    Performance of a Hierarchically Nanostructured W–Cu Composite Produced via Mediating Phase Separation

    2024-01-22 10:36:54ChoHouHoLuZhiZhoXintoHungTielongHnJunhuLunZengoJioXioynSongZuorenNie
    Engineering 2023年7期

    Cho Hou*, Ho Lu Zhi Zho Xinto Hung Tielong Hn Junhu Lun, Zengo Jio,Xioyn Song*, Zuoren Nie

    a Key Laboratory of Advanced Functional Materials, Ministry of Education, Faculty of Materials and Manufacturing, Beijing University of Technology, Beijing 100124, China

    b Department of Materials Science and Engineering, City University of Hong Kong, Hong Kong 999077, China

    c Department of Mechanical Engineering, The Hong Kong Polytechnic University, Hong Kong 999077, China

    Keywords:Immiscible-component composite Phase separation Nanostructure Mechanical properties Interface modulation

    ABSTRACT The challenge of fabricating nanostructured W–Cu composites by powder metallurgy has been solved by means of modulated phase separation.A hierarchically nanostructured (HN) W–Cu composite was prepared using intermediary Al through sluggish asynchronous phase separation.In addition to a dual network composed of a Cu phase and the W–Cu nanostructure,dense Al-containing nanoprecipitates with a body-centered cubic (bcc) structure are distributed in the W matrix.Compared with a pristine W/Cu interface,the newly formed W/Cu interfaces modulated by Al and the coherent W/Al-containing particle interfaces possess lower energy and enhanced bonding strength due to efficient electron transfer and strong coupling interactions.With a large number of stable heterogeneous interfaces and a ‘‘selflocking” geometry, the HN W–Cu composite exhibits excellent resistance against plastic deformation.The combination of the presented composite’s hardness and compressive strength outperforms all other sintered W–Cu composites with the same Cu content.Under a reciprocating sliding load, the reactive Al prevents excessive oxidation.The excellent synergy of the hardness and toughness of the friction-induced surface endows the HN composite with high abrasion resistance.This study provides a new strategy to modulate the structure and energy state of interfaces in metallic composites containing immiscible components in order to achieve high mechanical performance.

    1.Introduction

    Metallic X–copper(Cu)composites(where X denotes refractory metals such as tungsten(W),molybdenum(Mo),tantalum(Ta),or niobium(Nb))play an irreplaceable role in the aerospace and electric power industries due to their excellent strength, hardness,radiation-damage tolerance, and shock resistance in comparison with other materials [1–5].As the size of individual X and Cu phases decreases within a specific range, a ‘‘smaller-is-stronger”trend is always observed.This phenomenon has been widely investigated in lamellar X–Cu materials [6–8], with a great number of studies revealing that lamellar X–Cu can be orders of magnitude stronger than its homogeneous counterparts under compressive and tensile loads.

    These remarkable strengthening and hardening effects can be attributed to the unique interaction between the X/Cu interfaces and dislocations.When the dislocations glide to the vicinity of weakly bound X/Cu interfaces, they are easily captured by the interfaces through local shearing, leading to the spreading of the dislocation core across the interfaces [9,10].Therefore, having heterogeneous interfaces with high density can effectively limit dislocation transmission and improve the mechanical performance of X–Cu composites.Reducing one (e.g.the lamellar materials) or multiple dimensions of the phases inside X–Cu down to the nanoscale is an effective way to achieve sufficient interfaces.

    The topological configuration of the interfaces affects the mechanical behavior of metallic composites.The interfaces of lamellar materials are only abundant in a certain direction.A long-distance slip of dislocations within the interface plane tends to stress relaxation and softening [11–13].As a result, the strengthening of the material is not thorough.In comparison, a composite of mutually interpenetrating components leaves three-dimensionally distributed interfaces in the space, which are more effective in preventing the long-distance slip of dislocations[14].The intrinsic character of the interface, such as the compositional distribution and morphology, also contributes to the mechanical properties by modulating the bonding strength and interactions with dislocations.For example, it has been confirmed that interfaces with mutually compositional intervention can better resolve the contradiction between strength and plasticity due to their higher shear resistance in comparison with well-defined interfaces [15,16].Wavy X/Cu interfaces, as another example, feature a robust size-scaling effect and are more resistant to dislocation slip than planar interfaces [17].Therefore, it is desirable to have X–Cu composites that possess three-dimensionally distributed interfaces with adjustable bonding strength in order to modulate the mechanical responses and achieve excellent comprehensive performance.

    However, it is challenging to prepare such materials.A Mo–Cu composite thin film with a bicontinuous structure was fabricated recently by co-sputtering Cu and Mo at different temperatures[18].However, this method is very costly and time consuming.It is more desirable to obtain nanostructured X–Cu in a scalable manner, such as via powder metallurgy, to allow for mass production.In general, powder metallurgy demands a high sintering temperature to ensure effective densification.However, the X–Cu nanostructures cannot survive under high temperature due to the enthalpy of mixing and enthalpy of segregation of the two components [19].Consequently, the size of phases easily becomes coarsened to the submicron or micron scale in sintered composites,even when nanoscale raw powders and a pressure-assisted lowtemperature sintering technique are utilized [20–23].Therefore,obtaining nanostructured X–Cu via powder metallurgy remains extremely challenging.

    In this work, the challenge of fabricating nanostructured X–Cu composites via powder metallurgy has been solved by means of modulated phase separation in a W–Cu model system.A hierarchically nanostructured (HN) W–Cu composite was obtained under the assistance of an intermediary element through sluggish asynchronous phase separation.The HN W–Cu consists of a nanostructured W–Cu matrix and massive intermediary-element-containing nanoparticles that possess the same crystal structure and coherent interface as the W phase.With the aid of first-principles calculations, the formation mechanism of the hierarchical nanostructure is disclosed, and the interfacial energy and bonding strength are analyzed.The composite’s excellent mechanical properties under different loading modes, including uniaxial compression, indentation, and reciprocating sliding, are investigated in detail, along with the mechanisms behind them.

    2.Experiments and modeling

    Bulk HN W–Cu composites were fabricated by two-step ball milling followed by spark plasma sintering(SPS)densification.Aluminum (Al) was used as an intermediary element to adjust the final structure and the properties of the products.First, the W and Al powders were mechanically alloyed by ball milling at 580 r?min-1for 12 h to obtain W–Al solid solution powder.Then, Cu powder was blended with the W–Al powder using a milling speed of 300 r?min-1for an hour.Finally, the bulk composites were fabricated by SPS at 900°C for 5 min with a heating rate of 50°C?min-1and a constant pressure of 100 MPa.The temperature, working time,and pressure of SPS play an essential role in the densification of the composite materials.Those sintering parameters were optimized to obtain the highest relative density of the sintered composites.The Cu and Al contents in the composite were 30% (w/w)and 2.4% (w/w), respectively.For comparison, a W–Cu composite bulk without Al addition was also fabricated by the same route.A more detailed fabrication procedure can be found in our previous work [24].

    Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) were used to characterize the microstructures.Energy dispersive spectroscopy (EDS) maps were acquired via high-angle annular dark-field (HAADF) imaging in an aberrationcorrected scanning transmission electron microscope(STEM).After coming under a reciprocating sliding load, TEM samples for microstructure investigation were prepared using the focus ion beam (FIB) technique.The samples were cut perpendicular to the worn surface along the sliding direction.A high-resolution X-ray photoelectron spectroscopy (XPS, Kratos XSAM 800) was utilized to investigate the chemical state of the worn surface with a pass energy of 30 eV (1 eV = 1.602 × 10-19J).Atom probe tomography(APT) characterizations were performed using a local electrode atom probe LEAP 5000XR.The samples were analyzed at 60 K in laser mode at a pulse repetition rate of 125 kHz, a pulse energy of 30 pJ,and an evaporation detection rate of 0.2%atoms per pulse.

    The hardness was measured by a Vickers hardness tester with a load of 30 kg.The sample for the uniaxial compression test was made into a cylindrical shape with the dimensions of φ6 mm× 9 mm.The strain rate and the maximum compressive stain were set to be 0.005 s-1and 10%,respectively.A reciprocating sliding load was applied to the surface using a tribometer (Lanzhou Zhongke Kaihua Technology Development Co., Ltd., China) with a normal load of 10 N and a sliding speed of 2.5 m?min-1for 30 min.

    First-principles calculations were carried out using the density functional theory(DFT)implemented in the Vienna ab-initio simulation package(VASP)[25,26]with the projector-augmented wave(PAW) potential [27].The generalized gradient approximation(GGA) with the Perdew–Burke–Ernzerhof (PBE) exchangecorrelation functional [28] was employed.A 2 × 2 × 2 supercell for W on its primitive cell was constructed.One or two W atoms were substituted by Cu and Al atoms to investigate the microstructure evolution during phase separation.Representative interfaces with low index planes and possible different stacking sequences of W(110)/Cu(111) were built.The body-centered cubic (bcc) Al structure in the coherent W(110)/Al interface was obtained by replacing W with Al atoms, followed by structural relaxation.The interface energy and separation work were calculated for these interfaces with vacuum layers of 20 ? (1 ? = 10-10m).The cutoff energy was set to 385 eV for the plane wave basis.Monkhorst–Pack [29] k-points samplings of 6 × 6 × 6 and 16 × 16 × 1 were used in the calculation for W supercells and interface models, respectively.For sufficient convergence, the tolerance energy value in the geometry optimization was 1.0 × 10-5eV per atom.The atomic positions were relaxed until all forces were smaller than 0.02 eV??-1.The calculated electron localization function (ELF) was visualized using visualization for electronic and structural analysis (VESTA) code [30].The detailed interface energy and separation work were calculated according to the methods reported in the literature [31,32].

    3.Results

    3.1.Microstructures and elemental analysis

    Fig.1.Morphological characterization of the NC and HN W–Cu composites.(a)Morphology of the NC W–Cu composite at low magnification;(b)HAADF-STEM image at the edge of the NC W;(c)distribution of the W element in the area shown in(b);(d)morphology of the HN W–Cu composite at low magnification;(e)HAADF-STEM image at the edge of the nanostructured W in the HN W–Cu composite; (f) size distribution of the nanoparticles within the W nanograins in the HN W–Cu composite; (g–i) elemental distributions in the area shown in (e).

    Fig.1(a)shows the morphology of the W–Cu composite without the addition of Al.The bright and dark regions are the W and Cu phases, respectively.A nanocrystalline (NC) structure can be observed in the interior of the W phase (Figs.1(b) and (c)) with a grain size of less than 100 nm.The morphology of the HN W–Cu composite at low magnification is shown in Fig.1(d).The sharper contrast inside the W phase suggests a finer heterogeneous microstructure.The magnified microstructure at the edge of the W phase was further characterized using HAADF-STEM (Figs.1(e)–(i)).It was determined that the W phase is composed of W nanograins approximately 100 nm in size and two other phases with a darker appearance.The Cu-rich phase is tens of nanometers in size and is mainly distributed among the W nanograins.The other phase has a much smaller size of less than 10 nm and is homogeneously distributed inside the W nanograins.Unfortunately,it was difficult to identify the composition of these nanoparticles through EDS mapping due to the limited resolution.In order to reveal the microstructure and composition of these nanoparticles, atomresolution HAADF-STEM and three-dimensional (3D) APT characterizations were conducted.

    In the magnified HAADF-STEM image of the HN W–Cu nanostructure (Fig.2(a)), the majority of the dark nanoparticles are dispersed inside the W grains, while the others are located at the W grain boundaries and W/Cu interfaces.The composition of these nanoparticles was determined using a linear elemental scan.Fig.2(b) shows the variation in composition along line 1 in Fig.2(a).The tiny nanoparticles possess reduced W content and a considerable amount of Al.It can also be noticed that the W/Cu interface contains a certain amount of Al.Fig.2(c) shows the variation in composition along line 2 in Fig.2(a).There is no obvious change in the W,Cu,and Al contents across the W grain boundary without nanoparticles,indicating that Al does not segregate at the W/W interfaces.Surprisingly, the atom-resolution HAADF-STEM image (Fig.2(d)) shows that the Al-containing nanoparticle maintains a bcc crystal structure and is completely coherent with the W matrix.

    In order to further investigate the composition of the nanoparticles, the 3D APT technique was carried out.Fig.2(e) shows the compositional reconstruction of a W grain with an Al-containing nanoparticle.The isoconcentration surface of the phase boundary is shown to indicate the position of the Al-containing nanoparticle.The compositional variation across the surface of the W/Alcontaining nanoparticle (Fig.2(f)) shows that the Al atoms dissolved in the W phase are negligible.The concentrations of Al and W change gradually with the depth into the nanoparticle,indicating the formation of a concentration gradient at the phase boundary.The concentration of Al can reach up to 32 atom percent(at%) at the center of the nanoparticle.At the thermodynamically equilibrium state,the W–Al compound with this composition does not exist in the W–Al system.Also, no W–Al compound was detected by the X-ray diffraction (XRD) of the composite bulk in previous studies [24].This indicates that these nanoparticles are a supersaturated solid solution of Al in the W matrix.Moreover,the compositional analysis for the Cu phase (Figs.2(g) and (h))shows that about 15 at% of Al is uniformly dissolved in the Cu phase.

    Fig.2.Detailed analysis of elemental distribution in the composite.(a) Magnified HAADF-STEM image of the W–Cu nanostructure; (b, c) elemental distribution corresponding to (b) line scan 1 and (c) line scan 2 in (a); (d) the bcc Al-containing nanoparticle and its coherent interface with the W matrix (insets are the fast Fourier transform(FFT)patterns corresponding to the regions marked by the circle and square,respectively);(e)APT construction of the W grain with an Al-containing nanoparticle,in which the isoconcentration surface of the phase boundary is shown;(f)atomic concentration variations of Al and W across the surface of the Al-containing nanoparticle;(g, h) APT construction of the Cu–Al solid solution in the W-based nanostructure; (i) schematic diagram of the hierarchical nanostructure of the HN W–Cu composite.

    The above analysis confirmed that the as-prepared W–Cu composite with the addition of Al possesses a hierarchical structure containing three levels of microstructure.The first-level structure is composed of a refined micron-scale W-based phase and Cu phase, which is similar to the traditional fine-structured W–Cu composite.Within the W-based phase, there is a second-level structure containing nanosized W and Cu.The third-level structure comprises Al-containing nanoparticles dispersed in the W nanograin matrix and at the grain boundaries and W/Cu interfaces.Fig.2(i) provides a schematic diagram of the hierarchical microstructure described above.

    The above results indicate that the addition of Al plays an important role in the formation of the hierarchical nanostructure.Fig.3 illustrates the fabrication processes of the NC and HN W–Cu composites.Without Al, the particle size of the W powder is refined during the ball milling, and the NC structure forms inside the W particle.After mixing with Cu powder and subsequent sintering,the NC W–Cu composite bulk is obtained(Fig.3(a)).In contrast,mixing Cu powder with W–Al solid solution powder yields an HN W–Cu composite bulk after sintering (Fig.3(b)), in which a nanosized Cu phase and Al-containing nanoparticles are dispersed in the NC W matrix.The formation and stabilization mechanisms of the HN W–Cu composite will be demonstrated in Section 4.1.

    3.2.Mechanical properties

    The uniaxial compressive stress–strain curve of the HN W–Cu composite at room temperature is shown in Fig.4(a).For comparison, the same test was conducted for a conventional fine-grained W–Cu composite, whose microstructure is shown in Fig.S1 in Appendix A.The compressive strength of the HN W–Cu composite is 1270 MPa,which is approximately 1.7 times higher than that of the fine-grained W–Cu composite (~730 MPa) and 1.2 times as high as that of the NC W–Cu composite (1020 MPa).From these results, it can be determined that the HN W–Cu composite has superior compressive strength in comparison with the finegrained and NC W–Cu composites.In order to reveal the thermal stability of the hierarchical nanostructure, stress–strain curves of the HN W–Cu composite after heat treatments at 900, 1000, and 1100 °C were also measured.After heating at 900 and 1000 °C,the compressive strength of the HN W–Cu composite increased to about 1400 MPa, which may be attributed to the improved relative density after heat treatment.The retention of high compressive strength at elevated temperatures suggests that extending the durations of the sintering and cooling processes will not deteriorate the performance of the composite, demonstrating the high thermal stability of the hierarchical nanostructure.Only when the annealing temperature exceeds 1100 °C does the compressive strength start to decay(e.g.,to ~1100 MPa),which can be attributed to the occurrence of structural coarsening.

    Fig.3.Schematic diagrams showing the fabrication processes and representative microstructures of the NC and HN W–Cu composites.(a) NC W–Cu composite prepared without the addition of Al; (b) HN W–Cu composite prepared with the addition of Al.

    The hardness of W–Cu composites prepared via different methods was also measured (Fig.4(b)) [20,23,33–44].In general, the hardness of coarse-grained W–Cu composites with a W size of tens of micrometers decreased gradually with the increase of Cu content,whose value ranged from 120 to 280 Vickers pyramid number(HV).Hardening strategies for the W–Cu composite can be divided into two categories: refinement of the microstructure and the addition of other components.Although nanosized W–Cu composite powders can be prepared via chemical co-precipitation and mechanical alloying, the coarsening of grains is likely to happen during sintering due to the limited intrinsic thermal instability of the W–Cu nanostructures, leading to submicron-scale phases in the product.Therefore,the hardness of the refined W–Cu composites in the literature has seldom been higher than 400 HV.For example,the hardness of the commercial fine-grained W–Cu composite in the present work was 269 HV30.When additives are employed, the highest hardness of the W–Cu composite can reach 361 HV with the addition of zinc(Zn),due to the formation of rigid Cu–Zn intermetallic compounds [33].Introducing TiN as particle additives enhanced the hardness of a W–Cu composite with a Cu content of 30 weight percent (wt%) to about 220 HV [34].

    Based on the above investigations, it can be concluded that most strategies—whether relying on refining the microstructure or on additives—have limited ability to improve the hardness.In comparison, our strategy of introducing nanostructures in the W phase can effectively improve the hardness of the composite.A hardness of 463 HV30was obtained for the NC W–Cu composite by creating NC grains inside the W phase.Furthermore, an HN W–Cu composite with a Cu content of 30 wt% exhibited a significantly improved hardness of 512 HV.The combination of extraordinary hardness and compressive strength provides the HN W–Cu composite with a record-breaking comprehensive performance compared with all other sintered W–Cu composites with the same Cu content.These excellent mechanical properties can be attributed to the formation of a hierarchical nanostructure with a large number of heterogeneous W/Cu interfaces and W/Alcontaining particle interfaces.

    3.3.Plastic deformation under indentation

    The deformation behavior of composites composed of bcc- and face-centered cubic(fcc)-structured metals has been demonstrated by micro-column compression experiments in a previous study[14].When an indenter pierces into an fcc–bcc metallic composite,the softer fcc phase deforms first and undergoes work hardening as the penetration depth increases.As the onset ability of dislocation in the fcc phase increases to a comparable level to that in the harder bcc phase,slip and plastic deformation of concurrent dislocations occur in both phases.This process produces a typical compressive morphology of the bcc phase with a high length-to-width ratio.Interestingly, when the deformation morphology and microstructure of the HN W–Cu composite under indentation were analyzed, a different feature from the traditional fcc–bcc metallic composite was found.Although the Cu phase had a large degree of plastic deformation and work hardening, the entire W–Cu nanostructure provided a locally rigid skeleton to withstand the increased load without severe deformation (Fig.5(a)), due to the great number of W/Cu interfaces and W/Al-containing particle interfaces,endowing the HN composite with extremely high hardness.The plastic deformation occurred in the softer Cu phase by forming stacking faults (SFs) (Fig.5(b)).

    Fig.4.Mechanical properties of various W–Cu composites.(a) Uniaxial compressive stress–strain curves of the HN and commercial fine-grained W–Cu composites at different temperatures; (b) hardness of various W–Cu composites, including those strengthened by microstructure refinement [20,23,35–38], Cu-distribution homogenization[39],the addition of alloying elements[33,40],and the addition of compounds [34,41–44].LS: liquid sintering; HPS: high-pressure sintering.

    The deformation morphology and microstructure under indentation of the NC W–Cu composite were also investigated.It was found that the deformation features and mechanism of the NC W–Cu composite were similar to those of the traditional W–Cu composite, which showed severe plastic deformation in the W phase (Fig.5(c)).Correspondingly, there was a high density of interlaced edge dislocations in the severely deformed W phase(Fig.5(d)).Concurrent plastic deformation in both phases occurred as the onset ability of dislocation in the Cu phase increased to a comparable level with that in the W phase.Therefore, it can be inferred that the hardening degree of the Cu phase before the concurrent deformation of W and Cu should be greater than that of the traditional W–Cu, due to the more difficult dislocation onset and glide in the NC W.In other words, the simultaneous plastic deformation of the W and Cu phases in the NC W–Cu composite was retarded compared with the deformation in the traditional W–Cu composites without nanostructure inside the W phase.

    In order to compare the resistance against plastic deformation of the W–Cu nanostructure with dispersive nanoparticles with that of the NC W more intuitively,the powder containing NC W and W–Al alloy particles was simultaneously mixed with Cu powders.After sintering, both the W–Cu nanostructure with dispersive nanoparticles and the NC W were obtained in one sample.The higher degree of deformation of the NC W than of the hierarchical nanostructure was verified (Fig.5(e)), evidencing the more pronounced effect of the W/Cu interfaces and W/Al-containing particle interfaces on the blocking dislocation glide in comparison with the W grain boundaries.It can be anticipated that the hardness and strength of the composite can be significantly improved by decreasing the fraction of Cu to enhance the contribution of the hierarchical nanostructure to load bearing.

    3.4.Response to reciprocating sliding

    During practical service, wear resistance is one of the most important factors for the reliability and service life of a W–Cu composite.In our previous work, the morphologies of the worn surfaces of W–Cu composites with and without the addition of Al were compared.Delamination exfoliation with microcracks can be observed on the partially worn surface of the HN W–Cu composite.Such a wear mode differs from that of an NC W–Cu composite prepared via the same procedure without the addition of Al,where the delamination completely covered the worn surface with propagating cracks.Correspondingly, the wear rate of the HN W–Cu composite is less than a third of that of the NC W–Cu composite[24].It is generally agreed that the delamination forming on a worn surface derives from the gradual sticking of broken W particles with ductile Cu.Such a friction-induced transition structure is known as a mechanically mixed layer (MML) [45].As the MML reaches the maximum degree of work hardening by means of continuous severe deformation during the friction process,propagated cracks will appear in the MML and MML/subsurface interface,resulting in exfoliation of the delamination.To further understand the mechanism of wear resistance,the microstructure and composition of the reciprocating sliding-induced transformation film at the worn surface were investigated.

    A cross-section of the wear track along the sliding direction of the NC W–Cu composite is shown in Fig.6(a).With increments in depth,an MML with a thickness of about 2 μm first appears,followed by a severe plastic deformation region (PDR).There are numerous spindle-shaped W phases extending along the wear direction in the MML.A magnified view of the MML (Fig.6(b))shows that most particles are refined to an average size of approximately 7 nm (Fig.6(c)).The selected area electron diffraction(SAED)for the MML reveals that,besides oxides and the W phases,no Cu phase can be detected (Fig.6(d)), which implies that the Cu in the MML was oxidized completely during the friction process.The magnified TEM image(Fig.6(e))indicates that the grains were deformed to a strip shape in the spindle W phase after friction.Plastic deformation becomes difficult inside the refined grains due to the dramatically enhanced critical shear stress for the nucleation and motion of dislocations.It has been found that there is a critical grain size below which grain interiors are largely dislocation-free and contain few dislocation sources [46,47].Therefore, the grain boundaries act as both dislocation sources and sinks.Correspondingly, in our work, when the grain size decreases to 10 nm, the nucleation of dislocations occurs mainly at the boundaries of the strip grains (Fig.6(e)).The as-formed dislocations slip into the strip grains, resulting in continuous refinement.According to the concentration profile of oxygen from the worn surface to the PDR(inset of Fig.6(a)),it is evident that the oxygen concentration in the MML is relatively high and decreases gradually with increments in depth.This finding suggests that the environmental oxygen atoms tend to diffuse through the defects generated by the severe deformation during the reciprocating sliding process,leading to oxidation of the W grains and a change in its shape from a spindle to an equiaxed shape(Fig.6(b)).By characterizing the boundaries of tens of strip grains, it was found that lowangle grain boundaries (with a misorientation angle of less than 10°) are dominant for the strip grains (inset in Fig.6(e) and Figs.6(f)–(i)).These low-angle grain boundaries are generated by the‘‘screening” effect during the prolonged exposure to the slidinginduced heating environment.The large-angle grain boundaries with higher energy tend to migrate and are finally annihilated.

    Fig.5.Deformation morphology and microstructure of the composites under indentation.(a) Deformation morphology of the HN W–Cu composite; (b) deformation SFs in the Cu phase of the HN W–Cu composite;(c)deformation morphology of the NC W–Cu composite;(d)interlaced edge dislocations in the severely deformed W phase of the NC W–Cu composite; (e) deformation morphology of the composite containing both W–Cu nanostructure and NC W.

    Fig.7 shows the microstructure and composition of the worn surface of the HN W–Cu composite.Compared with that of the NC W–Cu composite, the thickness of the MML in the HN W–Cu composite has decreased to about 100 nm (Fig.7(a)).The reduced thickness is attributed to the less broken W particles due to the dragging effect of the Cu in the W–Cu nanostructure,which is confirmed by the morphology of the worn surfaces (Fig.S2 in Appendix A).Moreover, the HN W–Cu composite has a restricted PDR because of the strong resistance of the W–Cu nanostructure with dispersive nanoparticles against plastic deformation.Furthermore,SAED of the MML reveals that, in addition to oxide and W phases,the Cu phase can be detected after the reciprocating sliding load.A more detailed microstructure of the MML indicates that the W–Cu nanostructures are crushed into separated fine particles(Fig.7(b))rather than being sheared directly into strip grains as observed in other W–Cu composites (Fig.6(e)), due to the difficult nucleation and propagation of the dislocations.Furthermore, a large number of nanoparticles in the MML exhibit a deformation streamline in shape and have a large longitudinal-to-transverse ratio (~3), as shown in Fig.7(d).

    The composition distribution in the yellow box in Fig.7(b)shows that there are still numerous Cu-rich areas in the MML(Fig.7(c)), which is consistent with the SAED result (inset in Fig.7(a)).The composition in the MML was further determined by XPS.The peaks of metallic W 4f can be deconvoluted into three peaks: namely, W, Wx+, and W6+[48].Their binding energies are located at 31.1, 31.7, and 35.1 eV, respectively (Fig.7(e)).There is also a series of W oxides, such as WOx, WO3, and CuWO4, on the worn surface.The peaks of Al 2p located at 74.5 and 77.1 eV(Fig.7(f)) can be attributed to Al2O3and CuAl2O4, respectively[49,50].The maintenance of the Cu component in the MML of the HN W–Cu composite is associated with the formation of Al oxides,which acts as a barrier to prevent the further diffusion of oxygen.In addition,the remaining Cu component helps to improve the toughness of the MML and prevent nucleation and the propagation of cracks.Therefore,only microcracks form on the worn surface of the HN W–Cu composite,rather than the propagating cracks found in the NC W–Cu composite (Fig.S2).The different microstructure and composition also induce variation in the mechanical properties of the MML.Nanoindentation tests were performed to evaluate the mechanical properties of the MMLs(Fig.S3 in Appendix A).Under a controlled load of 30 mN,the hardness of the MMLs in the NC W–Cu and HN W–Cu composites is 5.6 and 9.7 GPa, respectively.Therefore, the excellent wear resistance of the HN W–Cu composite can be attributed to the formation of a protective film with excellent combined rigidity and toughness under a reciprocating sliding load.

    4.Discussion

    4.1.Formation of a hierarchical structure

    After adding Al into the W–Cu composite, a W–Cu nanostructure was formed even after high-temperature sintering.From a thermodynamic viewpoint, the W–Cu nanostructure should coarsen severely at such a temperature,especially when it is composed of a nanocomposite powder with high activity fabricated by means of mechanical alloying.In addition,Al-containing nanoparticles are produced within the W nanograins.The existing state of the Al in the W matrix is different from those of the titanium(Ti)and chromium (Cr) that have been reported as stabilizers for a W nanostructure [51,52].In those systems, the NC W was stabilized by the formation of a segregation film and nanoparticles with a diameter of tens of nanometers at the W grain boundaries.

    To explain the stability of the W–Cu nanostructure and the distribution of the Al in the HN W–Cu composite,the formation energies of the Cu and Al dissolved in the W matrix were calculated to evaluate the driving force of their phase-separation process(Fig.8).As for the W–Cu system, it is generally regarded that a positive energy indicates that it is difficult for a solid solution to form in the thermodynamic equilibrium state.As a result, when Cu dissolves into W through nonequilibrium methods,such as mechanical alloying, rapid phase separation should occur during subsequent heat treatment and sintering,leading to the formation of coarse-structured W and Cu.In our work, the calculated formation energy of the W–6.25 at%Cu solid solution is 1.80 eV,which is consistent with the immiscible nature of W and Cu.When the Cu concentration increases to 12.5 at%,the formation energy increases greatly to 3.03 eV.This high formation energy suggests that the Cu atoms have a strong tendency to separate from the W matrix.When a certain amount of Al is dissolved in the W–Cu system,the formation energy greatly decreases from 3.03 to 1.61 eV.In other words,the presence of the Al atom promotes the dissolution of Cu in W in the nonequilibrium state and significantly reduces the phase-separation tendency of the W–Cu system.

    Compared with the positive mixing enthalpy of the W–Cu system (36 kJ?mol-1) [53], the Cu–Al system has a negative mixing enthalpy of-1 kJ?mol-1[54].Therefore,it is easy for Cu–Al to form a solid solution or even intermetallic compounds at room temperature.Furthermore, the negative mixing enthalpy suggests a stronger atomic bond between Cu and Al than between Cu and W.Under constant temperature, the diffusion rate is inversely related to the activation energy based on the Arrhenius equation.When the Cu phase is excluded from the Al-containing W phase, the diffusion of Cu atoms must consume more energy to break the bonds with surrounding atoms.Therefore, Al effectively reduces the diffusion rate of Cu atoms in the W phase.Thus, the separation between Cu and W can be alleviated by Al in both thermodynamic and dynamic aspects, which explains the high stability of the W–Cu nanostructure.

    The formation energy of a W–6.25 at%Al solid solution was calculated to be 0.24 eV, which indicates that W and Al are also immiscible and tend to form individual phases at this concentration.However,compared with the W doped with the same concentration of Cu, the reduced formation energy indicates a lower tendency for the phase separation of a W–Al solid solution.To further investigate the phase-separation behavior of Al in W, the formation energy of a W–Al solid solution with different distances between Al atoms was calculated.The formation energy decreases by 1.08 eV(from 1.49 to 0.41 eV)when the distance between the Al atoms decreases, which implies that Al aggregation is preferable.Once sufficient energy fluctuation is provided during sintering,the formation of Al clusters in the W grains should be facilitated.To sum up,the modulated asynchronous phase-separation process among the W,Cu,and Al atoms and the‘‘self-segregation”trend of the Al atoms result in the formation of a hierarchical nanostructure.

    Fig.7.Microstructure and composition of the transformation film in the HN W–Cu composite under a reciprocating sliding load.(a)Cross-section of the worn surface under low magnification(inset shows the SAED pattern in the MML region);(b)microstructure of the MML at higher magnification;(c)elemental distribution corresponding to the boxed region in (b); (d) longitudinal and transverse size distributions of the nanoparticles in the MML; (e, f) XPS spectra of W and Al in the worn surface.

    Fig.8.Calculated formation energies(Ef)of dissolving Cu and Al into W at different concentrations and atomic configurations.

    4.2.Interface energy and bonding state

    The HN W–Cu composite possesses a great number of W/Cu and coherent W/bcc Al-containing particle interfaces.The intrinsic energy and bonding strength of these interfaces were evaluated through first-principles calculation(Figs.9 and 10).First,two representative combinations of W(110)/Cu(111) interfaces with different stacking sequences were constructed and denoted as W/Cu IF 1 and W/Cu IF 2 (Figs.9(a) and (b)).The relative orientation of(110)bcc/(111)fccis based on experimental observations and reported models in the literature [55–57].In order to disclose the intrinsic properties of the studied interfaces on an atomic scale,flat interfaces were used in the calculations.Compared with W/Cu IF 2(2.27 J?m-2), W/Cu IF 1, which has a lower interface energy(2.07 J?m-2), was chosen for the further doping of Al atoms.The calculated W/Cu interface energy is consistent with that reported in the literature [56].The Al atoms were doped in the Cu phase at three sites with different distances from the interface(Fig.9(a)).The interface has the lowest energy (1.09 J?m-2) and the highest separation work (4.83 J?m-2) when the substitution site is close to the interface(Fig.10),suggesting the localized effect of Al on the interface properties.The reduced interface energy also demonstrates an enhanced stability of the W/Cu interface by Al modulation.Moreover, numerous bcc Al-containing nanoparticles were observed dispersing inside the W grains, which implies that the W/bcc Al interface may have low energy.In order to confirm this supposition, the energy of a coherent W/bcc Al interface was also calculated.A low energy of 0.67 J?m-2was obtained, which is even lower than that of the W/Cu interface modulated by Al.This finding of a lower interface energy facilitates our understanding of the formation of bcc Al-containing nanoparticles by precipitation from the W matrix.

    The electron transfer at different interfaces was also investigated (Fig.11(a)).There is negligible electron transfer at the W/Cu interface, which is consistent with the weak bonding strength between immiscible components.However, the W and Cu atoms at the Al-doped W/Cu interface respectively gain 0.58 and 0.43 electrons from the Al atom.At the W/bcc Al interface,the W atoms gain 0.60 electrons from the surrounding Al atoms.Fig.11(b)shows the distribution of the ELF at different interfaces.The ELF is dimensionless and ranges from 0 to 1, reflecting the electron localization with respect to a uniform electron gas.A value of 1 corresponds to the perfect localization, while a value of 0 refers to absolute delocalization.In the present work,the ELF at a pristine W/Cu interface spans 0.3–0.4, indicating little evident electronic interaction.As for the W/Cu interface with doped Al and W/bcc Al connection,the ELF increases to about 0.6,suggesting improved electron localization.The local electronic density of state (LDOS)indicates that, at the W/Cu interface with doped Al—unlike the weak interaction of electrons at the pristine W/Cu interface(Fig.11(c))—the p-orbital electrons of the Al atoms strongly couple with the d-orbital electrons of Cu and W at peaks of-4 and-2 eV,respectively (Fig.11(d)).In other words, as a proper intermediary,the Al atoms interact with both Cu and W to stabilize and improve the bonding of the W/Cu interface.At the W/bcc Al interfaces, the p-orbital electrons of Al and the d-orbital electrons of W exhibit the same peak positions at-3 and-1 eV,revealing strong coupling(Fig.11(e)).

    4.3.The integrated strengthening effects of hierarchical structure and interfacial geometry

    The stress applied to the W/Cu interface can be decomposed into two components.The component along the interface may promote interface sliding, while the component perpendicular to the interface may cause dislocation slip and, hence, plastic deformation in the W and Cu phases.In the traditional coarse-grained(e.g., a W grain size larger than 10 μm) and fine-grained (e.g., a W grain size of a few microns) W–Cu composites, the W/Cu interfaces are basically smooth and locally flat, with a small curvature.It is easy for such W/Cu interfaces to slide due to the weak bonding strength [57–59].In the W and Cu phases, without any precipitation or solute solution atoms,there are few obstacles hindering the motion of dislocations; thus, considerable deformation results, as has been observed in previous studies [60].Therefore,effectively blocking dislocation slip and W/Cu interfacial sliding is crucial for improving the hardness and strength of the composite.

    Fig.11.Electronic analysis at different interfaces.(a)Electron transfer at various interfaces;(b)distribution of ELF;(c–e)LDOS of Cu,W,and Al atoms at(c)the pristine W/Cu interface, (d) the W/Cu interface with doped Al, and (e) the W/bcc Al interface.

    In the HN W–Cu composite,the numerous W/Cu and W/bcc Alcontaining particle interfaces effectively hinder the slip of dislocations.The motion of dislocations may occur at the interface and within the grain.When gliding along an interface, dislocations must move a longer distance over a rough interface than over a flat one.When crossing an interface, the dislocations encounter more obstacles at the interpenetrated interfaces in the HN composite than at the traditional counterparts.Inside the W grains, the motion of dislocations is hindered by the Al-containing nanoparticles,and dislocation slip may even be pinned by the nanoparticles.

    Aside from the blocked dislocation motion, interface sliding in the HN W–Cu composite is also restricted.After the insertion of the Al,the W/Cu interfaces have a lower energy and higher separation work than the pristine interfaces.This increases the interface’s intrinsic resistance to sliding.Moreover,the interpenetration of the W/Cu interfaces with a curved geometry plays a special role in‘‘self-locking”the interfaces,which inhibits effective interface sliding.That is, the rough, interpenetrating interfaces require more energy to be pulled apart than a flat interface would require [61].When the interfacial area increases to a certain extent,the strength of pulling out a single protrusion in the rough interface exceeds the yield strength of the single protrusion itself,resulting in protrusion deformation prior to interface separation.Under this particular condition, the additional force required to separate the interface is equal to the yield strength of the protrusion.In this case,the critical length in the depth direction lc(at which the separation force is equal to the yield strength) of the protrusion can be expressed as lc= aσ/(4τ), where τ is the sliding resistance between W and Cu,and σ and a are the yield strength and diameter of a cylindrical protrusion, respectively, which is set as a simplified model.Since the yield strength of W is much higher than that of Cu, yielding always occurs in the Cu protrusion.In addition, the yield strength of Cu depends on the diameter of the Cu protrusion [62].In this case, τ is set to be 300–550 MPa [63] and a is defined as 40 nm,according to our experiment.Thus, the lcof the protrusion is around 35–63 nm.Beyond such sizes,the yielding of the Cu protrusion dominates the resistance against interface sliding.The above analysis is verified by experimental observations.In the NC W–Cu composite, the broken surface of the W phase is smooth(Fig.S4(a) in Appendix A), while numerous Cu tearing ridges are observed at the fracture surface of the HN W–Cu composite(Fig.S4(b) in Appendix A).These different fracture morphologies indicate that the bonding strength of many interface regions in the HN W–Cu composite is higher than the yield or fracture strength of the Cu phase.Thus, interface sliding is effectively restricted in the HN W–Cu composite.

    5.Conclusions

    In this work, an HN W–Cu composite was fabricated by taking advantage of modulating the phase-separation process.The formation principle,mechanical behavior,and related mechanisms were demonstrated.The main conclusions are as follows:

    (1)The difficulty of preparing bulk nanostructured W–Cu composite materials by sintering was solved by modulating the phaseseparation process using an intermediary Al.A hierarchical structure composed of a W–Cu nanostructure and bcc Al-containing nanoprecipitates was produced.The formation of this unique structure resulted from asynchronous phase separation.This methodology is applicable to structural modulations for various bimetallic composites containing immiscible components.

    (2) The hardness and compressive strength of the HN W–Cu composite were measured as 512 HV and 1270 MPa at room temperature, respectively.This comprehensive performance is the highest among all reported sintered W–Cu composites with the same Cu content.The high thermal stability of the hierarchical nanostructure enables the composite to maintain a high compressive strength of about 1400 MPa even after 1000°C treatment.This demonstrates the essential contribution made by the nanostructured rigid skeleton to the superior mechanical performance.

    (3) Compared with a pristine W/Cu interface, the W/Cu interfaces modulated by Al and coherent W/Al-containing particle interfaces in the HN composite possess a lower interface energy and enhanced bonding strength.The interface modulation relies on the electron transfer and strong coupling interaction of the p-orbital electrons of Al with the d-orbital electrons of Cu and W.The interpenetrating geometry effectively hinders the slip of the interfaces.This substantial restriction of dislocation slip and interface sliding contributes to the high level of hardness and strength.

    (4) Under a reciprocating sliding load, the surfaces of the NC and HN W–Cu composites exhibit different transformation behaviors in terms of their microstructure and composition.The W phase is sheared into strips and the Cu is completely oxidized at the surface of the NC composite.In contrast, at the surface of the HN composite, the W–Cu nanostructure is crushed into fine particles due to its high resistance to plastic deformation.Moreover, the highly reactive Al prevents the oxidation of other components.Thus,the surface of the HN W–Cu composite exhibits much higher friction resistance than the surface of the NC W–Cu composite.

    Acknowledgments

    This work was supported by the National Natural Science Foundation of China (51621003, 52101003, 92163107, and 52101032),the National Key Research and Development Program of China(2021YFB3501502), and the International Cooperation Seed Fund of Beijing University of Technology (2021B26).

    Compliance with ethics guidelines

    Chao Hou,Hao Lu,Zhi Zhao,Xintao Huang,Tielong Han,Junhua Luan,Zengbao Jiao,Xiaoyan Song,and Zuoren Nie declare that they have no conflict of interest or financial conflicts to disclose.

    Appendix A.Supplementary data

    Supplementary data to this article can be found online at https://doi.org/10.1016/j.eng.2022.09.017.

    日日撸夜夜添| 亚洲欧美精品自产自拍| 亚洲成人中文字幕在线播放| 舔av片在线| 国产成人免费无遮挡视频| 久久久色成人| 国产一级毛片在线| 亚洲丝袜综合中文字幕| 免费观看av网站的网址| 亚洲天堂av无毛| 男人舔奶头视频| 国产欧美另类精品又又久久亚洲欧美| 一级毛片电影观看| 五月天丁香电影| 国产 一区 欧美 日韩| 伦理电影大哥的女人| 国产精品福利在线免费观看| 国产精品精品国产色婷婷| av不卡在线播放| 久久久久久久久久久丰满| 伊人久久精品亚洲午夜| 精品久久久久久久久亚洲| 免费大片18禁| 性色av一级| 亚洲精华国产精华液的使用体验| 日日啪夜夜撸| 久久久久人妻精品一区果冻| 一级黄片播放器| 人妻 亚洲 视频| 高清黄色对白视频在线免费看 | 少妇裸体淫交视频免费看高清| 国产成人aa在线观看| 又爽又黄a免费视频| 久久久久国产网址| 26uuu在线亚洲综合色| 午夜免费鲁丝| 欧美 日韩 精品 国产| 伦精品一区二区三区| 国产黄色免费在线视频| 亚洲欧洲日产国产| 51国产日韩欧美| 秋霞伦理黄片| 欧美精品人与动牲交sv欧美| 国产精品欧美亚洲77777| 国产精品久久久久久精品电影小说 | 免费少妇av软件| 精品国产一区二区三区久久久樱花 | av在线播放精品| 亚洲成人一二三区av| 欧美日本视频| 久久国产乱子免费精品| 国产av国产精品国产| 国产无遮挡羞羞视频在线观看| 亚洲精品一二三| freevideosex欧美| 天堂8中文在线网| 韩国高清视频一区二区三区| 欧美+日韩+精品| 街头女战士在线观看网站| 中国国产av一级| 97精品久久久久久久久久精品| 午夜免费观看性视频| 国产高潮美女av| 一级片'在线观看视频| 久久久色成人| 99久久精品一区二区三区| 日韩欧美 国产精品| 久久久国产一区二区| 国产精品嫩草影院av在线观看| 国产一区有黄有色的免费视频| 国产精品久久久久久久电影| 2018国产大陆天天弄谢| 午夜激情福利司机影院| 麻豆成人av视频| 国产精品福利在线免费观看| 久久6这里有精品| 日本黄色片子视频| 中国美白少妇内射xxxbb| 国产男女超爽视频在线观看| 亚州av有码| av不卡在线播放| 精品一区二区三卡| 日本免费在线观看一区| 亚洲天堂av无毛| 久久97久久精品| 成年av动漫网址| 免费av不卡在线播放| 精品久久久久久电影网| 久久久色成人| 久久亚洲国产成人精品v| 在线观看免费日韩欧美大片 | 日本猛色少妇xxxxx猛交久久| 亚洲欧美中文字幕日韩二区| 国产成人午夜福利电影在线观看| 日本午夜av视频| 啦啦啦视频在线资源免费观看| 欧美高清性xxxxhd video| 国产黄片美女视频| 日韩中文字幕视频在线看片 | 一区在线观看完整版| 久久97久久精品| 老熟女久久久| 91狼人影院| 肉色欧美久久久久久久蜜桃| 国产精品不卡视频一区二区| 青春草亚洲视频在线观看| 视频区图区小说| 最近最新中文字幕免费大全7| 日韩av免费高清视频| 美女福利国产在线 | 精品亚洲成a人片在线观看 | 精品一区二区免费观看| 舔av片在线| 亚洲四区av| 熟妇人妻不卡中文字幕| 亚洲性久久影院| 成人毛片60女人毛片免费| 成人国产麻豆网| 人人妻人人添人人爽欧美一区卜 | 免费看不卡的av| 永久网站在线| 九九久久精品国产亚洲av麻豆| 久久ye,这里只有精品| 成年人午夜在线观看视频| 久久久久久人妻| 一级爰片在线观看| 免费人成在线观看视频色| 日韩视频在线欧美| 欧美激情极品国产一区二区三区 | 蜜臀久久99精品久久宅男| 色婷婷av一区二区三区视频| 黑人高潮一二区| 观看美女的网站| 久久久久网色| 韩国av在线不卡| 97在线人人人人妻| 99re6热这里在线精品视频| 伊人久久精品亚洲午夜| 人妻夜夜爽99麻豆av| 五月伊人婷婷丁香| 自拍欧美九色日韩亚洲蝌蚪91 | 最近中文字幕高清免费大全6| 黄色视频在线播放观看不卡| 中文字幕人妻熟人妻熟丝袜美| 十八禁网站网址无遮挡 | 国内揄拍国产精品人妻在线| 成人特级av手机在线观看| 春色校园在线视频观看| 亚洲成人一二三区av| 亚洲av中文字字幕乱码综合| 亚洲国产精品999| 国产黄色免费在线视频| av一本久久久久| 国产视频内射| 久久久精品免费免费高清| 亚洲激情五月婷婷啪啪| 免费大片18禁| 男人狂女人下面高潮的视频| 久久久久国产网址| 久久精品久久久久久噜噜老黄| 国产精品一区二区在线不卡| 国产黄片视频在线免费观看| 性色av一级| 色5月婷婷丁香| 欧美xxⅹ黑人| 一级毛片 在线播放| 王馨瑶露胸无遮挡在线观看| 91精品国产九色| 熟女av电影| 男女边摸边吃奶| 国产精品免费大片| 午夜福利影视在线免费观看| 极品教师在线视频| 日韩在线高清观看一区二区三区| 欧美+日韩+精品| 国产乱人视频| 亚州av有码| 观看美女的网站| a 毛片基地| 免费黄频网站在线观看国产| 亚洲在久久综合| 国产女主播在线喷水免费视频网站| 日韩制服骚丝袜av| 观看美女的网站| av卡一久久| 美女高潮的动态| 国产午夜精品一二区理论片| 国产精品.久久久| 国产高清不卡午夜福利| 我的老师免费观看完整版| 在线观看一区二区三区| 在线观看国产h片| 久久久色成人| 免费黄网站久久成人精品| 日韩在线高清观看一区二区三区| 国产免费一级a男人的天堂| 国产一区二区三区av在线| 国产国拍精品亚洲av在线观看| 国产免费一区二区三区四区乱码| 国产老妇伦熟女老妇高清| 久久精品国产亚洲av天美| 国产成人freesex在线| 我的老师免费观看完整版| 一级毛片 在线播放| 91精品伊人久久大香线蕉| 99热全是精品| 国产精品麻豆人妻色哟哟久久| 国产精品国产av在线观看| 亚洲电影在线观看av| 少妇人妻 视频| 偷拍熟女少妇极品色| 色婷婷久久久亚洲欧美| 国产大屁股一区二区在线视频| 日本黄色日本黄色录像| 男的添女的下面高潮视频| 亚洲精品乱久久久久久| 国产免费一区二区三区四区乱码| 99热6这里只有精品| 联通29元200g的流量卡| 你懂的网址亚洲精品在线观看| 亚洲真实伦在线观看| 男女边吃奶边做爰视频| 老司机影院成人| 极品少妇高潮喷水抽搐| 少妇人妻精品综合一区二区| 日本欧美视频一区| 三级国产精品欧美在线观看| 久久人人爽人人爽人人片va| 天美传媒精品一区二区| 中文字幕制服av| 亚洲色图av天堂| 国产精品秋霞免费鲁丝片| 天美传媒精品一区二区| 成人二区视频| 免费少妇av软件| 熟女电影av网| 亚洲欧美精品专区久久| 精品一区二区免费观看| 色哟哟·www| 婷婷色综合www| 国产成人精品一,二区| 成人毛片a级毛片在线播放| 亚洲内射少妇av| 秋霞在线观看毛片| 91狼人影院| av国产免费在线观看| 一二三四中文在线观看免费高清| 亚洲精品乱码久久久v下载方式| 夫妻性生交免费视频一级片| 亚洲国产精品专区欧美| 免费观看无遮挡的男女| 免费在线观看成人毛片| 午夜免费男女啪啪视频观看| 人妻夜夜爽99麻豆av| xxx大片免费视频| 国产精品久久久久久精品电影小说 | 黄色欧美视频在线观看| 亚洲欧美一区二区三区黑人 | 久久鲁丝午夜福利片| 亚洲av国产av综合av卡| 国产高清国产精品国产三级 | 国产爱豆传媒在线观看| 国产精品人妻久久久影院| 99久国产av精品国产电影| 久久久久久久亚洲中文字幕| 欧美日韩综合久久久久久| 搡女人真爽免费视频火全软件| 久久 成人 亚洲| 高清毛片免费看| 91狼人影院| 少妇人妻一区二区三区视频| 嫩草影院新地址| 成年免费大片在线观看| 91狼人影院| 3wmmmm亚洲av在线观看| 久久韩国三级中文字幕| 亚洲精品456在线播放app| 99re6热这里在线精品视频| av国产免费在线观看| 日韩成人av中文字幕在线观看| a级毛色黄片| 一级毛片aaaaaa免费看小| 久久久亚洲精品成人影院| 日韩强制内射视频| 乱系列少妇在线播放| 黄色欧美视频在线观看| 亚洲av欧美aⅴ国产| 久久ye,这里只有精品| 国产精品一区www在线观看| 赤兔流量卡办理| 亚洲精品,欧美精品| 国产精品精品国产色婷婷| 欧美丝袜亚洲另类| 欧美97在线视频| 亚洲一区二区三区欧美精品| av又黄又爽大尺度在线免费看| 成年人午夜在线观看视频| 国产午夜精品一二区理论片| 久久久亚洲精品成人影院| 我要看日韩黄色一级片| 免费看av在线观看网站| 看十八女毛片水多多多| 少妇人妻 视频| 亚洲国产色片| 中文资源天堂在线| av免费观看日本| 中文字幕精品免费在线观看视频 | 亚洲av欧美aⅴ国产| 黄色怎么调成土黄色| 精品人妻一区二区三区麻豆| 在线观看av片永久免费下载| 亚洲欧美日韩卡通动漫| 国产精品麻豆人妻色哟哟久久| 边亲边吃奶的免费视频| 嫩草影院新地址| 直男gayav资源| av在线蜜桃| 我要看日韩黄色一级片| 国产亚洲一区二区精品| 亚洲精华国产精华液的使用体验| 天堂中文最新版在线下载| 久久综合国产亚洲精品| tube8黄色片| 亚洲欧美精品专区久久| 18禁裸乳无遮挡免费网站照片| 国产午夜精品一二区理论片| 九九久久精品国产亚洲av麻豆| 亚洲精品国产av成人精品| 秋霞伦理黄片| 精品人妻视频免费看| 一区二区三区免费毛片| 成年女人在线观看亚洲视频| 亚洲欧美精品专区久久| 欧美国产精品一级二级三级 | 国产精品久久久久久精品古装| 人人妻人人爽人人添夜夜欢视频 | 肉色欧美久久久久久久蜜桃| 亚洲国产欧美在线一区| 狂野欧美白嫩少妇大欣赏| 伊人久久精品亚洲午夜| av免费在线看不卡| 一本一本综合久久| kizo精华| 亚洲欧美成人综合另类久久久| 美女cb高潮喷水在线观看| 免费少妇av软件| 久久久午夜欧美精品| 男男h啪啪无遮挡| 日日啪夜夜爽| 成人毛片a级毛片在线播放| 天美传媒精品一区二区| 一区二区三区精品91| 免费大片18禁| 欧美成人午夜免费资源| 纵有疾风起免费观看全集完整版| 国产一区亚洲一区在线观看| a 毛片基地| 蜜桃在线观看..| 精品一区二区免费观看| 99热6这里只有精品| 蜜桃在线观看..| 亚洲欧美日韩另类电影网站 | 99视频精品全部免费 在线| 伦理电影免费视频| 中文字幕制服av| 亚洲国产高清在线一区二区三| 美女xxoo啪啪120秒动态图| 国产黄频视频在线观看| 亚洲精品日韩av片在线观看| 啦啦啦中文免费视频观看日本| 欧美xxxx性猛交bbbb| 亚洲中文av在线| 搡女人真爽免费视频火全软件| 中文乱码字字幕精品一区二区三区| 亚洲久久久国产精品| 日韩三级伦理在线观看| 亚洲av免费高清在线观看| 欧美老熟妇乱子伦牲交| 日日撸夜夜添| 天堂俺去俺来也www色官网| 麻豆成人av视频| 十分钟在线观看高清视频www | 国产精品国产三级国产av玫瑰| 99热这里只有是精品在线观看| 亚洲成色77777| 国产成人精品婷婷| 男人狂女人下面高潮的视频| 亚洲国产高清在线一区二区三| 99九九线精品视频在线观看视频| 99久久人妻综合| 国产免费福利视频在线观看| 我要看日韩黄色一级片| 国产日韩欧美亚洲二区| 亚洲av国产av综合av卡| 久久6这里有精品| 欧美97在线视频| 少妇丰满av| av女优亚洲男人天堂| 91狼人影院| 日韩三级伦理在线观看| 免费看av在线观看网站| 大话2 男鬼变身卡| 国产高清国产精品国产三级 | 精品国产乱码久久久久久小说| 99久国产av精品国产电影| 日日摸夜夜添夜夜添av毛片| 国产精品一及| 国产精品国产三级国产专区5o| 女性生殖器流出的白浆| 自拍欧美九色日韩亚洲蝌蚪91 | 亚洲图色成人| 男女免费视频国产| 久久久久久久精品精品| 久久婷婷青草| 亚洲伊人久久精品综合| 午夜激情福利司机影院| 网址你懂的国产日韩在线| 免费久久久久久久精品成人欧美视频 | 高清日韩中文字幕在线| 久久精品久久久久久久性| 老司机影院毛片| 日韩强制内射视频| 国产 一区 欧美 日韩| 亚洲天堂av无毛| 99热全是精品| 成人亚洲欧美一区二区av| 我要看日韩黄色一级片| 又黄又爽又刺激的免费视频.| 免费观看a级毛片全部| 最近2019中文字幕mv第一页| 精品酒店卫生间| 激情 狠狠 欧美| 高清毛片免费看| 亚洲天堂av无毛| 国产69精品久久久久777片| 人妻夜夜爽99麻豆av| 成人漫画全彩无遮挡| 国产日韩欧美在线精品| 免费播放大片免费观看视频在线观看| 久久精品夜色国产| 夜夜看夜夜爽夜夜摸| 日本猛色少妇xxxxx猛交久久| 欧美极品一区二区三区四区| 男人舔奶头视频| 五月天丁香电影| 欧美最新免费一区二区三区| 一级毛片电影观看| av线在线观看网站| 国产午夜精品久久久久久一区二区三区| 老司机影院成人| av福利片在线观看| 成人影院久久| 夜夜爽夜夜爽视频| 亚洲国产精品专区欧美| 免费看日本二区| 亚洲精品久久久久久婷婷小说| 亚洲成人手机| 亚洲在久久综合| 狂野欧美激情性xxxx在线观看| 最近最新中文字幕大全电影3| 久久久成人免费电影| 国产乱来视频区| 亚洲精品乱码久久久久久按摩| 最近手机中文字幕大全| 人人妻人人澡人人爽人人夜夜| 中文字幕精品免费在线观看视频 | 最新中文字幕久久久久| a级毛色黄片| 国产av精品麻豆| 91在线精品国自产拍蜜月| 另类亚洲欧美激情| 爱豆传媒免费全集在线观看| 亚洲精品国产av成人精品| 熟女av电影| 18禁裸乳无遮挡动漫免费视频| 高清毛片免费看| 久久99热这里只有精品18| av黄色大香蕉| 搡女人真爽免费视频火全软件| 精品一区二区三区视频在线| 黄色日韩在线| 久久99热这里只频精品6学生| 国产一区有黄有色的免费视频| 欧美bdsm另类| 久热这里只有精品99| 中文乱码字字幕精品一区二区三区| 麻豆成人av视频| 97在线视频观看| 男人添女人高潮全过程视频| 亚洲一级一片aⅴ在线观看| av线在线观看网站| av在线观看视频网站免费| 欧美xxxx性猛交bbbb| 在线观看免费日韩欧美大片 | 中国三级夫妇交换| 99久久人妻综合| 26uuu在线亚洲综合色| 免费在线观看成人毛片| 纵有疾风起免费观看全集完整版| 最后的刺客免费高清国语| 亚洲色图av天堂| 亚洲,一卡二卡三卡| 成人午夜精彩视频在线观看| 亚洲自偷自拍三级| 观看免费一级毛片| 少妇人妻久久综合中文| 九九爱精品视频在线观看| 在线观看免费日韩欧美大片 | 欧美日韩精品成人综合77777| 狂野欧美白嫩少妇大欣赏| av在线蜜桃| 2021少妇久久久久久久久久久| 熟女电影av网| 一区二区三区免费毛片| 成人亚洲精品一区在线观看 | 欧美丝袜亚洲另类| 午夜日本视频在线| 亚洲欧美一区二区三区国产| 插逼视频在线观看| videossex国产| 国产男女超爽视频在线观看| 六月丁香七月| .国产精品久久| 亚洲欧美日韩卡通动漫| 欧美人与善性xxx| 欧美日韩视频高清一区二区三区二| 在线播放无遮挡| 国产精品一区二区在线不卡| 成人综合一区亚洲| xxx大片免费视频| 黄色欧美视频在线观看| 在线观看三级黄色| 国产高清三级在线| 99久久中文字幕三级久久日本| 国产91av在线免费观看| 美女主播在线视频| 欧美极品一区二区三区四区| 日韩中字成人| 欧美成人午夜免费资源| 免费观看a级毛片全部| 一级av片app| 欧美日韩视频精品一区| 国产精品伦人一区二区| 91aial.com中文字幕在线观看| 国产视频内射| 久久99精品国语久久久| 91精品国产九色| www.色视频.com| 在线播放无遮挡| 夜夜骑夜夜射夜夜干| 两个人的视频大全免费| 亚洲国产精品成人久久小说| 边亲边吃奶的免费视频| 精品人妻熟女av久视频| 日韩av不卡免费在线播放| 少妇 在线观看| 欧美精品一区二区大全| 国产 精品1| 男女啪啪激烈高潮av片| 久久人人爽人人片av| 久久99精品国语久久久| 少妇人妻精品综合一区二区| 亚洲激情五月婷婷啪啪| 韩国av在线不卡| 午夜日本视频在线| 天堂俺去俺来也www色官网| 黄片无遮挡物在线观看| 成年免费大片在线观看| 黄片无遮挡物在线观看| 中文字幕制服av| www.色视频.com| 国产高清三级在线| 大片电影免费在线观看免费| 免费少妇av软件| 有码 亚洲区| 免费看不卡的av| 国产精品女同一区二区软件| 日韩,欧美,国产一区二区三区| 国产精品久久久久久av不卡| 色5月婷婷丁香| 国产成人免费无遮挡视频| 欧美日韩综合久久久久久| 免费看av在线观看网站| 亚洲国产av新网站| 日本欧美视频一区| 欧美国产精品一级二级三级 | 久久久久久久久久成人| 亚洲色图综合在线观看| 国产白丝娇喘喷水9色精品| 女人十人毛片免费观看3o分钟| 亚洲av二区三区四区| 插阴视频在线观看视频| 寂寞人妻少妇视频99o| 欧美精品亚洲一区二区| 亚洲精品视频女| 久久精品国产亚洲网站| 亚洲美女黄色视频免费看| 蜜桃久久精品国产亚洲av| 26uuu在线亚洲综合色| 久久久久久久久久久丰满| 各种免费的搞黄视频| 久久久久久久久久久丰满| 观看av在线不卡| 亚洲精品国产av蜜桃| 在线观看一区二区三区| 观看免费一级毛片| 国产综合精华液| 你懂的网址亚洲精品在线观看| 国产黄色视频一区二区在线观看| av在线观看视频网站免费| 久久精品夜色国产| 三级国产精品欧美在线观看| 亚洲va在线va天堂va国产| 寂寞人妻少妇视频99o| av女优亚洲男人天堂|