    Effect of Broaching Machining Parameters on Low Cycle Fatigue Life of Ni-Based Powder Metallurgy Superalloy at 650 ℃

    2023-11-22 09:11:20,,,,,,3*

    ,,,,,,3*

    1.Key Laboratory of Aero-engine Thermal Environment and Structure, Ministry of Industry and Information Technology,College of Energy and Power Engineering, Nanjing University of Aeronautics and Astronautics, Nanjing 210016, P.R.China;

    2.Jiangsu Province Key Laboratory of Aerospace Power System, College of Energy and Power Engineering, Nanjing University of Aeronautics and Astronautics, Nanjing 210016, P.R.China;

    3.State Key Laboratory of Mechanics and Control Mechanical Structures, Nanjing University of Aeronautics and Astronautics,Nanjing 210016, P.R.China

    Abstract: Effects of different broaching machining techniques on fatigue damages are studied.Low cycle fatigue tests at high temperature 650 ℃ in air environment are carried out for specimens with four processing techniques.The roughness characterization method, electron backscatter diffraction (EBSD) and nanoindentation test are used to obtain the surface roughness, residual stress and work hardening, respectively.The wire cut electrical discharge machining (WEDM) specimens exhibit the highest fatigue life of average 80 360 cycle with the lowest surface roughness of 0.226 and residual stress, while specimens machined by blunt tool suffer the lowest fatigue life of average 43 978 cycle, decreasing 45% compared to WEDM ones.SEM results show that fatigue cracks are mainly initiated from the coarse non-recrystallized grains and machining defects.The broaching machining methods and parameters have significant influences on the level of fatigue damages and fatigue lives.

    Key words:broaching machining techniques; fatigue life; nickel-based powder metallurgy superalloy; surface roughness; residual stress; work hardening

    0 Introduction

    Nickel-based powder metallurgy superalloy is a kind of metal material suitable for aeroengines, but it is also vulnerable to the influence of machining process on fatigue life.The damage generated in the machining process will cause the fatigue damage to the high load components, thus damaging the integrity of components[1-2].

    The failure of surface integrity is the main inducement of fatigue failure[3-4].Machining damage will lead to surface tearing, inclusion cracking, cavity formation, carbide cracking or grain pulling,which will undermine the surface integrity of parts[1,5-8].Aggressive machining conditions will produce a “white layer” composed of nanoscale grain structure to induce local changes in the microstructure[5-9].Under high temperature and high stress conditions, such changes will seriously reduce the fatigue life[1,9-10].In addition, local stress concentration during machining will also lead to early crack initiation[11-12].Quan et al.[13]used the stress concentration factor to measure the fatigue life, and the results showed that the emergency concentration factor and the fatigue life fitted well.

    The fatigue life of turbine components is very important to the integrity of aeroengines when they work under high temperature and high load.The turbine components are usually manufactured by broaching.Since turbines are usually made of high strength super-alloy materials, the increased cutting rates and feed rates will lead to an increase in the degree of work hardening of the “white layer”[14-15].Meanwhile, broaching tools will have rapid wear[16], which is affected by broaching speed,broaching force, lubrication and other factors[12,17].Tool wear can lead to changes in coating and surface roughness[1,18], and the inevitable vibration in the machining process will also lead to the increase of surface roughness[19], and ultimately affect the fatigue life.Rengen et al.[20]studied the surface integrity characteristics of Udimet 720Li under slight damage and damage machining conditions.The correlation between machining conditions and plastic deformation is established.The mechanical effect of traditional machining can lead to serious plastic deformation and work hardening of metal workpiece[2].Therefore, the hardness characterization of specimens in fatigue test is indispensable.The residual stress produced by machining will also affect the fatigue life[21-23], and the dominant factor is to consider the equivalent stress of shear stress and normal stress at the same time[24-25].

    There is little research on the effect of machining conditions on the fatigue life of nickel base superalloys.Quan et al.[26]conducted a comparative study on the surface integrity and fatigue performance of GH4169 superalloy components manufactured by the combined process of milling, grinding and polishing.The results show that polishing has the greatest influence on fatigue performance, and a typical“hook” residual stress distribution is produced on the surface by milling.Chen et al.[27]studied broaching operations (similar to the machining of cold wood grooves on turbine disks) and the subsequent heat treatments at 550 ℃ and 650 ℃ on fatigue properties and corresponding crack initiation behavior.The combined effect of heat treatment on the fatigue properties and corresponding crack initiation behavior of forged Inconel 718.The research shows that the broaching specimen has a longer fatigue life than the polished one, but the 650 ℃-heat treatment reduces the fatigue life of the broaching specimen and increases the fatigue life of the polished specimen.Telesman et al.[28]studied the influence of tool wear and broaching speed on fatigue life.The research shows that the average fatigue life of “blunt” cutter is longer, but the fatigue life is more dispersed at different broaching speeds.Connolley et al.[29]studied the influence of different broaching processes on fatigue life at 600 ℃.The research shows that fatigue life is related to surface roughness, and notch polishing has a favorable effect on fatigue life.

    In this paper, the influence of different machining conditions on the fatigue life of the third-generation nickel base powder superalloy is studied.The surface roughness, hardness and electron backscatter diffraction (EBSD) characterization of specimens with different machining conditions are carried out, and the influence of different machining conditions on the fatigue life and fracture characteristics are analyzed.

    1 Materials and Methods

    1.1 Material and specimen machining

    The third-generation nickel-based powder metallurgy superalloys is used in this study.The specimen is designed according to the standard GB/T 3075—2008 as shown in Fig.1.Specimens are 95 mm in length.Middle segment of specimen is 11 mm in width and 3 mm in thickness.M4×23 threads are machined in both ends of specimen to suit the fixture.Connections between the threaded specimen and the middle specimen are chamfered to reduce the stress concentration.A finite element model with a notchrof 4 mm, depth of 1.3 mm,the elastic modulus of 169 GPa at 650 ℃ and Poisson’s ratio of 0.3 is established.The fixed constraint is applied to the right end face with the triangular waveform with stress ratio of 0.05, the maximum stress of 700 MPa and frequency of 10 Hz.The results show that the maximum stress and maximum strain are both at root of the notch, with the value of 1 413 MPa and 0.823%, respectively.The location and depth of the notch can be therefore determined.The notch with radiusrof 4 mm and depth of 1.3 mm is processed in the middle of specimens.

    Fig.1 Specimen shape and dimension drawing and some processed test pieces (Unit: mm)

    Through repeated trial production and exploration of different machining techniques (wire-electrode cutting, conventional tool and blunt tool)and machining parameters (milling spindle speed and feed rate), the roughness and other indicators caused by machining are investigated, and the following four machining conditions are finally determined.(1) Wire cut electrical discharge machining(WEDM), slow-feeding EDM wire-cut + removal of surface corrosion layer; (2) conventional tool, feed rate F260, spindle speed S2800; (3)conventional tool, feed rate F260, spindle speed S2000; (4) blunt tool, feed rate F600, spindle speed S3500.Five sets of experiments are performed for each process condition as shown in Table 1.

    Table 1 Experimental scheme for research on effect of machining damage on fatigue properties of powder superalloys

    Under the condition of 650 ℃, triangular wave stress with a stress ratio of 0.05 and a frequency of 10 Hz is applied to the test piece for fatigue test.The maximum load applied shall ensure that the maximum strain at the bottom of the notch is 0.823%.

    1.2 Fatigue test and fracture analysis method

    The test is carried out by a 100 kN MTS Landmark hydraulic-servo fatigue testing machine combined with a high temperature furnace.The test system consists of heating, loading, cooling, temperature monitoring and other parts.The fatigue testing machine is used for loading, and the high temperature furnace is used for heating with one thermocouple, connected to temperature monitoring.The fatigue test equipment is shown in Fig.2.Fatigue life is obtained by repeated stretching until specimen failure.The fatigue test is stress-controlled, with the maximum stress of 700 MPa, stress ratio of 0.05 and frequency of 10 Hz, at temperature of 650 ℃.

    Fig.2 Low cycle fatigue test equipment

    In order to reveal the damage mechanism of the material under uniaxial thermomechanical fatigue load, after the fatigue failure, the fracture is cut off and cleaned with an ultrasonic cleaner.When fracture occurs, the acceleration voltage is set to 15 kV.

    1.3 Specimen characterization method

    The notch roughness under different machining technologies is tested by Taylor Hobson Form Talysurf i-Series 5 shape and surface roughness tester.The thimble is in contact with the surface of the notch root, and the trajectory is reciprocated three times to obtain the average value of the measured roughness.Nano Test Vantage is used to measure the microhardness in the notch root area of specimens with different machining techniques.In order to exclude the influence of acquisition parameters on the related data of different specimens, the uniform load for microhardness measurement is 20 mN, the holding time is 30 s, the microhardness indentation spacing is 4 μm, and the area size is 32 μm ×48 μm.In the process of hardness and characterization EBSD analysis of FGH4099 notched specimens under different machining conditions, a 400 μm×400 μm area at the root of the notched specimen is selected for observation.It is selected mainly because the load on this area during the specimen machining is relatively high.It can be used to evaluate the residual stress field introduced by different machining processes and the variation law of residual stress on fatigue life during subsequent lowcycle fatigue tests.In order to avoid excessive deformation, the processed notch specimen is cut by EDM machining method, and then 400#, 800#,1000#, 2000#, 3000# and 5000# sandpapers are used for grinding and polishing in turn by cold inserting treatment.Then, the specimens are mechanically polished with oxide polishing suspension for 20 min, and finally electropolished with 10 ml perchloric acid and 90 ml ethanol solution for 10 s.EBSD measurements are performed on a Zeiss Gemini 500 field emission SEM equipped with an Oxford EBSD detector.In order to exclude the influence of EBSD acquisition parameters on the disorientation data of different specimens, a series of unified parameters, 15 kV accelerating voltage, 60 μm aperture and 0.5 μm step size, are adopted.Finally, the EBSD data are processed using Aztec Crystal software and the open-source toolbox MTEX, and the derived geometrically necessary dislocation (GND)density maps are calculated with a 3×3 core size.

    2 Experiment Results

    2.1 Influence of machining conditions on fatigue life and fracture analysis

    To avoid the influence of randomness on the four machining technologies, five groups of experiments are conducted under each machining technology.The results of fatigue life are given by low cycle fatigue test equipment, represented by the number of cycle when specimen breaks.The average low cycle fatigue life and average notch roughness under four processes are compared as shown in Fig.3.The average fatigue life of specimens machined by WEDM is the highest with 80 360 cycle, and that of specimens machined by blunt tool is the lowest with 43 978 cycle.The average fatigue life of specimens machined by conventional tool decreases from 72 035 to 48 603 when spindle speed decreases from 2 800 r/min to 2 000 r/min.It is observed that the average low cycle fatigue life is negatively correlated with the average notch roughness.That is, the higher the roughness, the shorter the life, but not linearly correlated.It is observed that the average roughness of notch is less than or equal to 0.8 μm and the average low cycle fatigue life decreases gradually with the increase of roughness in the range of 0.6×105—1.0×105.While the average notch roughness is greater than 0.8 μm, the average low cycle fatigue life is about 0.6×104.

    Fig.3 Relationship between average low cycle fatigue life and average notch roughness in different machining processes

    For each machining technology, a typical fatigue fracture is selected for SEM characterization.The microstructures of the fatigue fracture surfaces of the specimen machined by WEDM and surface corrosion layer removal machining technology are shown in Fig.4.Under this machining technology,the cracks of specimen are initiated from the coarse non-recrystallized grains on the sub surface at the center of the notch root, and these cracks exhibit transgranular propagation[30-32].Fatigue bands and secondary cracks exhibiting transgranular propagation can be observed in the crack growth area, and there are a lot of step slip surfaces similar to cleavage in the transient fault zone.It shows that due to the minimum notch work hardening and the minimum plastic deformation under this machining technology, the cracks are initiated from the material defects inside the specimen, and this case has the longest average low-cycle fatigue life.

    Fig.4 Low cycle fatigue micro fracture diagram of WEDM specimen

    The microstructure of the fatigue fracture surface of the specimen machined by conventional tool with F260S2800 is similar to that of WEDM, as shown in Fig.5.Under this machining technology,the cracks of specimen are also initiated from the non-recrystallized grains on the sub surface at the right of the notch root, and the cracks exhibit transgranular propagation.The fatigue bands and secondary cracks exhibiting transgranular propagation can be observed in the crack propagation area, and secondary cracks can be observed in the transient fracture area.The cracks are initiated from the material defects on the sub-surface of the specimen under this machining condition.

    Fig.5 Low cycle fatigue micro fracture diagram of F260S2800 specimen

    The microstructure of the fatigue fracture surface of the specimen machined by conventional tool with F260S2000 is similar to that of WEDM, as shown in Fig.6.Under this machining technology,the cracks of specimen are initiated at the left edge of the notch root at the machining defect location.Due to the machining defects, the stress concentration between the notch root surface and the side interface has led to the initiation of cracks at the left edge of the notch root section.The crack exhibites transgranular propagation, and a secondary crack can be observed in the crack transient zone.Compared with the conventional tool with F260S2800, this kind of machining condition brings higher work hardening and plastic deformation due to greater roughness.Therefore,the crack is initiated from the machining defects at the corner of the notch root, resulting in a significant reduction in the average low cycle fatigue life.

    Fig.6 Low cycle fatigue micro fracture diagram of F260S2000 specimen

    The microstructure of fatigue fracture surface of the specimen machined by blunt tool with F600S3500 machining technology is similar to that of WEDM, as shown in Fig.7.Under this machining technology,the crack source of specimen is at the left edge of the notch root where there is a machining defect.Because of the machining defect, the stress at the interface between the notch root surface and the side surface is concentrated, which leads to the crack initiation at the upper left corner of the notch root cross section.The crack propagates transgranularly.Fatigue striations are observed in the crack growth zone, and there is a step like sliding surface similar to cleavage in the transient fracture zone.Blunt tools produce large plastic deformation, so cracks are initiated from the machining defects where the surface of the notch root meets the flank.The average low cycle fatigue life under this machining condition is the smallest but not much different from the average low cycle fatigue life of the conventional tool with F260S2000.

    Fig.7 Low cycle fatigue micro fracture diagram of blunt tool specimen

    2.2 Roughness characterization results

    Roughness test is carried out on the notches processed by four different processes, whose results are shown in Table 2.

    Table 2 Test results of notch roughness of different machining processes

    Among the four machining conditions, slowfeeding EDM wire-cut has the lowest surface roughness, and blunt tool milling with a feed rate of F600 and a spindle speed of S3500 has the highest surface roughness.Higher spindle speeds for conventional tool milling correspond to lower surface roughness.

    2.3 EBSD microstructure characterization results and hardness characterization

    EBSD characterization results of four machining notches (WEDM, conventional tool cutting with F260S2800, conventional tool cutting with F260S2000, blunt tool cutting with F600S3500)are shown in Fig.8.There are about six grains in the transverse range, and the presence of strengthening phase can be clearly seen in the EBSD image.It can be seen from the GND image that the specimen machined by blunt tool has the highest geometrically necessary dislocations on the whole.The work hardening layer of WEDM is the thinnest, and the work hardening layer of blunt tool is thicker.With the decrease of rotational speed, the work hardening layer of specimen machined by conventional tool thickens.The effect of machining technology to the working hardening of specimens is obvious.The work hardening of specimens machined by WEDM is the smallest and that of specimens machined by blunt tool is the biggest.With the increase of spindle speed, the work hardening of specimens machined by conventional tool decreases.

    Fig.8 EBSD of four machining notches

    In order to qualitatively analyze the plastic deformation caused by work hardening at the notch,the GND value of the notch with smaller roughness in each machining technology is selected for comparison.The GND value of most areas in the visual field is small, and the GND value at the notch is large, so the part with GND=0.5 is selected for comparison.The GND distribution of the notch of the four machining processes is shown in Fig.9.It is found that the depth of work hardening under the slow-feeding EDM wire-cut process is the minimum, and the depth of work hardening under the F350S3500 process is the maximum.The peak of GND close to notch root of specimens machined by blunt tool is the biggest at 1.464×1014/m2, and that of specimens machined by WEDM is the smallest at 0.985×1014/m2.With the spindle speed decreasing from 2 800 r/min to 2 000 r/min, the peak of GND close to notch root of specimens machined by conventional tool increases from 1.065 to 1.330.

    The hardness of 32 μm ×48 μm area at the notch root of four machining technologies is characterized.The results are shown in Figs.10—12.With the increase of the distance from the notch, the depth of indentation becomes deeper and deeper, indicating that the work hardening decreases with the increase of the distance from the notch, and finally tends to be stable.WEDM and F260S2800 have the lower hardness at the notch root, F260S2000 and Blunt tool has the higher hardness.Blunt tool has the thickest work hardening layer and the work hardening layer of WEDM and F260S2800 is thinner.The hardness of notch root of specimens machined by blunt tool is the biggest at 7.507 GPa, and that of specimens machined by conventional tool F260S2800 is the smallest at 7.001 GPa.The work hardening of specimens machined by conventional tool is higher with spindle speed slower.

    Fig.10 Hardness nephogram of notch root with different machining technologies

    Fig.11 Variation of hardness with notch distance

    Fig.12 Force-depth curves of nanoindentation tests for different machining technologies

    3 Discussion

    Specimens machined by blunt tool has the lowest fatigue life, with the highest residual stress and work hardening.Specimens machined by WEDM has the highest fatigue life, with the lowest residual stress and lower work hardening.Effect of spindle speed to specimens machined by conventional tool is obvious, in which the spindle speed increases 800 r/min, the fatigue life increases 48%, and the residual stress and the work hardening decrease.The fatigue damage of WEDM is the smallest, and the blunt tool has the worst fatigue damage on specimens.

    Through SEM characterization of fractures, it is found that under the two machining parameters of low surface roughness and work hardening, the machining defects are not enough to produce cracks,and the cracks are caused by the internal defects of the material.Under these two machining parameters, the fatigue life of the specimen is higher.However, when the surface roughness and work hardening are higher, the crack initiation occurs at the stress concentration of the machining defect, so the specimen is more prone to fatigue fracture.The fatigue life is higher when the cracks are initiated from the defects at the subsurface, while the crack initiation at the specimen surface leads to lower fatigue life.

    Secondary cracks are caused by weak structures in the plastic zone around the main cracks in the process of material failure, which may be related to metal preparation processes such as inclusion,grain orientation such as large angle grain boundaries and other structures.The fatigue life of the material is mainly affected by the crack initiation mode.In the low cycle fatigue life, the crack initiation life occupies the main part and the crack propagation life is secondary.

    The influence of different machining technologies on fatigue life is investigated.As shown in Fig.3,the surface roughness is inversely proportional to the fatigue life.There is no significant difference in the work hardening between F260S2800 and WEDM through EBSD and hardness characterization, indicating that the fatigue failure of these two machining processes is mainly affected by surface roughness.The work hardening degree of F260S2000 and blunt tool is significantly higher than that of WEDM and F260S2800, and the fatigue life of specimens under these two machining techniques is lower.There is little difference in work-hardening between F260S2000 and blunt tool, but there is a big difference in surface roughness.Result shows that there is little difference in fatigue life between F260S2000 and blunt tool, and the influence of roughness on fatigue life is small when the roughness is greater than or equal to 0.563 μm.The cracks of specimens machined by blunt tool and conventional tool with F260S2000 are initiated at stress concentration caused by the combination of high surface roughness and work hardening, which gives a shorter fatigue crack initiation time.

    According to the analysis of the fracture, the work hardening of WEDM and F260S2800 notch is small, the work hardening of F260S2000 and blunt tool is significantly higher, and the crack initiation is concentrated in the machining defect of notch root.

    4 Conclusions

    For the third-generation nickel-based superalloy FGH4099, the influence of different machining techniques to the damage of specimens on low-cycle fatigue properties are studied.The conclusions are as follows.

    (1) The order of machining techniques with the notch surface roughness increasing from 0.226 to 0.776 is as follows: WEDM, conventional tool with F260S2800, conventional tool with F260S2000,and blunt tool with F600S3500.

    (2) WEDM and removal of the surface corrosion layer have the least residual work hardening and minimum plastic deformation.Compared with conventional tool, blunt tool has more work hardening and greater plastic deformation.

    (3) The average low cycle fatigue life is negatively correlated with the average notch roughness.That is, the higher the roughness, the shorter the life, but it is not linear.The fatigue life decreases 45% when the surface roughness increases 243%.

    (4) The average roughness sum is less than or equal to 0.405 μm, and the defect size produced by machining is too small to produce cracks.When the average roughness is greater than or equal to 0.563 μm, the low cycle fatigue life is mainly affected by the notch machining defects.The notch roughness is large, and the crack starts from the stress concentration of machining defect at the notch root.

    (5) The level of fatigue damage of specimens machined by WEDM is the lowest with the highest fatigue life of 80 360 cycle, and specimens machined by blunt tool suffer the most significant fatigue damage with the lowest fatigue life of 43 978 cycle.

    一区福利在线观看| www国产在线视频色| 男女之事视频高清在线观看| 一区福利在线观看| 婷婷六月久久综合丁香| 国产伦一二天堂av在线观看| 久久久久久久久中文| 欧美成人免费av一区二区三区| 别揉我奶头~嗯~啊~动态视频| 男女视频在线观看网站免费 | 一二三四在线观看免费中文在| 久久久久久久久中文| 丁香六月欧美| 怎么达到女性高潮| 亚洲国产中文字幕在线视频| 久久这里只有精品19| 亚洲成av人片免费观看| 国产精品久久久久久人妻精品电影| 18禁美女被吸乳视频| 露出奶头的视频| 国产亚洲欧美在线一区二区| 久久久久久久久久黄片| 免费av毛片视频| 亚洲美女黄片视频| 久久久久久九九精品二区国产 | 欧美性长视频在线观看| 亚洲av片天天在线观看| 国产成人av激情在线播放| 国产精品 欧美亚洲| 九色国产91popny在线| 久久草成人影院| 91国产中文字幕| 视频在线观看一区二区三区| 一级片免费观看大全| 少妇裸体淫交视频免费看高清 | av天堂在线播放| 欧美成人午夜精品| 午夜两性在线视频| 国产精品一区二区精品视频观看| 一级黄色大片毛片| 一二三四在线观看免费中文在| 又紧又爽又黄一区二区| 黄色成人免费大全| 亚洲专区国产一区二区| 国产视频一区二区在线看| 精品不卡国产一区二区三区| 在线观看www视频免费| 亚洲精品在线美女| 国内少妇人妻偷人精品xxx网站 | xxxwww97欧美| 欧美黄色淫秽网站| 成人国语在线视频| 首页视频小说图片口味搜索| 两人在一起打扑克的视频| 亚洲免费av在线视频| 国产单亲对白刺激| 精品欧美一区二区三区在线| 午夜成年电影在线免费观看| 亚洲欧洲精品一区二区精品久久久| 亚洲avbb在线观看| 久久久久精品国产欧美久久久| 国产aⅴ精品一区二区三区波| 欧美一级a爱片免费观看看 | 成人一区二区视频在线观看| 黄色毛片三级朝国网站| 91在线观看av| 黑人操中国人逼视频| 日本熟妇午夜| 国产黄片美女视频| 精品一区二区三区视频在线观看免费| 精品国产亚洲在线| 日韩中文字幕欧美一区二区| 丝袜在线中文字幕| 午夜福利高清视频| 日韩成人在线观看一区二区三区| 丁香欧美五月| 国产又爽黄色视频| 午夜a级毛片| 少妇被粗大的猛进出69影院| 久久精品国产清高在天天线| 99精品欧美一区二区三区四区| 19禁男女啪啪无遮挡网站| 丁香欧美五月| 脱女人内裤的视频| 国产在线精品亚洲第一网站| 91老司机精品| 一级黄色大片毛片| 黄色毛片三级朝国网站| 可以在线观看毛片的网站| 黄色毛片三级朝国网站| 国产精品亚洲美女久久久| 日韩精品中文字幕看吧| 国产精品一区二区精品视频观看| 一级毛片精品| 亚洲欧美日韩高清在线视频| 久久久久久久久免费视频了| 50天的宝宝边吃奶边哭怎么回事| 国产精品野战在线观看| 在线观看舔阴道视频| 亚洲av成人一区二区三| 超碰成人久久| 熟女电影av网| 成人国产一区最新在线观看| 亚洲国产精品sss在线观看| avwww免费| 亚洲国产欧洲综合997久久, | 九色国产91popny在线| 一级毛片精品| 国产一卡二卡三卡精品| 国产亚洲精品第一综合不卡| 中文字幕人成人乱码亚洲影| 久久中文看片网| videosex国产| 日本免费a在线| 久久精品成人免费网站| 国产av又大| 男人操女人黄网站| x7x7x7水蜜桃| 狂野欧美激情性xxxx| 黄色丝袜av网址大全| 亚洲av中文字字幕乱码综合 | 俄罗斯特黄特色一大片| 大型av网站在线播放| 91国产中文字幕| 无人区码免费观看不卡| 亚洲男人的天堂狠狠| 欧美国产日韩亚洲一区| 黄色a级毛片大全视频| 久久久久久久久中文| 国语自产精品视频在线第100页| 精品少妇一区二区三区视频日本电影| 每晚都被弄得嗷嗷叫到高潮| 日韩精品青青久久久久久| 国产又色又爽无遮挡免费看| 波多野结衣高清作品| 久久中文字幕一级| a在线观看视频网站| 久久久精品国产亚洲av高清涩受| 法律面前人人平等表现在哪些方面| 脱女人内裤的视频| 欧美性长视频在线观看| 国产亚洲精品久久久久久毛片| 神马国产精品三级电影在线观看 | 女人高潮潮喷娇喘18禁视频| 草草在线视频免费看| 亚洲精品美女久久久久99蜜臀| 欧美日韩亚洲综合一区二区三区_| 最近最新免费中文字幕在线| 久9热在线精品视频| 狂野欧美激情性xxxx| 人妻久久中文字幕网| 精品国内亚洲2022精品成人| 91在线观看av| 日韩中文字幕欧美一区二区| 波多野结衣av一区二区av| 1024香蕉在线观看| 国产欧美日韩精品亚洲av| 亚洲黑人精品在线| 女警被强在线播放| 亚洲国产中文字幕在线视频| 夜夜躁狠狠躁天天躁| 国产精品国产高清国产av| 亚洲av成人不卡在线观看播放网| 亚洲男人天堂网一区| 久久久久久大精品| 天堂动漫精品| 免费高清在线观看日韩| 欧美激情极品国产一区二区三区| 日本免费a在线| 99精品久久久久人妻精品| 精品久久久久久久久久久久久 | 人人妻,人人澡人人爽秒播| www日本黄色视频网| 天堂√8在线中文| 欧美日本视频| netflix在线观看网站| 不卡av一区二区三区| 免费在线观看影片大全网站| 男人舔女人下体高潮全视频| or卡值多少钱| 十八禁人妻一区二区| xxxwww97欧美| 国产1区2区3区精品| 亚洲专区国产一区二区| 无遮挡黄片免费观看| 国产精品一区二区三区四区久久 | 国产成人av教育| svipshipincom国产片| 中文字幕高清在线视频| 欧美不卡视频在线免费观看 | 久久精品91蜜桃| 亚洲国产毛片av蜜桃av| 久久婷婷人人爽人人干人人爱| АⅤ资源中文在线天堂| 国产精品 国内视频| 天天躁夜夜躁狠狠躁躁| 亚洲专区中文字幕在线| 美女午夜性视频免费| 久久中文字幕人妻熟女| 亚洲最大成人手机在线| 中出人妻视频一区二区| 国产av麻豆久久久久久久| 免费无遮挡裸体视频| 国产午夜精品久久久久久一区二区三区 | 蜜桃久久精品国产亚洲av| 日韩一区二区视频免费看| 欧美日韩一区二区视频在线观看视频在线 | 久久这里只有精品中国| 国产一区亚洲一区在线观看| 国产黄色小视频在线观看| 成人性生交大片免费视频hd| 亚洲精品乱码久久久v下载方式| 在线国产一区二区在线| av.在线天堂| 国产精品无大码| 免费高清视频大片| videossex国产| 国产v大片淫在线免费观看| 成人av在线播放网站| 一级av片app| 日日摸夜夜添夜夜添小说| 黄色日韩在线| 久久人人精品亚洲av| 最近视频中文字幕2019在线8| 亚洲av免费高清在线观看| 别揉我奶头 嗯啊视频| 日韩,欧美,国产一区二区三区 | 日韩制服骚丝袜av| 寂寞人妻少妇视频99o| 在线观看66精品国产| 亚洲精华国产精华液的使用体验 | 久久精品国产亚洲av涩爱 | 亚洲人成网站高清观看| 男人的好看免费观看在线视频| 天天躁日日操中文字幕| 美女 人体艺术 gogo| 午夜福利成人在线免费观看| 老女人水多毛片| 小蜜桃在线观看免费完整版高清| 国产精品1区2区在线观看.| 国产精品综合久久久久久久免费| 3wmmmm亚洲av在线观看| 国产成人91sexporn| 亚洲av第一区精品v没综合| 亚洲欧美中文字幕日韩二区| 久久久国产成人精品二区| 国产精品永久免费网站| 日韩在线高清观看一区二区三区| 亚洲欧美精品自产自拍| 午夜福利18| 亚洲综合色惰| 日韩欧美免费精品| 亚洲国产精品成人久久小说 | 美女cb高潮喷水在线观看| 免费在线观看成人毛片| 国产综合懂色| 亚洲av中文字字幕乱码综合| 三级经典国产精品| 国产精品久久久久久亚洲av鲁大| 久久久久久久久大av| 我要搜黄色片| 久久午夜亚洲精品久久| 女的被弄到高潮叫床怎么办| 国产色婷婷99| 婷婷精品国产亚洲av| 国产精品亚洲一级av第二区| 国产三级在线视频| 十八禁网站免费在线| 国产精品久久视频播放| 久久99热6这里只有精品| 欧美xxxx黑人xx丫x性爽| 色综合站精品国产| 春色校园在线视频观看| 成年av动漫网址| 日本一本二区三区精品| 国产单亲对白刺激| 国产精品伦人一区二区| aaaaa片日本免费| 国产 一区 欧美 日韩| 麻豆一二三区av精品| 波野结衣二区三区在线| 国产av在哪里看| 女生性感内裤真人,穿戴方法视频| 国模一区二区三区四区视频| 日本撒尿小便嘘嘘汇集6| 亚洲在线观看片| 一个人看的www免费观看视频| 日产精品乱码卡一卡2卡三| 国产精品一及| 少妇猛男粗大的猛烈进出视频 | 欧美又色又爽又黄视频| 97超视频在线观看视频| 少妇猛男粗大的猛烈进出视频 | 国产精品久久久久久久电影| 少妇被粗大猛烈的视频| 我要看日韩黄色一级片| 日本一二三区视频观看| 国产单亲对白刺激| 真人做人爱边吃奶动态| 九九在线视频观看精品| 村上凉子中文字幕在线| 日本精品一区二区三区蜜桃| 性插视频无遮挡在线免费观看| 日本撒尿小便嘘嘘汇集6| 久久人妻av系列| 国产伦一二天堂av在线观看| 国内少妇人妻偷人精品xxx网站| 国产精品人妻久久久影院| 夜夜爽天天搞| 如何舔出高潮| 免费一级毛片在线播放高清视频| 国产一级毛片七仙女欲春2| 久久久久久伊人网av| 日日摸夜夜添夜夜爱| 久久精品夜色国产| 亚洲人成网站高清观看| 中文亚洲av片在线观看爽| 久久精品久久久久久噜噜老黄 | 亚洲欧美日韩高清在线视频| 亚洲最大成人中文| 亚洲精品在线观看二区| 免费高清视频大片| 男插女下体视频免费在线播放| 久久精品国产亚洲av天美| 日日摸夜夜添夜夜添av毛片| 精品人妻偷拍中文字幕| 精品乱码久久久久久99久播| 久久午夜福利片| 99热这里只有精品一区| 天天一区二区日本电影三级| 久久人人精品亚洲av| 深爱激情五月婷婷| 久久草成人影院| 久久亚洲国产成人精品v| 国产高潮美女av| 免费不卡的大黄色大毛片视频在线观看 | 成人亚洲精品av一区二区| 在线播放无遮挡| 麻豆久久精品国产亚洲av| av免费在线看不卡| 夜夜爽天天搞| 蜜桃久久精品国产亚洲av| 亚洲,欧美,日韩| 自拍偷自拍亚洲精品老妇| 18禁在线播放成人免费| 非洲黑人性xxxx精品又粗又长| 午夜精品一区二区三区免费看| 人人妻人人澡人人爽人人夜夜 | 国产免费男女视频| 2021天堂中文幕一二区在线观| 成年女人永久免费观看视频| 给我免费播放毛片高清在线观看| 中文字幕人妻熟人妻熟丝袜美| .国产精品久久| 99热网站在线观看| 97热精品久久久久久| 亚洲av电影不卡..在线观看| 99久国产av精品| 成人无遮挡网站| 国产爱豆传媒在线观看| 最近在线观看免费完整版| 久久精品人妻少妇| 如何舔出高潮| 超碰av人人做人人爽久久| 日韩成人av中文字幕在线观看 | 日本熟妇午夜| 久久热精品热| 露出奶头的视频| 麻豆av噜噜一区二区三区| 尾随美女入室| 日韩中字成人| 国产一区二区激情短视频| 好男人在线观看高清免费视频| 亚洲最大成人中文| 色播亚洲综合网| 国产黄片美女视频| 男女视频在线观看网站免费| 在线播放无遮挡| 我要看日韩黄色一级片| 免费av观看视频| 激情 狠狠 欧美| 国产亚洲精品综合一区在线观看| 中文字幕熟女人妻在线| 91狼人影院| 日本免费a在线| 欧美人与善性xxx| 嫩草影院新地址| 欧美绝顶高潮抽搐喷水| 一个人观看的视频www高清免费观看| 黄色一级大片看看| 午夜福利在线观看吧| 成人亚洲欧美一区二区av| 俺也久久电影网| 亚洲经典国产精华液单| 亚洲欧美日韩卡通动漫| 亚洲av二区三区四区| 欧美成人a在线观看| 精品不卡国产一区二区三区| 毛片女人毛片| 悠悠久久av| 三级毛片av免费| 2021天堂中文幕一二区在线观| 男人狂女人下面高潮的视频| 男女做爰动态图高潮gif福利片| 久久久久精品国产欧美久久久| 香蕉av资源在线| av在线老鸭窝| 国产av不卡久久| 小蜜桃在线观看免费完整版高清| 免费观看人在逋| 免费看光身美女| 久久6这里有精品| av天堂中文字幕网| 欧美色视频一区免费| 国产乱人视频| 最新在线观看一区二区三区| 一本久久中文字幕| 色哟哟哟哟哟哟| 亚洲欧美中文字幕日韩二区| 自拍偷自拍亚洲精品老妇| 成年女人毛片免费观看观看9| 亚洲精品成人久久久久久| 九九爱精品视频在线观看| 丰满的人妻完整版| 淫妇啪啪啪对白视频| 哪里可以看免费的av片| 欧美高清成人免费视频www| 超碰av人人做人人爽久久| 国产精品国产高清国产av| 国产成人a∨麻豆精品| 在线天堂最新版资源| 午夜精品在线福利| av天堂在线播放| 成人鲁丝片一二三区免费| 精华霜和精华液先用哪个| 高清毛片免费看| 亚洲av免费在线观看| 成人综合一区亚洲| 18禁在线播放成人免费| 国语自产精品视频在线第100页| 97热精品久久久久久| 麻豆久久精品国产亚洲av| 精品无人区乱码1区二区| 亚洲精品日韩av片在线观看| 亚洲天堂国产精品一区在线| 国产一区二区亚洲精品在线观看| 国产伦在线观看视频一区| 亚洲七黄色美女视频| 欧美日韩综合久久久久久| 亚洲最大成人手机在线| 日本五十路高清| 99久国产av精品| 久久久久久久久大av| 一级毛片aaaaaa免费看小| 露出奶头的视频| 天天一区二区日本电影三级| 亚洲欧美清纯卡通| 天天躁夜夜躁狠狠久久av| 夜夜夜夜夜久久久久| 国产不卡一卡二| 一本精品99久久精品77| 国产成人福利小说| 免费看光身美女| 性色avwww在线观看| 午夜福利高清视频| 如何舔出高潮| 深夜精品福利| 97超碰精品成人国产| 两个人视频免费观看高清| 亚洲专区国产一区二区| 国产片特级美女逼逼视频| av在线观看视频网站免费| 精品久久久久久成人av| АⅤ资源中文在线天堂| 国产免费男女视频| 亚洲精品国产av成人精品 | 精品福利观看| 国产男人的电影天堂91| 国产伦在线观看视频一区| 欧美成人a在线观看| 1000部很黄的大片| 日本黄色片子视频| 亚洲av.av天堂| 亚洲av中文字字幕乱码综合| 69av精品久久久久久| 亚洲中文字幕日韩| 国产日本99.免费观看| 欧美bdsm另类| 淫妇啪啪啪对白视频| 黄色视频,在线免费观看| 国产精品一区二区三区四区免费观看 | 欧美潮喷喷水| 我要搜黄色片| 日本黄色视频三级网站网址| 秋霞在线观看毛片| 日韩精品有码人妻一区| 成人一区二区视频在线观看| 一个人免费在线观看电影| 三级男女做爰猛烈吃奶摸视频| 最近在线观看免费完整版| 国产一区二区三区av在线 | 永久网站在线| 女人被狂操c到高潮| 我的女老师完整版在线观看| 91在线观看av| 亚洲高清免费不卡视频| 日韩av不卡免费在线播放| 国产91av在线免费观看| 麻豆国产97在线/欧美| 成人高潮视频无遮挡免费网站| 给我免费播放毛片高清在线观看| 亚洲美女黄片视频| 国产色爽女视频免费观看| 国产精品精品国产色婷婷| h日本视频在线播放| 亚洲国产色片| 少妇丰满av| 中文字幕久久专区| 国产黄色小视频在线观看| 亚洲人成网站在线播放欧美日韩| 97超级碰碰碰精品色视频在线观看| 丰满的人妻完整版| 欧美高清成人免费视频www| 18禁在线无遮挡免费观看视频 | 成年av动漫网址| 国产成人福利小说| 免费无遮挡裸体视频| 久久久国产成人免费| 日韩中字成人| 国产欧美日韩精品一区二区| 成人午夜高清在线视频| 麻豆久久精品国产亚洲av| 极品教师在线视频| 精品午夜福利在线看| 国产成人freesex在线 | 一级a爱片免费观看的视频| 真实男女啪啪啪动态图| 亚洲av一区综合| 午夜福利在线观看免费完整高清在 | 午夜福利成人在线免费观看| 麻豆国产97在线/欧美| 亚洲av五月六月丁香网| 国产人妻一区二区三区在| 日韩精品有码人妻一区| 亚洲中文日韩欧美视频| 最后的刺客免费高清国语| 自拍偷自拍亚洲精品老妇| av在线老鸭窝| 69人妻影院| 麻豆久久精品国产亚洲av| 老司机福利观看| 99在线人妻在线中文字幕| 国产精品一区二区三区四区免费观看 | 伦理电影大哥的女人| 国产精品美女特级片免费视频播放器| 国产精品av视频在线免费观看| 在线国产一区二区在线| 一本久久中文字幕| 国产 一区精品| 成人美女网站在线观看视频| 亚洲七黄色美女视频| 欧美一区二区精品小视频在线| 女的被弄到高潮叫床怎么办| 国产精品日韩av在线免费观看| 亚洲色图av天堂| 少妇熟女欧美另类| 日韩欧美三级三区| 日韩,欧美,国产一区二区三区 | 午夜福利视频1000在线观看| 色在线成人网| 欧美一级a爱片免费观看看| 精品免费久久久久久久清纯| 麻豆久久精品国产亚洲av| 亚洲人成网站在线播| 天美传媒精品一区二区| 精品一区二区三区视频在线观看免费| 成人二区视频| 国产精品三级大全| 在线观看66精品国产| 日本黄色片子视频| 免费高清视频大片| 婷婷精品国产亚洲av| 97超级碰碰碰精品色视频在线观看| 日韩欧美三级三区| 国产精品国产高清国产av| 非洲黑人性xxxx精品又粗又长| 在线免费观看的www视频| 不卡视频在线观看欧美| 国产精品美女特级片免费视频播放器| 一进一出好大好爽视频| 国产亚洲精品综合一区在线观看| 俺也久久电影网| 亚洲精品成人久久久久久| 小蜜桃在线观看免费完整版高清| 俺也久久电影网| 精品久久久久久久久亚洲| 中文字幕av在线有码专区| 午夜福利视频1000在线观看| 日韩中字成人| 亚洲成av人片在线播放无| 国产精华一区二区三区| 五月伊人婷婷丁香| 中文字幕av在线有码专区| 99久久精品国产国产毛片| 搡老岳熟女国产| 国产在线男女| 亚洲最大成人手机在线| 亚洲欧美成人综合另类久久久 | 国产欧美日韩精品一区二区| 亚洲精品久久国产高清桃花| 无遮挡黄片免费观看| 啦啦啦韩国在线观看视频| av卡一久久| 少妇人妻一区二区三区视频| 可以在线观看毛片的网站|