    Preparation and characterization of pH-responsive metal-polyphenol structure coated nanoparticles

    2024-01-24 01:10:48QileXiYnLingAilingCoYnCoLuyunCi

    Qile Xi, Yn Ling, Ailing Co, Yn Co, Luyun Ci

    a Key Laboratory of Post-Harvest Handling of Fruits, Food Science Institute, Zhejiang Academy of Agricultural Sciences, Hangzhou 310021, China

    b Ningbo Research Institute, College of Biosystems Engineering and Food Science, Zhejiang University, Ningbo 315100, China

    c School of Biological and Chemical Engineering, Zhejiang Engineering Research Center for Intelligent Marine Ranch Equipment, NingboTech University, Ningbo 315100, China

    d College of Food Science and Engineering, Bohai University, Jinzhou 121013, China

    e Hangzhou Customs District, Hangzhou 310007, China

    Keywords: Metal Phlorotannins Nanoparticles pH-Responsive Characterization

    ABSTRACT In this paper, tannic acid (TA) and Fe3+ were added to form a layer of metal-polyphenol network structure on the surface of the nanoparticles which were fabricated by zein and carbon quantum dots (CQDs) encapsulating phlorotannins (PTN). pH-Responsive nanoparticles were prepared successfully (zein-PTN-CQDs-FeIII).Further, the formation of composite nanoparticles was conf irmed by a series of characterization methods. The zeta-potential and Fourier transform infrared spectroscopy data proved that electrostatic interaction and hydrogen bonding are dominant forces to form nanoparticles. The encapsulation efficiency (EE) revealed that metal-polyphenol network structure could improve the EE of PTN. Thermogravimetric analysis and differential scanning calorimetry experiment indicated the thermal stability of zein-PTN-CQDs-FeIII nanoparticles increased because of metal-polyphenol network structure. The pH-responsive nanoparticles greatly increased the release rate of active substances and achieved targeted release.

    1. Introduction

    Zein was the main protein in corn, accounting for about 50% of the total protein content currently[1]. Zein had been used to prepare various delivery systems due to its high encapsulation capacity and good biodegradability[2]. There were many methods to prepare zein nanoparticles, including anti-solvent precipitation, composite condensation and spray drying. Among them, the anti-solvent precipitation method was the most commonly used method, which was also used in this paper to prepare nanoparticles. Anti-solvent precipitation (ASP) also known as liquid-liquid dispersion or phase separation. Deionized water droplets were put into zein ethanol aqueous solution (70%–80%), and water accounted for an increasing proportion in this process. The solubility of zein decreased since zein was only dissolved in the binary system of water and ethanol.Combined with the molecular self-assembly characteristics, molecules clustered and formed particles[3].

    Phlorotannins (PTN), a kind of unique polyphenols in the ocean,were the main polyphenols existing in brown algae and secondary metabolites of algae. They were composed of phloroglactil monomers with different antioxidant activities and were linked together through the acetomalonic acid pathway. Their molecular weight ranged from 126 Da to 650 kDa[4]. According to the number of hydroxyl groups and the properties of structural connections between phlorogluogl units, PTN could be divided into 6 subclasses: eckols, fuhalols,fucophlorethols, phlorethols, fucols and ishofuhalols[5]. Polyphenols from brown algae had potential biological activities, regulating metabolic disorders, and could be anti-tumor, anti-diabetes, anti-virus,anti-allergy, anti-bacterial, anti-oxidation and anti-inflammatory[6].The anti-inflammatory mechanism of PTN mainly included inhibition of nitric oxide, tumor necrosis factor and interleukin 6 production and expression of nitric oxide synthase and cyclooxygenase 2[7]. PTN also inhibited the activity of inflammatory genes and reduced the mRNA expression of acute and chronic inflammatory markers and Toll-like receptors (TLR4 and TLR9) in 3T3-L1 adipocytes.

    Tannic acid (TA) was a kind of weakly acidic polyphenol compound, containing diethylene glycol group, which was connected to the central core of glucose through ester bond, and was an important member of the natural polyphenol family. Tannin was usually divided into 2 groups: hydrolyzable and non-hydrolyzable with different chemical structures. Tannic acid had abundant aromatic rings and hydroxyl groups in chemical structure, which could be modified in many ways. The modification of tannic acid could be divided into 3 main pathways: 1) heterocyclic opening accelerated the rearrangement of chemical structure; 2) -OH groups on the aromatic ring enhanced the reactivity of nucleophilic sites, resulting in electrophilic aromatic substitution; 3) -OH groups react directly.Tannic acid rich hydroxyl groups could be used as hydrogen donors to connect with molecules containing hydrogen receptors forming stronger hydrogen bonds[8]. Tannin could interact with metals,proteins, alkaloids and polysaccharides to perform a variety of physiological and ecological functions.

    Supramolecular networks were self-assembled by various molecular interactions (hydrogen bonding, hydrophobic interaction,π-π superposition, electrostatic interaction and metal coordination).Individual metal ligand could provide stable and reversible cross-linking points between polymers to enable self-assembly of polymers[9]. Combining metal ions into supramolecular structures could improve their application performance and had a wide application prospect. It was a very efficient and useful method to encapsulate and deliver polyphenols by using environmental acidbase differences[10]. Tannins could interact with 18 different metal ions (AlIII, VIII, CrIII, MnII, FeIII, CoII, NiII, CuII, ZnII, ZrIV, MoII, RuIII,RhIII, CdII, CeIII, EuIII, GdIIIand TbIII) successfully prepared a robust metal phenolic network (MPN)[11]. The properties of MPN capsules were determined by the coordination metal and could control film thickness, disassembly characteristics and fluorescence behavior[12].This network structure could increase drug loading and had pH response characteristics, which were critical for the release of active substances[13].

    Compared with traditional encapsulated technology, polyphenols embeded in nanoparticles had the following advantages: 1) Volume effect and distribution specificity; 2) Surface modified nanocarriers could prolong the half-life in blood and achieve targeted release; 3) The absorption, transport and bioutilization efficiency of small intestinal cells were improved; 4) It could improve the physical and chemical stability of nutrients and avoid their early decomposition under the special pH environment of gastrointestinal and various digestive enzymes;5) The nanosystem was more stable and could prevent agglomeration,precipitation or emulsification of system particles[14].

    Nanoparticles were microscopic particles between 1 and 100 nm, usually spherical in structure and composed of a solid polymer matrix. It had good biocompatibility, natural non-toxicity and biodegradability[15]. There were many methods to prepare nanoparticles, including anti-solvent precipitation, liquid-liquid dispersion and phase separation. These preparation methods did not require complex equipment, low preparation conditions and high packaging efficiency[16]. Nanoparticles generally had a core-shell structure, which played an important role in loading, protecting and releasing bioactive substances. There were many substances that could be used as shell structures, such as polysaccharides, protein and aliphatic polyesters. The nuclear structure was generally well suited to encapsulating lipophilic small molecules. Encased bioactive substances could be isolated from the tissue environment, thus avoiding degradation or burst release caused by factors such as pH,temperature, enzymes, etc.

    In this study, PTN is encapsulated by zein and CQDs forming zein-PTN-CQDs nanoparticles. Then, TA and Fe3+were introduced to form metal-polyphenol network structure coating the surface of zein-PTN-CQDs nanoparticles. pH-responsive zein-PTN-CQDs-FeIIInanoparticles were prepared successfully. Zein-PTN-CQDs-FeIIInanoparticles are characterized by Fourier transform infrared (FTIR),X-ray diffraction (XRD), differential scanning calorimetry (DSC)and thermogravimetry analysis (TGA). The innovation of this work is based on the use of TA and Fe3+to obtain pH-responsive metalpolyphenol network structure.

    2. Materials and methods

    2.1 Materials

    D-Glucose (97%) and lysine (> 97%) were purchased from Beijing Solarbio Technology Co., Ltd.; zein (97%) was purchased from Shanghai Yuanye Bio-Technology Co., Ltd.; PTN was purchased from Tianmen Hengchang Chemical Co., Ltd. Tannic acid (AR) and FeCl3(99%) were purchased from Shanghai Macklin Biochemical Technology Co., Ltd. Carbon quantum dots (CQDs)were synthesized by glucose and lysine. Other analytical grade reagents were all from Tianjin Fengchuan Chemical Reagent Co., Ltd.

    2.2 Preparation of pH-responsive PTN-zein-CQDs nanoparticles

    2.2.1 Preparation of CQDs

    CQDs were generated by Maillard reaction[17]. First, 0.6 g glucose and 0.6 gL-lysine were dissolved in 40 mL deionized water in an ultrasonic processor (KQ-400 KDE, Kunshan Ultrasonic Instrument Co., Ltd., Kunshan, Jiangsu, China) to form solution which was heated in the microwave for 30 min. During this process, the color of the solution changed from colorless to light yellow, and eventually solid was formed indicating the formation of CQDs. Then, prepared CQDs were dissolved in a small amount of deionized water and centrifuged (10 000 r/min, 10 min) to remove solid precipitate obtaining supernatant which was further filtered by disposable needle filter (0.22 μm hydrophilic membrane). Finally, the supernatant was placed in a dialysis bag and dialyzed in deionized water for 24 h.After that, the supernatant was transferred to a freeze dryer (Free Zone 2.5, Labconco Corporation, Kansas city, Missouri, USA) and dried for one day (-40 °C) to obtain solid pure CQDs. Dried CQDs were kept at 4 °C for further use.

    2.2.2 Preparation of pH-responsive zein-FeIII and zein-CQDs-FeIII nanoparticles

    Zein (0.1 g) was dissolved in 70% (V/V) ethanol solution to form solution of concentration of 2 mg/mL, adding 500 μL 24 mmol/L tannic acid solution then. After mixing, 500 μL 24 mmol/L FeCl3was added. The solution was stirred with magnetic for 2 h, and then placed in a dialysis bag. After dialysis in pure water for 24 h, zein-FeIIInanoparticles were freeze-dried for later use.

    Zein (0.1 g) was dissolved in 70% (V/V) ethanol solution to form solution of concentration of 2 mg/mL. CQDs (0.02 g) were added,and then 500 μL 24 mmol/L tannic acid solution was added. After mixing, 500 μL 24 mmol/L FeCl3solution was added. The solution was magnetically stirred for 2 h, and then placed in a dialysis bag.After dialysis in pure water for 24 h, it was freeze-dried for later use,and zein-CQDS-FeIIInanoparticles were obtained.

    2.2.3 Preparation of pH-responsive zein-PTN-FeIII and zein-PTN-CQDs-FeIII nanoparticles

    First, 0.1 g zein and 0.01 g PTN were dissolved in 70% (V/V)ethanol solution. Second, the solution was stirred magnetically at 1 000 r/min for 1 h. Third, adding 500 μL 24 mmol/L tannic acid solution. After mixing, adding 500 μL 24 mmol/L FeCl3solution,freeze drying to obtain zein-PTN-FeIIIcomposite particles.

    First, 0.1 g zein and 0.01 g PTN were dissolved in 70% (V/V)ethanol solution, and added 0.02 g CQDs. Second, the solution was stirred magnetically at 1 000 r/min for 1 h. Third, adding 500 μL 24 mmol/L tannic acid solution. After mix well, adding 500 μL 24 mmol/L FeCl3solution, freeze drying to obtain zein-PTN-CQDs-FeIIIcomposite particles.

    2.3 Characterization of pH-responsive PTN-zein-CQDs nanoparticles

    2.3.1 Zeta-potential and particle size

    The size and zeta potential of prepared samples were measured by nano-particle analyzer. The sample was diluted to 0.1 mg/mL with deionized water, and particle size obtained was the cumulative average diameter. The temperature was measured at 25 °C for three times.

    2.3.2 Encapsulation efficiency (EE) and loading capacity (LC)

    Folinol method was used to measure EE and LC of nanoparticles.The gallic acid solution of 0.2 mg/mL was diluted to different concentrations of the standard solution. One milliliter gallic acid solution of different concentrations was mixed with 0.25 mol/L 1 mL folinol stand for 3 min, then adding 2 mL 15% Na2CO3solution standing for 30 min. The absorbance was measured by spectrophotometer at 760 nm to obtain standard curve of gallic acid.

    Sample solution (0.1 mg/mL) was prepared, and the absorbance was measured at 760 nm. The content of embedded PTN in the sample was calculated according to the following equation:

    2.3.3 TGA

    TGA was used to analyze the thermal stability of the prepared nanoparticles. Nitrogen was used as the protective gas and the flow rate was 50 mL/min. The thermogravimetric curve was obtained from 30 to 700 °C at a rate of 10 °C/min.

    2.3.4 DSC

    DSC was used to measure the thermal shrinkage temperature and thermal value of the sample. About 5 mg freeze-dried samples were weighed and placed in the crucible of a differential scanning calorimeter, sealed with a pressure plate, and heated from 20 to 250 °C with a temperature rise rate of 10 °C/min and nitrogen flow rate of 20 mL/min with an empty crucible as the control.

    2.3.5 FTIR spectroscopy

    FTIR spectroscopy could be used to obtain the chemical groups on the surface of particles, and the composition of samples could be analyzed according to the different vibration frequencies of different functional groups. A certain proportion of powder to be tested was mixed with potassium bromide and fully grounded in an agate mortar,and then the powder was pressed for testing. The scanning range was generally 400–4 000 cm-1with a resolution of 0.5 cm-1, and each group was repeated 3-5 times.

    2.3.6 XRD

    XRD was a technique to analyze the structure of crystalline materials. The object to be measured was made into dry powder.During the test, the scanning speed was 4°/min, the scanning range was 5° to 60°, the tube flow of the X-ray generator was 30 mA, the tube pressure was 36 kV, and three were parallel in each group.

    2.3.7 Fluorescence spectrum

    Deionized water was used to dilute the dispersion solution of composite colloidal particles to 0.2 mg/mL. Fluorescence spectra were scanned by fluorescence spectrophotometer with fluorescence group in zein molecule as probe. The excitation wavelength was 280 nm (excitation tryptophan fluorescence), and the emission wavelength was 290–450 nm. The excitation and emission slit widths were 5 and 3 nm, respectively.

    2.3.8 X-ray photoelectron spectroscopy (XPS)

    The surface elements of the freeze-dried samples were analyzed by XPS. Test conditions were: aluminum target (1 486.7 eV), high voltage 14.0 kV, power 250 W, pass energy 93.9 eV. Full scan is performed within 0–1 000 eV.

    2.4 Statistical analysis

    Univariate analysis of variance (ANOVA) analysis of all quantitative data (P< 0.05) was followed by the Duncan multiple range test, expressed as mean ± standard deviation (SD) (SPSS 22.0, SPSS Inc., Chicago, IL, USA). All figures were drawn using OriginPro 9.0 (OriginLab Co., Northampton, MA, USA). The datasets generated and/or analyzed during the current study are available from the corresponding author on reasonable request.

    3. Results and discussion

    3.1 Zeta-potential and particle size

    The particle size and potential of pH-responsive metal ion-coated nanoparticles are shown in Fig. 1. After introducing tannic acid and Fe3+into zein, the particle size was 957.33 nm and the potential was 7.12 mV. After the addition of CQDs and PTN, the particle size decreased to 717.63 and 559.93 nm, respectively, and the potential was negative (-4.42 mV) and positive (9.93 mV), which may be due to the electrostatic interaction between negatively charged CQDs and positively charged zein. The particle size decreased and the potential became negative. PTN tended to bind more tightly to proline-rich zein and formed a more compact structure. After the combination of zein,CQDs and PTN, the particle size was significantly reduced to 428.40 nm(P< 0.05). On the one hand, the electrostatic repulsion increased due to the increase of potential. On the other hand, a more intense interaction between three substances occurred and the addition of tannic acid and Fe3+formed a layer of polyphenol-metal encapsulation network on the surface of nanoparticles[8,18]. These results indicated that the addition of tannic acid and Fe3+could form nanoparticles with smaller particle size. Besides, SEM and TEM images of zein-FeIII,zein-CQDs-FeIII, zein-PTN-FeIII, zein-PTN-CQDs-FeIIInanoparticles were inserted in Fig. 2.

    Fig. 1 Mean size (a) and zeta-potential (b) of zein-FeIII, zein-CQDs-FeIII,zein-PTN-FeIII, zein-PTN-CQDs-FeIII nanoparticle. Different lowercase letters indicate significant differences (P < 0.05).

    Fig. 2 SEM and TEM images of zein-FeIII (a, e), zein-CQDs-FeIII (b, f),zein-PTN-FeIII (c, g), zein-PTN-CQDs-FeIII (d, h) nanoparticles.

    3.2 EE and LC

    The determination of EE and LC could effectively explain the embedding situation of polyphenols. Fig. 3 showed the EE and LC of zein-PTN-FeIIIand zein-PTN-CQDs-FeIII. The figure showed that the embedding rates of zein-PTN-FeIIIand zein-PTN-CQDs-FeIIIare 76.16% and 87.72% respectively, which was slightly higher than the EE of zein-PTN and zein-PTN-CQDs nanoparticles without tannic acid and Fe3+. This was due to the presence of tannic acid and Fe3+.There were multiple phenolic hydroxyl groups in the structure of tannic acid, and phenolic hydroxyl groups could have complexation and electrostatic interaction with Fe3+, forming supramolecular network structure on the surface of nanoparticles, and TA and Fe3+had synergistic effect on the encapsulation of polyphenols. The embedding rate of zein-PTN-CQDs-FeIIIwas higher than that of zein-PTN-FeIIIbecause the addition of CQDs provided more interaction sites and formed a more compact structure, tightly wrapping the PTN, which was consistent with the measurement results of particle size. The loading rates of zein-PTN-FeIIIand zein-PTN-CQDs-FeIIIare 8.96% and 6.83%, respectively, because the addition of CQDS increases the mass of nanoparticles after drying.According to the formula of loading rate in Equation 2, the LC of the latter decreased[19].

    Fig. 3 EE and LC of zein-PTN-FeIII and zein-PTN-CQDs-FeIII nanoparticles.

    3.3 TGA

    TGA was to analyze whether a substance was dehydrated,decomposed and vaporized according to the mass change in the heating process[20]. Thermogravimetric curves of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIIIwere shown in Fig. 4. As could be seen from Fig. 4, the mass loss of the four nanoparticles could be roughly divided into three stages. In the zein-FeIIIcurve, the first stage was between 50 and 250 °C, with only a slight weight loss (4%) due to the loss of free and bound water of the nanoparticles; The second stage was 250 to 574 °C, where mass loss was very high (81%) due to thermal decomposition of zein. The final stage was from 574 to 690 °C, during which the mass loss remains about the same, leaving only some solid residue to decompose at a very slow rate. After the addition of CQDs and PTN, zein-CQDs-FeIII,zein-PTN-FeIIIand zein-PTN-CQDs-FeIIInanoparticles were not very different from zein-FeIIInanoparticles in the first and third stages.But the mass loss in the second phase was 67%, 68%, and 63%,respectively. This indicated that zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIIInanoparticles had higher thermal stability than zein-FeIIInanoparticles. In particularly, zein-PTN-CQDs-FeIIInanoparticles had the highest thermal stability[21].

    Fig. 4 TGA thermogram of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIII,and zein-PTN-CQDs-FeIII nanoparticles.

    3.4 DSC

    The thermal properties of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIIInanoparticles were studied by DSC.DSC curves and denaturation temperature (Tm) and enthalpy change (ΔH) of the four nanoparticles were shown in Fig. 5 and Table 1, respectively. The first peak of the four curves was smaller than the second peak in bothTmand ΔH. The first peakTmof zein-FeIIInanoparticles was 64.08 °C and ΔHwas 8.31 J/g. With the addition of CQDs and PTN,Tmand ΔHwere significantly increased to 67.45 and 70.86 °C, respectively, and 9.42 and 10.35 J/g,respectively (P< 0.05), indicating that the addition of CQDs and PTN could improve the thermal denaturation resistance of nanoparticles.When CQDs and PTN were added at the same time,Tmand ΔHincreased further,Tmincreased to 72.09 °C, ΔHincreased to 10.83 J/g,indicating that the addition of CQDs and PTN at the same time could improve the thermal denaturing ability of nanoparticles more than the addition of PTN alone. The second peak of zein-FeIIInanoparticles was thermal denaturated at 121.15 °C, and ΔHwas 85.81 J/g.Compared with CQDs and PTN alone, the stable structure of zein-FeIIInanoparticles was formed by the interaction between CQDs and PTN at the same time.Tm(135.15 °C) and ΔH(102.25 J/g) were improved.The thermal stability was improved. The zein-PTN-CQDs-FeIIIcurve has two peaks and the thermal denaturation temperature of the second peak (135.15 °C) increases, which may be because the addition of TA and Fe3+causes the thermal denaturation of nanoparticles at 72.09 °C.TA and Fe3+formed a metal-polyphenol network on the surface of nanoparticles to improve their thermal resistance[22].

    Table 1 Thermal denaturation temperature and enthalpy of zein-FeIII, zein-CQDs-FeIII,zein-PTN-FeIII, and zein-PTN-CQDs-FeIII nanoparticles.

    Fig. 5 DSC thermogram of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIII,and zein-PTN-CQDs-FeIII nanoparticles.

    3.5 FTIR spectroscopy

    Infrared spectroscopy was used to study the interactions among zein, PTN, CQDs and TA, and to explore the interactions that occurred during the formation of nanoparticles. Bands in the spectrum could be connected with specific functional groups in related molecules[23]. Zein-FeIII, zein-CQDS-FeIII, zein-PTN-FeIII, zein-PTNCQDs-FeIIIand the infrared spectra of zein, PTN and TA were shown in Fig. 6. The hydrogen bond characteristic peak of zein at 3 346 cm-1shifted to 3 425, 3 439, 3 448 and 3 404 cm-1in the infrared curves of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIII,respectively, which represented the formation of hydrogen bonds. The amide I band of zein (1 647 cm-1) represented the stretching vibration of C=O, and moved to the vicinity of 1 652 cm-1in all 4 curves, and the intensity of zein-PTN-CQDs-FeIIIcurve was greater than that of the other three curves. This might be due to the stronger hydrogen bond and hydrophobic interaction formed by the simultaneous addition of PTN and CQDs. In addition, the vibration of TA at 3 417 cm-1was caused by O-H stretching vibration. Representing carboxyl and carbonyl groups at 1 715, 1 611 and 1 534 cm-1represent -C=C- groups in the aromatic ring. The peak at 1 448 cm-1represented the deformation of -C-C- in phenol; 1 324 cm-1represented the phenol group; 1 203 cm-1represents C-H bond,1 088 cm-1represented the deformation of -C-O- in phenol;1 031 cm-1represented the deformation of C-H; peaks at 868 and 757 cm-1represented the C-H bond on the benzene ring. But these characteristic peaks disappeared after the nanoparticle was formed.This indicated that TA was involved in the formation of nanoparticles and interacts with zein, PTN and CQDs[24].

    Fig. 6 FTIR of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIII, zein-PTN-CQDs-FeIII nanoparticles (a), and zein powder, TA powder (b).

    3.6 XRD

    XRD was usually used to evaluate the crystallinity of the encapsulated or biopolymer matrix[25]. Fig. 7 showed the XRD patterns of FeCl3, TA, zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIII. FeCl3has sharp peaks at 14.78°, 15.18°,28.12°, 36.74° and 46.42°, indicating that FeCl3was in a highly crystalline state. The wide peak at 24.52° indicates that TA was in an amorphous state. However, zein-FeIII, zein-CQDs-FeIII, zein-PTNFeIIIand zein-PTN-CQDs-FeIIIshowed a new wide peak at 21.12°,and the crystallization peak of FeCl3disappeared. This indicated that metal ion-polyphenol network was formed between FeCl3and TA, and the coated film was formed on the surface of nanoparticles,and the nanoparticles formed were in an amorphous state. The 4 curves of zein-CQDS-FeIII, zein-PTN-FeIII, zein-PTN-CQDs-FeIIIand zein-FeIIIwere similar, but the intensity of the first three peaks was higher than that of zein-FeIII. This indicated that the interaction during the formation of zein-FeIIInanoparticles was not as strong as that of the first three nanoparticles. In addition, compared with zein-FeIII,zein-CQDs-FeIIIand zein-PTN-FeIII, the curves of zein-PTN-CQDs-FeIIInanoparticles showed a new small peak at 58.72°. The emergence of new peaks indicated that intermolecular interactions occured between FeCl3, TA, zein, PTN and CQDs, and the intermolecular interactions changed the physical states of each substance before the reaction[26]. The above results indicated that zein-PTN-CQDs nanoparticles could be formed by adding FeCl3and TA based on intermolecular interaction.

    Fig. 7 XRD spectra of FeCl3, TA, zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIII,zein-PTN-CQDs-FeIII nanoparticles.

    3.7 Fluorescence spectrum

    Fluorescence spectroscopy was a technique widely used to study proteins and peptides. Aromatic amino acids, such as tryptophan,tyrosine and phenylalanine, had inherent fluorescence and could provide information on protein conformation, dynamics and intermolecular interactions. In this paper, the interaction between biopolymers was studied by analyzing the fluorescence intensity of tryptophan residues, which were highly sensitive to changes in the surrounding environment of proteins, excited at 280 nm[19]. Fig. 8 showed the fluorescence spectra curves of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIIIand zein-PTN-CQDs-FeIII. After the addition of TA and Fe3+, the fluorescence emission peak shifted to the vicinity of 340 nm and the fluorescence intensity was also enhanced. On the one hand, the addition of TA and Fe3+made the denaturation of zein greater, and the fluorescence chromogenetic group inside, namely tryptophan, was more exposed. On the other hand, there were many phenolic hydroxyl groups and aromatic rings in the structure of PTN and TA, which increased the number and degree of thickening of rings[27]. Compared with TA and Fe3+alone, the fluorescence intensity was stronger when TA and Fe3+were added at the same time, which might be because TA and Fe3+were water-soluble substances, and the polar environment of the protein was changed when TA and Fe3+were added at the same time, and the fluorescent chromogenic groups inside the protein were more exposed to the polar environment, and the fluorescence intensity increased[28].

    Fig. 8 Fluorescence spectra of zein-FeIII, zein-CQDs-FeIII, zein-PTN-FeIII, and zein-PTN-CQDs-FeIII nanoparticles.

    3.8 XPS

    The nanoparticles were characterized by XPS, which could be used to analyze the types of elements on the surface of nanomaterials[21]. Fig. 9 showed the XPS spectra of each substance.Fig. 9a was the XPS spectrum of zein. It could be seen from the figure that the signal of C, N and O elements on zein surface was very strong, indicating the existence of these three elements. Zein was composed of a large number of amino acids, among which the carboxyl group (-COOH) and the amino group (-NH2) contain a large number of C, N and O elements. After the addition of PTN and CQDs (Fig. 9b), the peak intensity of O signal and N signal increased significantly, while the intensity of C signal decreased slightly. C1spectrum includes 4 peaks of C-C/C-H (284.88 eV),O-C-O (287.97 eV), and C-O-H (286.54 eV) (Fig. 9d).O1sspectrum includes three peaks C=O (531.51 eV), C-O-H/C-O-C(533.43 eV) and O-H (532.33 eV) (Fig. 9e), and N1sspectrum includes two peaks N-H (401.45 eV) and C-N-C (399.51 eV)(Fig. 9f)[26]. After modification with TA and Fe3+, a weak Fe signal peak appeared at 702.94 eV. Meanwhile, compared with the XPS spectra of zein-PTN-CQDS, the C1sspectrum had a more C=N signal peak (289.25 eV) (Fig. 9c). In the C1sspectrum of zein-PTN-CQDSFeIII, C-C/C-H peak at 284.88 eV, C-O-H peak at 286.54 eV,O-C-O peak at 287.97 eV, O=C-O peak at 288.41 eV. At 289.25 eV,there was a peak C=N (Fig. 9g); In O1sspectrum, C=O peak at 531.52 eV, O-H peak at 533.82 eV, C-O-H/C-O-C peak at 532.75 eV(Fig. 9h); In N1sspectrum, there was a C-N-C peak at 400.62 eV and an N-H peak at 402.35 eV (Fig. 9k). Based on the type distribution of surface elements and the binding energy and strength of various chemical bonds, it could be concluded that TA and Fe3+form a layer of polyphenol-metal encapsulation network on the surface of nanoparticles[16].

    Fig. 9 XPS spectra of zein (a), zein-PTN-CQDs (b), zein- PTN-CQDs-FeIII (c), zein-PTN-CQDs C1s (d), zein-PTN-CQDs O1s (e), zein-PTN-CQDs N1s (f),zein-PTN-CQDs-FeIII C1s (g), zein-PTN-CQDs-FeIII O1s (h), zein-PTN-CQDs-FeIII N1s (i).

    4. Conclusion

    In the present study, pH responsive zein-PTN-CQDSFeIIInanocomposites are prepared to improve the stability and bioavailability of PTN and a series of methods (FTIR, XRD, DSC,TGA and XPS) are used to characterize the nanoparticles. The zein-PTN-CQDS-FeIIIsupramolecular systems are formed by noncovalent interactions, offering improvement of PTN physicochemical properties as water solubility, thermal stability and its slow release in biological systems. Additionally, TA and Fe3+formed metalpolyphenol network structure endowed nanoparticles with pH response characteristics, which made nanoparticles stable under neutral condition while disintegrated under acidic conditions. This work is of great potential for pH-responsive nanoparticles as delivery vehicle for bioactive compounds.

    Conflict of interests

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgements

    This study is supported by the National Key R&D Program of China (2018YFD0901106), the Wenzhou Major Science and Technology Project (ZN2021002) and the Ningbo “3315 series program” for high-level talents (2020B-34-G).

    18禁美女被吸乳视频| 变态另类成人亚洲欧美熟女| 国产99白浆流出| 搡女人真爽免费视频火全软件 | 少妇人妻一区二区三区视频| 国产成年人精品一区二区| 18禁美女被吸乳视频| 在线看三级毛片| 蜜桃亚洲精品一区二区三区| 欧美中文日本在线观看视频| 久久精品国产99精品国产亚洲性色| 在线免费观看不下载黄p国产 | 成年女人永久免费观看视频| 悠悠久久av| 在线观看免费午夜福利视频| 成年人黄色毛片网站| av天堂中文字幕网| 成人亚洲精品av一区二区| 日韩亚洲欧美综合| 免费人成视频x8x8入口观看| 久久精品91无色码中文字幕| a在线观看视频网站| 国产亚洲av嫩草精品影院| 又爽又黄无遮挡网站| 国产综合懂色| 在线播放无遮挡| 搞女人的毛片| 身体一侧抽搐| 日本黄色视频三级网站网址| 午夜影院日韩av| 国产精品久久久久久精品电影| 久久久成人免费电影| 国产精品影院久久| 丁香欧美五月| 色综合亚洲欧美另类图片| av在线天堂中文字幕| 国产精品 国内视频| 黄片大片在线免费观看| 国产精品美女特级片免费视频播放器| 欧美日韩一级在线毛片| 尤物成人国产欧美一区二区三区| 两个人视频免费观看高清| 欧美成人一区二区免费高清观看| 啦啦啦免费观看视频1| 男女床上黄色一级片免费看| 69av精品久久久久久| 欧美日韩福利视频一区二区| 国产久久久一区二区三区| 成年女人毛片免费观看观看9| 亚洲欧美激情综合另类| 国产69精品久久久久777片| 欧美色欧美亚洲另类二区| 男女之事视频高清在线观看| 欧美黑人巨大hd| 午夜免费激情av| 热99re8久久精品国产| 特大巨黑吊av在线直播| 尤物成人国产欧美一区二区三区| 一级毛片女人18水好多| 好看av亚洲va欧美ⅴa在| 一级黄色大片毛片| 国产高清视频在线播放一区| 一区福利在线观看| 亚洲国产欧洲综合997久久,| 桃红色精品国产亚洲av| 少妇的丰满在线观看| xxxwww97欧美| 色噜噜av男人的天堂激情| 丁香欧美五月| 国产蜜桃级精品一区二区三区| 久久中文看片网| 亚洲av电影在线进入| 亚洲aⅴ乱码一区二区在线播放| 国内毛片毛片毛片毛片毛片| 午夜福利视频1000在线观看| 麻豆国产av国片精品| 国产视频内射| 国产精品 欧美亚洲| 看免费av毛片| www日本在线高清视频| 日本黄大片高清| av在线蜜桃| 久久精品人妻少妇| 国产精品久久久久久精品电影| av在线天堂中文字幕| 国产单亲对白刺激| 99视频精品全部免费 在线| 久久国产精品影院| АⅤ资源中文在线天堂| 最新在线观看一区二区三区| 成年版毛片免费区| 91麻豆精品激情在线观看国产| 国产成人影院久久av| 精品久久久久久久久久免费视频| 嫩草影视91久久| 听说在线观看完整版免费高清| 69av精品久久久久久| 丰满人妻熟妇乱又伦精品不卡| 国产乱人伦免费视频| 国产成人系列免费观看| 欧美激情在线99| 国产精品美女特级片免费视频播放器| 99久久99久久久精品蜜桃| 国产成人系列免费观看| 国产精品 国内视频| 国产 一区 欧美 日韩| 亚洲精品一卡2卡三卡4卡5卡| 国产免费av片在线观看野外av| 蜜桃亚洲精品一区二区三区| 久久精品亚洲精品国产色婷小说| 亚洲激情在线av| 午夜精品在线福利| 一本综合久久免费| 精品国产美女av久久久久小说| 黄片大片在线免费观看| 日韩欧美在线乱码| 日韩成人在线观看一区二区三区| 十八禁人妻一区二区| 中文字幕久久专区| 午夜福利18| 日日干狠狠操夜夜爽| 久久伊人香网站| 在线天堂最新版资源| 搡女人真爽免费视频火全软件 | 亚洲在线自拍视频| 午夜福利18| 久久亚洲真实| 亚洲人成网站高清观看| 97碰自拍视频| 色播亚洲综合网| 精品久久久久久久久久久久久| 久久国产精品影院| 久久久精品欧美日韩精品| 少妇的丰满在线观看| 免费av不卡在线播放| 日韩欧美一区二区三区在线观看| 国产麻豆成人av免费视频| 好看av亚洲va欧美ⅴa在| 最新中文字幕久久久久| 亚洲精品久久国产高清桃花| 一级毛片高清免费大全| 精品久久久久久,| 日本 欧美在线| 久久久精品大字幕| 人人妻人人澡欧美一区二区| 国产高清有码在线观看视频| 国产av一区在线观看免费| 日本黄大片高清| 国产一区二区亚洲精品在线观看| 亚洲人成伊人成综合网2020| 国语自产精品视频在线第100页| 亚洲av免费在线观看| 1024手机看黄色片| 久久精品亚洲精品国产色婷小说| 中文字幕人妻丝袜一区二区| 午夜福利成人在线免费观看| 欧美一区二区精品小视频在线| 18禁在线播放成人免费| 欧美极品一区二区三区四区| 不卡一级毛片| 亚洲七黄色美女视频| av黄色大香蕉| 亚洲 国产 在线| а√天堂www在线а√下载| 真实男女啪啪啪动态图| 久久久久亚洲av毛片大全| 91在线精品国自产拍蜜月 | 欧美日韩中文字幕国产精品一区二区三区| 久久精品国产99精品国产亚洲性色| 激情在线观看视频在线高清| a级毛片a级免费在线| 欧美中文日本在线观看视频| 日本黄大片高清| 欧美性猛交黑人性爽| 国产视频内射| 熟女电影av网| 天天添夜夜摸| 高潮久久久久久久久久久不卡| 午夜免费成人在线视频| 久久午夜亚洲精品久久| 免费无遮挡裸体视频| www.999成人在线观看| aaaaa片日本免费| 一个人看的www免费观看视频| 在线免费观看的www视频| 狂野欧美白嫩少妇大欣赏| 香蕉久久夜色| 国产精品免费一区二区三区在线| 久久精品国产99精品国产亚洲性色| 婷婷精品国产亚洲av| 五月玫瑰六月丁香| 99精品久久久久人妻精品| 欧美乱色亚洲激情| 亚洲熟妇熟女久久| svipshipincom国产片| 久久久久久人人人人人| 最近最新免费中文字幕在线| 91九色精品人成在线观看| 国产伦精品一区二区三区视频9 | 国产高清视频在线播放一区| 亚洲精华国产精华精| 国产欧美日韩精品一区二区| 欧美在线黄色| 午夜激情欧美在线| 国产视频一区二区在线看| 乱人视频在线观看| 一本精品99久久精品77| 中文字幕av成人在线电影| 少妇裸体淫交视频免费看高清| 亚洲av不卡在线观看| 九九在线视频观看精品| 俄罗斯特黄特色一大片| 精品国内亚洲2022精品成人| 久久久成人免费电影| 在线观看日韩欧美| 又紧又爽又黄一区二区| 91在线精品国自产拍蜜月 | 天美传媒精品一区二区| 一级毛片女人18水好多| 久久精品国产清高在天天线| 婷婷丁香在线五月| 日本黄大片高清| 欧美一区二区亚洲| 99热这里只有是精品50| 97人妻精品一区二区三区麻豆| 久久久久国内视频| 亚洲va日本ⅴa欧美va伊人久久| 天堂动漫精品| 国产成人啪精品午夜网站| 97碰自拍视频| 免费观看的影片在线观看| 中文字幕av在线有码专区| 男女下面进入的视频免费午夜| 欧美成狂野欧美在线观看| 少妇熟女aⅴ在线视频| 国产一区二区在线av高清观看| 亚洲男人的天堂狠狠| 国产乱人视频| 高清毛片免费观看视频网站| 亚洲欧美日韩东京热| 国产精品,欧美在线| 成年免费大片在线观看| 精品一区二区三区视频在线观看免费| 亚洲国产精品成人综合色| 国产av麻豆久久久久久久| 亚洲精品日韩av片在线观看 | 国产老妇女一区| 国产黄a三级三级三级人| 午夜福利成人在线免费观看| 伊人久久大香线蕉亚洲五| 日韩欧美精品免费久久 | 精华霜和精华液先用哪个| 青草久久国产| 日韩国内少妇激情av| 五月玫瑰六月丁香| 亚洲人成网站在线播| 一区二区三区高清视频在线| 变态另类成人亚洲欧美熟女| or卡值多少钱| 精品久久久久久久人妻蜜臀av| 中文字幕人成人乱码亚洲影| 操出白浆在线播放| 精品国产亚洲在线| 亚洲精品影视一区二区三区av| 午夜视频国产福利| 国产一区二区在线观看日韩 | 亚洲中文字幕一区二区三区有码在线看| 国产一区二区在线av高清观看| 久久久久精品国产欧美久久久| 午夜影院日韩av| 国产真实乱freesex| 少妇熟女aⅴ在线视频| 有码 亚洲区| 成人亚洲精品av一区二区| 亚洲av成人不卡在线观看播放网| 真人一进一出gif抽搐免费| 国语自产精品视频在线第100页| 深爱激情五月婷婷| 久久国产精品人妻蜜桃| 国产欧美日韩一区二区三| 久久精品国产99精品国产亚洲性色| 身体一侧抽搐| 久久午夜亚洲精品久久| 欧美三级亚洲精品| 欧美日韩乱码在线| 搡老熟女国产l中国老女人| 九色成人免费人妻av| 99热这里只有精品一区| 村上凉子中文字幕在线| 精品无人区乱码1区二区| 国产午夜福利久久久久久| 欧美在线一区亚洲| 看片在线看免费视频| 色吧在线观看| 免费看日本二区| 人妻夜夜爽99麻豆av| 亚洲黑人精品在线| 99国产精品一区二区三区| 国产亚洲欧美在线一区二区| 国产探花在线观看一区二区| 欧美午夜高清在线| av黄色大香蕉| 国产主播在线观看一区二区| 内地一区二区视频在线| 丁香欧美五月| 91麻豆av在线| 成人三级黄色视频| 国产精品久久久久久久久免 | 男女做爰动态图高潮gif福利片| 午夜激情欧美在线| 精品一区二区三区人妻视频| a在线观看视频网站| 免费无遮挡裸体视频| 一夜夜www| 18+在线观看网站| 国产成年人精品一区二区| 亚洲第一电影网av| 国产精品久久久久久精品电影| 国产单亲对白刺激| 亚洲国产精品999在线| aaaaa片日本免费| 精品电影一区二区在线| 51国产日韩欧美| 99视频精品全部免费 在线| а√天堂www在线а√下载| 好看av亚洲va欧美ⅴa在| 欧美性猛交黑人性爽| 国产高清三级在线| 久久99热这里只有精品18| 色视频www国产| av在线蜜桃| 欧美成人一区二区免费高清观看| 免费无遮挡裸体视频| 国产高清有码在线观看视频| 久久精品国产综合久久久| 女生性感内裤真人,穿戴方法视频| 欧美一级a爱片免费观看看| 最新中文字幕久久久久| 色综合欧美亚洲国产小说| 日本与韩国留学比较| 最近在线观看免费完整版| 欧美日韩综合久久久久久 | 黄色女人牲交| 午夜久久久久精精品| 国产主播在线观看一区二区| 欧美日韩亚洲国产一区二区在线观看| 国产一区二区在线观看日韩 | 人人妻,人人澡人人爽秒播| 51国产日韩欧美| 精品一区二区三区人妻视频| 久久久久国内视频| 成年女人看的毛片在线观看| 欧美成人一区二区免费高清观看| 国产黄片美女视频| 99久久无色码亚洲精品果冻| 757午夜福利合集在线观看| 亚洲欧美一区二区三区黑人| 日本熟妇午夜| 51午夜福利影视在线观看| 内射极品少妇av片p| 国产亚洲欧美在线一区二区| 亚洲国产欧美网| 亚洲无线在线观看| 亚洲成av人片在线播放无| 老汉色av国产亚洲站长工具| 真人做人爱边吃奶动态| a级毛片a级免费在线| 欧美最黄视频在线播放免费| 国产亚洲欧美在线一区二区| 国产亚洲精品综合一区在线观看| 午夜福利免费观看在线| 午夜免费男女啪啪视频观看 | 欧美最新免费一区二区三区 | 狂野欧美白嫩少妇大欣赏| av在线蜜桃| 美女cb高潮喷水在线观看| 欧美最新免费一区二区三区 | 非洲黑人性xxxx精品又粗又长| 伊人久久大香线蕉亚洲五| 午夜激情欧美在线| 男人舔奶头视频| 成人性生交大片免费视频hd| 日韩欧美 国产精品| 日本一二三区视频观看| 99视频精品全部免费 在线| 嫩草影院入口| 一级黄色大片毛片| 男人和女人高潮做爰伦理| 小说图片视频综合网站| 十八禁人妻一区二区| 亚洲 欧美 日韩 在线 免费| 麻豆成人午夜福利视频| av在线蜜桃| 成年人黄色毛片网站| 国产免费一级a男人的天堂| 男人的好看免费观看在线视频| 国产精品98久久久久久宅男小说| 十八禁人妻一区二区| 国产99白浆流出| 成人av在线播放网站| 人妻夜夜爽99麻豆av| 一本一本综合久久| 久久久久久人人人人人| 欧美色欧美亚洲另类二区| 欧美又色又爽又黄视频| 亚洲人成伊人成综合网2020| 亚洲成人中文字幕在线播放| 99热这里只有精品一区| avwww免费| 欧美国产日韩亚洲一区| 久久久久久久久久黄片| 欧美一级a爱片免费观看看| 亚洲av免费在线观看| 日本一本二区三区精品| 国产欧美日韩精品亚洲av| 国产伦精品一区二区三区四那| 老汉色av国产亚洲站长工具| 99久久99久久久精品蜜桃| 亚洲av一区综合| 欧美乱色亚洲激情| 最近最新免费中文字幕在线| 国内精品美女久久久久久| 久久久国产成人免费| 国产乱人视频| 两人在一起打扑克的视频| 亚洲精品日韩av片在线观看 | 成人三级黄色视频| 在线播放国产精品三级| 天堂动漫精品| 欧美日本视频| 欧美zozozo另类| 亚洲色图av天堂| 中国美女看黄片| 国产一区二区三区视频了| 18禁黄网站禁片午夜丰满| av天堂在线播放| 婷婷丁香在线五月| 香蕉av资源在线| av视频在线观看入口| 国产精品1区2区在线观看.| www.www免费av| 亚洲成人久久性| 无人区码免费观看不卡| 国产真人三级小视频在线观看| 欧美中文综合在线视频| 波多野结衣高清作品| 成人欧美大片| 国内毛片毛片毛片毛片毛片| 亚洲精品一卡2卡三卡4卡5卡| 毛片女人毛片| 日韩欧美 国产精品| 操出白浆在线播放| 午夜影院日韩av| 久久草成人影院| 国内揄拍国产精品人妻在线| 亚洲精品乱码久久久v下载方式 | 99热精品在线国产| 国产精品爽爽va在线观看网站| 少妇的逼水好多| 99在线人妻在线中文字幕| 亚洲中文日韩欧美视频| 日日干狠狠操夜夜爽| 久久香蕉精品热| 一级作爱视频免费观看| 亚洲真实伦在线观看| www国产在线视频色| 久久99热这里只有精品18| 真实男女啪啪啪动态图| 国产黄a三级三级三级人| 欧美日本视频| 久久精品91无色码中文字幕| 日韩免费av在线播放| 日本黄色片子视频| 一区福利在线观看| 99热精品在线国产| av在线天堂中文字幕| 白带黄色成豆腐渣| 十八禁人妻一区二区| 91字幕亚洲| 欧美一级毛片孕妇| 男女床上黄色一级片免费看| netflix在线观看网站| 女人十人毛片免费观看3o分钟| av福利片在线观看| 1024手机看黄色片| 精品人妻1区二区| 欧美另类亚洲清纯唯美| АⅤ资源中文在线天堂| 免费看光身美女| 国产精品久久视频播放| 日韩免费av在线播放| 99久久综合精品五月天人人| 欧美黑人欧美精品刺激| 国产亚洲精品av在线| 最近最新免费中文字幕在线| 中文字幕av成人在线电影| 欧美黄色淫秽网站| 国产精品免费一区二区三区在线| netflix在线观看网站| 嫩草影院入口| 每晚都被弄得嗷嗷叫到高潮| 国产v大片淫在线免费观看| av欧美777| 夜夜躁狠狠躁天天躁| 亚洲性夜色夜夜综合| h日本视频在线播放| 午夜精品在线福利| 丁香欧美五月| 亚洲欧美日韩高清在线视频| 叶爱在线成人免费视频播放| 中文亚洲av片在线观看爽| 精品无人区乱码1区二区| 久久这里只有精品中国| 国产成人a区在线观看| 久久久国产精品麻豆| 岛国在线观看网站| 精品一区二区三区视频在线 | 精品一区二区三区av网在线观看| 在线观看美女被高潮喷水网站 | 人人妻人人澡欧美一区二区| 法律面前人人平等表现在哪些方面| 国产国拍精品亚洲av在线观看 | 国产精品精品国产色婷婷| 亚洲精品一卡2卡三卡4卡5卡| 一进一出抽搐动态| 久久这里只有精品中国| 夜夜躁狠狠躁天天躁| 国产伦人伦偷精品视频| 色哟哟哟哟哟哟| 免费看日本二区| 精品国产美女av久久久久小说| 小蜜桃在线观看免费完整版高清| 成人午夜高清在线视频| 夜夜看夜夜爽夜夜摸| 最新在线观看一区二区三区| 精品乱码久久久久久99久播| 香蕉久久夜色| 成年人黄色毛片网站| 亚洲国产精品999在线| 国内精品久久久久精免费| а√天堂www在线а√下载| 老汉色∧v一级毛片| 国产v大片淫在线免费观看| 日韩欧美三级三区| 国产伦在线观看视频一区| 午夜福利在线观看吧| 国产精品久久久久久亚洲av鲁大| 日韩欧美国产在线观看| 免费大片18禁| 亚洲人成网站在线播放欧美日韩| 美女高潮的动态| 高清日韩中文字幕在线| 久久久久久久久中文| 免费看十八禁软件| 亚洲美女黄片视频| 黑人欧美特级aaaaaa片| а√天堂www在线а√下载| 国产高潮美女av| 最新在线观看一区二区三区| 亚洲国产欧洲综合997久久,| 内射极品少妇av片p| 精品免费久久久久久久清纯| 国产精品国产高清国产av| 18禁美女被吸乳视频| 国产淫片久久久久久久久 | 国产高清videossex| 亚洲精品国产精品久久久不卡| 国产免费男女视频| 一个人观看的视频www高清免费观看| 国产伦一二天堂av在线观看| а√天堂www在线а√下载| www日本在线高清视频| 桃红色精品国产亚洲av| 午夜免费成人在线视频| 在线免费观看不下载黄p国产 | 搞女人的毛片| 欧美成人一区二区免费高清观看| 亚洲电影在线观看av| 99精品久久久久人妻精品| 国产精品影院久久| 国产日本99.免费观看| 日韩欧美精品v在线| 久久草成人影院| 国产欧美日韩一区二区三| 真人做人爱边吃奶动态| а√天堂www在线а√下载| 网址你懂的国产日韩在线| 在线观看午夜福利视频| 国产高潮美女av| 精品无人区乱码1区二区| 国产一区二区在线观看日韩 | 91久久精品电影网| 别揉我奶头~嗯~啊~动态视频| 神马国产精品三级电影在线观看| 久久久久性生活片| 国产av在哪里看| 成人18禁在线播放| 十八禁网站免费在线| 欧美高清成人免费视频www| 制服丝袜大香蕉在线| 小说图片视频综合网站| 亚洲成av人片免费观看| 99国产极品粉嫩在线观看| 女人被狂操c到高潮| 18禁国产床啪视频网站| 国产伦精品一区二区三区四那| 18禁在线播放成人免费| 成年版毛片免费区| 麻豆成人午夜福利视频| 伊人久久大香线蕉亚洲五| 午夜福利成人在线免费观看| 国产蜜桃级精品一区二区三区| 精品一区二区三区av网在线观看| 九九热线精品视视频播放| 老司机深夜福利视频在线观看|