴ在线观看| 亚洲人与动物交配视频| 汤姆久久久久久久影院中文字幕 | 中国国产av一级| 成人高潮视频无遮挡免费网站| 亚洲av熟女| 夜夜看夜夜爽夜夜摸| 国产成人aa在线观看| 亚洲成人中文字幕在线播放| 男女那种视频在线观看| 成人特级av手机在线观看| 搞女人的毛片| 美女内射精品一级片tv| 国产av码专区亚洲av|