    Anisotropy in dynamic recrystallization behavior of AZ31 magnesium alloy

    2023-01-08 10:22:22FtemiKheyrdiPul
    Journal of Magnesium and Alloys 2022年12期

    S.M.Ftemi,S.Kheyrdi,H.Pul

    aDepartment of Metallurgy and Materials Engineering,Shahid Rajaee Teacher Training University,136-16785 Tehran,Iran

    b Institute of Metallurgy and Materials Science,Polish Academy of Sciences(PAS),25 Reymonta Street,30-059 Krakow,Poland

    Abstract Deformation behavior as well as microstructural evolutions of a rolled AZ31 magnesium alloy with and without pre-existing extension twins were studied using compression tests which performed along different orientations at a temperature range of 25-350 °C.The results implied that the initial texture not only influenc the evolution of fl w stress,but also change the size and fraction of recrystallized grains.In contrast to samples parallel to rolling and transverse directions,compression along normal direction resulted in a respectful softening at 150 °C.The largest size and fraction of new grains at 250 °C were recorded after deformation along rolling direction,while the maximum fl w softening was observed during deformation along normal direction.The anisotropy in microstructural evolutions was still retained at 350 °C.Pre-existing twins could reduce the anisotropy of material in respect of fl w stress as well as DRX progression,where TD sample showed the lowest DRX fraction at 250 °C.Quaternion misorientation data obtained from EBSD analysis of pretwinned material implied that initial texture could not significantl influenc fina texture.A different misorientation distribution was realized after deformation of pretwinned material along ND and RD directions.? 2021 Chongqing University.Publishing services provided by Elsevier B.V.on behalf of KeAi Communications Co.Ltd.This is an open access article under the CC BY-NC-ND license(http://creativecommons.org/licenses/by-nc-nd/4.0/)Peer review under responsibility of Chongqing University

    Keywords:Slip;Recrystallization;Grain size;Growth;Twin.

    1.Introduction

    There is currently growing interest in developing new applications for magnesium alloys in the aerospace and automotive industry sectors considering their desirable properties such as low density and high specifi strength[1].However,their hexagonal symmetry leads to workability limitations in magnesium alloy,which restrict their potential applications.The workability of magnesium is influence by different deformation mechanisms including basal and nonbasal slip as well as contraction and extension twinning[2].The ease of slip on basal plane of magnesium and related operating dislocation mechanisms were well-known to promote sharp textures in wrought alloy[3].Nevertheless,the predominant mechanisms will depend strongly on the loading mode and direction with respect to the c-axes of the grains[4].Accordingly,a textured material exhibited anisotropic mechanical behavior and as well as microstructural evolution along its different direction during deformation.The latter limits,in turn,the formability of material during secondary industrial processing[5].The anisotropic and asymmetric behavior of textured magnesium alloys at room temperatures have been the subject of different studies[6-8].

    Processing of wrought magnesium alloys usually perform at high temperatures.With increasing temperature the critical resolved shear stresses(CRSSs)for nonbasal slip systems and contraction twinning gradually decrease,while those remain relatively constant for basal slip and extension twinning[9].Thus,the degree to which different nonbasal slip contribute during deformation is enhanced with increasing temperature and the deformation is progressively accommodated by multiple slips[10].So,it is expected that the anisotropy in mechanical behavior to be reduced at high temperatures.However,due to anisotropic nature of crystal structure in magnesium,dislocation-dislocation and dislocation-boundary interactions describe the hardening behavior of the material along different directions.Moreover,magnesium alloys undergo dynamic recrystallization(DRX)during deformation at high temperatures,which is influence by multiple system activities[11].Therefore,the anisotropy in microstructural evolutions is complicated by diverse influenc of temperature and texture-loading orientationship.Al-Samman et al.[12]investigated the tension-compression anisotropy of an extruded AZ31 alloy at high temperatures.Their result implied that compression at 200 °C and 300 °C parallel to the extrusion axis favors tensile twinning over prismatic slip,which gives rise to high hardening rates.At 400 °C the deformation is carried out by a combination of prismatic slip,〈a〉pyramidal slip and basal slip.The study of high strain rate deformation of an AZ31 sheet at 250 °C showed that the highest resistance to dynamic recrystallization was found when the material was tested in tension along the rolling direction[13].Liu et al.[14]Studied deformation behavior of as-pressed AZ31 magnesium at 300 °C along different directions.They believed that it is crucial to have significan local dislocation accumulation to promote DRX,which is achieved by extensive dislocation activities starting from the early stages of deformation.However,the works by Li et al.[15]and Wang et al.[16]claimed that no effect of initial texture could be traced microstructures recrystallized during extrusion and rolling experiments,respectively.The results reported by Sabat et al.[9]implied that the anisotropy in recrystallization is remarkable during static annealing,where the rate of subgrain formation was enhanced in the grains of orientations>40° from the normal direction.The aforementioned researches mainly dealt with the operation of different deformation mechanisms and related fl w stresses during loading at a given temperature along different direction.Nevertheless,rare researches could be found in the literature that systematically study the anisotropy in deformation behavior and in development of DRX at different temperatures in wrought magnesium alloys.Such information can shed light on the challenges of the workability of magnesium alloys at high temperatures.Moreover,pre-existing twins have been shown,in recent years,that could considerably influ ence the slip and twinning activities during deformation of magnesium[5,17-20].Accordingly,the material anisotropy may be varied by the presence of pre-existing twins.Inplane deformation characteristics of rolled AZ31 alloy containing pre-existing twins were investigated at room temperature using in-situ electron backscatter diffraction technique(EBSD)[21].The results implied that pretwins gave rise to in-plane anisotropic activities of slips and twinning controlled the combined effect of the texture and effective grain size.

    Present work was aimed to investigate the evolutions of fl w stress as well as progression of DRX during compressive deformation along different directions of an AZ31 rolled alloy at a temperature range of 25-350 °C.The anisotropic characteristics were also evaluated after introducing pre-existing extension twins in the experimental material at the same conditions.

    2.Experimental procedure

    A commercial rolled AZ31 magnesium alloy(Mg-2.9Al-0.9Zn-0.7Mn,%wt.),with 22 mm thickness,was employed as the experimental alloy for this research.The as-received material was annealed for 1 h at 350 °C,after that it exhibited a fully recrystallized equiaxed microstructure without twins.The ND inverse pole figur(IPF)map of the initial material was given in Fig.1.The mean grain size was measured to be 45μm.Cylindrical compression samples with 10 mm diameter and 15 mm height were cut from annealed and pretwinned materials along rolling,transverse and normal directions,which hereafter are denoted as RD,TD,ND,respectively.Teflo tape was used as lubricant between the specimens and the anvils.The compression experiments were performed using GOTECH A17000 universal testing machine equipped with programmable resistance furnace.Before testing,the specimens were soaked for 5 min at the predetermined temperature to allow equilibration of temperature throughout the specimens.The experiments were conducted at the temperatures range of 25,150,250 and 350 °C under initial strain rate of 0.01 s-1.Each compression test was repeated at least three times with three different samples.The compression trials were programed to apply up to strain of 0.6.The stress-strain data was corrected for friction between the samples and compression anvils.To trace microstructure evolutions,some extra tests were conducted and interrupted at different strains,after that the specimens were quenched in water immediately.Sections parallel to the deformation axis were cut from the deformed specimens for metallographic investigations.The dynamically recrystallized grains could be almost readily distinguished from the pre-existing grains.The dynamically recrystallized grain size was determined utilizing a powerful image analyzing system.Scanning electron microscopy(SEM)investigations were conducted by utilizing scanning electron microscope(FEGSEM,FEI Quanta 3D)furnished with electron back scattered diffraction(EBSD)facility.

    To study the effect of pre-existing twins on the anisotropy of microstructural evolutions,precompression by strain of 6% was conducted on a part of annealed material along rolling direction.The magnitude of precompression was chosen according to the previous results[18,22],where it has been shown that 6% pstraining would produce a very high area fraction of twins.This could easily generate a high density of extension twins with 79% volume fraction.This yielded an effective mean grain size of 25μm(not presented here),considering initial grain boundaries as well as twin boundaries.The Series of compression tests along different directions as well as related microstructural investigations were performed for the material with pre-existing twins.

    Fig.1.IPF map of the microstructure of the initial annealed material.

    Fig.2.Pole figure of(0002),(10-10)and(11-20)planes of the initial experimental alloy.

    3.Results and discussion

    3.1.The effect of sample direction at different temperatures

    Rolled samples after the annealing treatment is characterized by basal texture with the c-axis aligned parallel to the ND and randomized a-axis in the rolling plane,as shown in Fig.2.Assuming the later major component,the orientation factor and thereby activation stress as well as the extent of contribution to plastic fl w for different slip systems may be assessed using the standard stereographic projection for magnesium[23].The Schmid factors were calculated for different slip and twinning mechanisms during loading along different directions and given in Table 1.CRSS values of 10,55,30,and 19 MPa are considered for basal slip,prismatic slip,{10-12}twinning,and{10-12}detwinning,respectively[24].

    The fl w curves of the experimental alloy deformed along different directions were plotted in Fig.3.Different shapes for the fl w curves,in terms of sigmoid trend,were observed for different directions up to 250 °C.At 25 and 150 °C,RD and TD samples show a rise in hardening rate at low strains,so called sigmodal hardening behavior,after that the hardening rate decreases.In contrast,the hardening rate of the ND sample at these temperatures is characterized with a monotonic decrease.However,it is interesting to note that a slight softening is realized in ND sample after reaching a peak stress at 150 °C.No softening regime could be distinguished in TD and RD samples.

    Table 1The absolute Schmid factor for different deformation mechanism during compression along different directions.

    RD samples locates basal planes parallel to the compression axis and this considerably reduces the contribution of basal slip.Thus,according to Table 1,the sample could be deformed at 25 and 150 °C primarily by twinning as well as prismatic slips.The{10-10}planes lie either perpendicular or at 30° with respect to the compression axis,where only the latter may contribute to a limited extent.Referring to Table 1,TD sample provides desired orientation for occurrence of extension twinning as well as prismatic slip.In agreement with the lower CRSS for twinning material fl w occurred at low stresses in RD and TD cases.At the late strains contraction twins with needle like morphology could be promoted in the work hardened material.The microstructures of the experimental alloy deformed along different directions at 150 °C are shown in Fig.4.A typical analysis for twin boundaries are presented in Fig.5 for the RD and TD samples,where boundaries corresponding to extension,contraction and double twins are showd in red,blue and green respectively..It is evident that the deformation of RD(and also TD)samples mainly is associated with the development of extension twinning.However,ND compression provides unfavorable orientation for extension twinning,and basal/prismatic slips.Therefore,the fl w stress is increased to activate non-basal slip,particularly〈c+a〉which assist in strain accommodating along c-axis.Owing to the high CRSS of nonbasal slip at low temperatures[25],the material hardenability is quickly exhausted and hardening rate dropped sharply.Thus,the critical stress for compression twins may be reached at low strain.Close observations indicated that localization of strain in the form of shear bands was developed in ND sample at late strains(Fig.4c),within which the occurrence of DRX within shear band might be triggered.Moreover,new grains may be geometrically generated through the intersection of compression twins.Thus,formation of shear regions,within which the deformation is localized,may also contribute to fl w softening in the ND sample at 150 °C.Though these evolutions led to the highest failure strain along ND,this could not provide enough hardenability to prevent cracking before targeted stain 0f 0.6.

    Fig.3.True stress-strain curves obtained during compressive deformation of the experimental alloy along different orientations at a)25,b)150,c)250 and d)350 °C.

    With increasing the temperature the CRSSs of basal slip and extension twinning remain relatively constant,while it decreases for non-basal slip systems in Mg[26],leading to substantial contribution of independent slip systems.Nonbasal slips are invoked for homogeneous deformation.Prismatic slip take a significan role at temperatures above beyond about 225 °C,while pyramidal slip may operates at temperature as high as 350 °C[10],although some previous works reported the activation of prismatic and second-order pyramidal slip at lower temperatures,due to compatibility stresses[27,28].Thus,the alteration of yield strength with temperature in the uniaxial loading is connected to the temperature dependence of the CRSS of the corresponding non-basal slip.Flow curves obtained at 250 °C show that the ND compression is still characterized with highest fl w stress.It is also surprising that a noticeable anisotropic behavior were obtained for RD and TD samples.The variation in the maximum anisotropy in yield and peak fl w stress of the material depicted in Fig.6.Accordingly,the anisotropy in fl w stress did not remarkably decrease with increasing temperature to 250 °C,while a sharp decrease in fl w stress anisotropy was realized as the temperature was raised to 350 °C.

    For ND samples,according to Table 1,the second-order pyramidal plane is favorably oriented for activation.However,according to their high CRSS slip systems,it can hardly operate during deformation at 250 °C.The latter condition may provide multiple slip activity only close to the prior grain boundaries,leading to rapid exhaustion of material hardenability and thereby the promotions of fl w localization.Hardening behavior of ND sample,shown in Fig.7,better illustrates a continuous drop in hardenability of material with increasing strain.This may end up crack initiation and premature fracture of the sample.Moreover,as the deformation starts remarkable scope for cross slip of prismatic dislocations may occur according to its high stacking fault energy(173 mJ/m2)[25].The occurrence of multiple slip and following dynamic recovery may render nucleation of new grains at the vicinity of prior grain boundaries.McQueen et al.[29]emphasized the role of nonbasal slip,in the formation of a 3D network of recrystallization nuclei.

    Fig.4.The microstructure of a)RD,b)TD and c)ND sample deformed at 150 °C.

    Fig.5.Grain boundary map of a)RD and b)ND samples deformed at 150 °C showing different twin boundaries including extension twin(86°),contraction twin(56°),double{10-11}-{10-12}twins delineated as red,blue and green color,respectively.

    For RD sample,the concave-up shape of the fl w curve represents that twinning,though at lower degree,yet take a respectful role during deformation of RD samples at 250 °C.Also,TD specimens present highly favorable orientation for prismatic slip and twinning,according to Table 1.The limited dynamic twinning could align the basal slip perpendicular to loading axis,resulting in a stage of work hardening,as obviously seen in Fig.7.The occurrence of twinning postponed the development of slip-dominated substructure preceding DRX nucleation.Therefore,the operation of prismatic slip as well as pyramidal slip could provide substructure condition for grain boundary nucleation of new grains at higher strains.Microstructure of the samples deformed along different directions at 250 °C were given in Fig.8.The evolutions of mean size and volume fraction of DRXed grains were given in Fig.9.It is evident that initial texture affect the DRX grain size and progression.Based on the author knowledge this is presented for the first-tim in magnesium alloys.Previous results[15,16]in these regards reported that initial texture does not have considerable effect on evolutions of DRXed microstructure.The largest grain size and DRX fraction at 250 °C were obtained after deformation of DR sample,while the minimum grain size and DRX fraction were obtained for ND one.The magnitude of the DRX fraction and fina grain size can be rationalized in terms of the effects of the various parameters on the nucleation and growth processes.Presumably,nucleation in magnesium is related to evolution of low angle boundary which,in turn,governed by climb and cross slip of nonbasal dislocations[28,30].Moreover,the deformation inhomogeneities may readily provide such nucleation conditions.However,growth rate of the nuclei,including diffusion of atoms to and from the adjacent grains,is controlled by driving force and mobility of grain boundary[31].Present results represent the lowest peak strain for ND direction,where,according to Table 1,just〈c+a〉slip with a high CRSS was favorable.However,it causes a more inhomogeneous deformation microstructure so that nucleation of new grains is triggered at pre-formed nuclei,i.e.areas with localized deformation.Recrystallization generally presents an incubation time,associated with the formation of a nucleus.Pre-existing nuclei are associated with a reduced DRX incubation time(and strain).Thus,it may be concluded that the initial texture-load orientationship,which stimulate inhomogeneous deformation such as ND compression,may promote the nucleation of DRX more quickly,than those facilitate the operation of different slip systems.The latter explanation is in line with the results reported on tension testing of AZ31 along different directions[32].They discussed that the activation of〈c+a〉slip render the occurrence of DRX because of their easy cross-slip and climb.However,nucleation of new grains during deformation along TD and RD invoke the time for the formation of a substructured nuclei with sufficien high mobility boundary.After the nucleus formation,recrystallization is controlled by growth,in which high angle grain boundaries migrate over the strained matrix(non-recrystallized),removing the crystalline defects until grains meet mutually.Major part of the energy spent during the deformation process is stored in the material in the form of dislocations.If the dislocation density during deformation(after nucleation)isρ,the driving force F is given by[33]:

    Fig.6.The evolution of work hardening rate ND,TD and RD sample at 250 °C.

    Fig.7.The variation of anisotropy in yield and peak fl w stresses of the experimental material with pre-existing twins at different temperatures.

    where G is the shear modulus and b is the modulus of the Burgers vector.Thus,promoted multiple slip activities in TD and RD samples gave rise to larger DRXed grain size and fraction.It should be noted that higher Schmid factor in TD sample for multiple slip may cause an extended dynamic recovery occurring concurrently with recrystallization,reducing the available dislocation density and thus driving pressure for DRX.This provide a rational base for the lower DRX fraction developed during deformation of TD sample compared to RD.Consistently,previous work has pointed out that potential for intensive recovery may lead to a lower DRX rate[31].Del Valle et al.[34]have discussed that the effect of texture on DRX evolution in Mg alloys during tensile test could be attributed to the strain necessary to development a basal fibe with〈01-10〉parallel to the tensile axis.While Li et al.[15]believed the influenc of initial texture on DRX is not connected with the changes in deformation mechanisms.

    At 350 °C,the anisotropy in fl w stress was significantl reduced,so that a yield and peak stress ratios of close to unity were achieved.The CRSSs for nonbasal slip systems decrease at higher temperatures[35],so that these may contribute more homogenously to deformation of samples with different orientation.Accordingly,the role of twinning is diminished at such high temperatures.The fina microstructures obtained after compression at 350 °C were illustrated in Fig.10.The size and fraction of DRX grains,given in Fig.9,indicate that anisotropy in DRX is almost vanished at 350 °C for RD and TD samples,while a lower DRX fraction(~60%)was observed after compression along ND.This is in agreement with the high strain required for achieving steady state stress in ND direction.The orientation relationship of the DRX grains formed at 350 °C with respect to the parent grains was also considered.Fig.11 and 12 depict the pole figure of(0002),(10-10)and(11-20)planes for DRXed and parent grains of the experimental alloy deformed along RD and ND samples,respectively.The results implied that DRXed grains adopted a texture corresponding to that of parent grains during deformation of AZ31 alloy along both RD and ND samples.

    Fig.8.The microstructure of a)RD,b)TD and c)ND sample deformed at 250 °C.

    Fig.9.Variations of DRX grain size and fraction and fl w stress softening during deformation along different direction at 250 and 350 °C.

    Fig.10.The microstructure of a)RD,b)TD and c)ND sample deformed at 350 °C.

    Fig.11.Pole figure of(0002),(10-10)and(11-20)planes for a)DRX grains,and b)parent grains of the experimental alloy deformed along RD at 350 °C.

    To further study the influenc of sample direction on the material fl w behavior,the fractions of fl w softening were calculated.The latter was performed through dividing the peak stress by the fl w stress attained at true strain of 0.5,which is the maximum strain experienced in all specimens.The values are given in Fig.9 as interconnecting blue points.As is commonly reported in FCC and BCC metals,the softening fraction tends to reduce with increasing temperature[34].Similarly,the present results implied that the softening fraction dropped with increasing temperature from 250 to 350 °C,which is related to more efficien dynamic recovery.As is seen in Fig.9,the softening characteristic has been significantl influence by the sample orientation.The highest softening fraction was obtained for ND sample at both 250 and 350 °C.The evolution of softening fraction may be discussed relying on the amount of heterogeneity and strain energy accumulated in the deformed material that would be substituted by new soft grains.In the case ND sample,the inhomogeneous deformation trigger the DRX at lower strain and thus recrystallization of the regions with high stored energy would lead to a more effective softening in the fl w stress.More interestingly,the results denote a significan discrepancies between the DRX fraction in the microstructure and softening fraction of the fl w stress.It is in contrast to the model usually used for calculating the DRX fraction,in which the DRX volume fraction is considered to be equal to softening fraction in fl w stress[36,37].Chen et al.[38]discussed that such inconsistency is related to the strengthening effects of new fin DRXed grains.Nevertheless,for the present results this is not the case,because the higher DRX volume fraction at 250 °C was obtained for RD sample while the highest softening fraction was obtained for ND direction.

    Fig.12.Pole figure of(0002),(10-10)and(11-20)planes for a)DRX grains,and b)parent grains of the experimental alloy deformed along ND at 350 °C.

    Beside drop in dislocation density,two main factors may further contribute to the fl w softening fraction.The firs is the strain energy of deformed material which would be substitutes by new soft grains.So,if there could be a dynamic recovery prior to DRX(concurrent to deformation)the strain energy of the deformed material would be lower,and thereby its substitution with new grain give rises to a lower softening fraction.The second is the possible effect of development of a texture.There may be different texture hardening/softening effects during substitution of different deformed textures by DRX one.

    3.2.Effect of pre-existing twins on anisotropic microstructural evolution

    To study the effect of initial twins on the anisotropy evolution of fl w stress and DRX,the deformation regimes employed for the material with pre-existing twins.The texture components developed in the pretwinned material are presented in Fig.13 as pole figure for(0002),(10-10)and(11-20)planes.As the twinning occurred through 86° rotation about one a-axes of HCP crystal,the c-axis is oriented close to RD while one of the prismatic plane is located almost inclined to the rolling plane.

    The fl w curves of the experimental alloy,with pre-existing twins were plotted in Fig.14.A close inspection of the curves implied that,in contrast to annealed material,TD and RD sample exhibited higher yield strength.Comparison of the curve appearance indicated that pretwins caused a remarkable changes in the shape of fl w curves,in terms of sigmoid trend,for ND samples at 25 and 150 °C.The pre-twinned ND samples show a rise in hardening rate at low strains,so called sigmodal hardening behavior,after that the hardening rate decreases.the maximum fl w stress ratios for yield and peak stress along different directions of the pretwinned material is given in Fig.15.It is interesting to note that the anisotropy in fl w stress has been remarkably reduced due to pre-existing twins.This is more pronounced at 250 °C.Using the main texture components,obtained in Fig.13,the values of Schmid factor for different deformation mechanisms in twinned area were given in Table 2.It should be noted that the twinned area provide relatively a higher orientation factors for deformation along ND directions which suffer from low Schmid factor in the untwinned areas.Therefore,it is rationalized that the twinned material(constituting both twinned and untwinned areas)exhibited less-anisotropic fl w stress.

    Fig.13.The pole figure of different planes of the pretwinned alloy.

    Fig.14.True stress-strain curves obtained during compressive deformation of the pretwinned experimental alloy along different orientations at a)25,b)150,c)250 and d)350 °C.

    According to Table 2,the pretwinned regions oriented caxis of the crystal perpendicular to the ND direction and thus prismatic slip as well as extension twinning may be activated in pretwinned areas.However,such reverse loading,relative to preloading,may also cause detwinning or shrinkage of pretwins so that the grains shear back to their initial twin-free state[39].Detwinning with low CRSS happens by the twin dislocations with an opposite sign in the twin along the twin boundaries[40].Detwinning is assisted by back stresses generated by twin growth[17].As the deformation progressed compression twin may also be formed leading to a premature fracture.It should be noted that the occurrence of detwinning,through dislocation interaction with twin boundaries,includes either dissociating into interfacial defects or penetrating(transmitting)into the twin[39].The latter interactions are accompanied with a strain hardening effect in the fl w curve of ND sample,corresponding to a sharp rise in hardening rate at 25 and 150 °C.For RD sample,the twinned areas provide a hard orientation for extension twinning and basal slip.The occurrence of{10-12}twinning and basal slip in untwined grain parts is also important in deformation.However,as the critical stress for slip and twinning increased due to Hall-Petch effect of pretwins,a greater fl w stress was developed for RD samples.Also,RD samples are expected to be deformed at low strains by the growth of pretwins.It has been determined that twin growth occurs under stresses lower than those required for new twin nucleation[41].As pretwins continuation is exhausted the fl w stress is rapidly increased,developing a high hardening rate.Growth of pretwins give rise to dominance of the texture component with c-axis parallel to RD.

    Table 2The absolute Schmid factor for different deformation mechanism in twinned area during compression along different directions.

    Fig.15.The evolution in anisotropy of yeild and peak fl w stresses of material with pre-existing twins at different temperatures.

    For TD samples,deformation at early deformation is governed by twinning in either pretwinned or untwined regions.The orientation of twinned regions is highly favorable for new twinning with variant different to that of pretwins.It should be noted that the occurrence of extension twinning in the narrow twinned area invoke a higher critical stress which further increase the yield strength through the Hall-Petch effect of pretwin boundaries.The prismatic slip direction lie either parallel or at 60° with respect to the compressive loading.Thus the latter orientation may contribute to prismatic slip.As the deformation is further progressed beyond yielding,the occurrence of basal and prismatic slips and then growth of pretwins provide respectful hardenability and gradual increase of fl w stress.The dominance of twin intersection justifie the greater yield stress in TD sample.

    Fig.16.The evolution of work hardening rate during compression along ND,TD and RD at 250 °C.

    With increasing the temperature the CRSSs of basal slip and extension twinning remain relatively constant,while it decreases for non-basal slip systems in Mg[26],leading to substantial contribution of independent slip systems.Nonbasal slips are invoked for homogeneous deformation.Prismatic slip take a significan role at temperatures beyond about 225 °C,while pyramidal slip may operates at temperature as high as 350 °C[10].Although,some previous works reported the activation of prismatic and second-order pyramidal slip at lower temperatures,due to compatibility stresses[27,28].Thus,the anisotropy of yield strength is connected to the different activated mechanisms.

    The shape of the fl w curves were changed by pretwins for all of the RD,TD and ND samples at 250 °C,denoting the alteration of dominant deformation mechanism at low strains.While a concave-up fl w curve behavior for ND sample at low strains was obtained.Fig.16 compares the hardening behaviors of the material with pre-twins during compression at 250 °C where a stage of strain hardening was realized for ND sample and a monotonic descending hardening rates observed for RD and TD samples.ND sample exhibited the lowest fl w stress.This is related to operation of basal,prismatic and firs order pyramidal slips and〈c+a〉slip in twined regions,though new extension twins may be also formed in the twinned areas.Thus,texture softening resulted by pretwins was the prominent factor during deformation along ND direction of the pretwinned material.The microstructural investigation at low strain implied that the occurrence of detwinning was hindered at 250 °C due to stabilizing the twins against shrinkage or growth at such high temperatures[42].Thus,the high hardening rate for ND sample at early strains can be related to persistence of pretwin boundaries as obstacles for dislocation glides.Moreover,as the deformation starts remarkable scope for cross slip of prismatic dislocations may occur according to its high stacking fault energy(173 mJ/m2)[25].

    For RD sample at 250 °C,in the untwinned regions the operation of new twinning as well as prismatic slip are hardened due to Hall-Petch effect of pretwins boundaries.The Schmid factor for contribution of slip system in the twinned area is very low.The growth of pretwins was also hindered at this temperature up to medium strain.So the yield strength of material was increased due to the pretwins.As the deformation progresses,the operation of nonbasal slip is facilitated at untwinned areas according to proper Schmid factor(see Table 2).Nevertheless,the effect of pretwins on work hardening of the material at low strain is not pronounced.However,pretwins hardening was significan during low strain deformation of ND sample.

    Fig.17.The microstructure of the experimental material with pre-existing twins deformed along a)RD,b)TD and c)ND at 250 °C.

    TD sample of the material with pre-existing twins presents a slip dominated shape of fl w curve.This is related to high Schmid factor for nonbasal slip(see Table 2),while extension twinning is hard to occur according to the Hall-Petch strengthening of pretwin boundaries.Thus,pretwins led to an increase in yield strength of TD sample at 250 °C due to higher CRSS of nonbasal slip.The contribution of different types of nonbasal slip and their following cross slip accelerated the microstructure evolution,preceding DRX nucleation.The occurrence of multiple slip and following dynamic recovery render nucleation of DRX at twin intersections,rather at the prior grain boundaries.Triggering of DRX is associated with a relatively low peak strain for TD sample.This caused the appearance of stress peak at lower strain,after that a gentle work softening trend is developed.

    Fig.18.Variations of DRXed grain size and fraction,and fl w stress softening during deformation along different direction at 250 and 350 °C.

    Microstructure of the samples deformed along different orientations at 250 °C were presented in Fig.17.The evolutions of mean size and volume fraction of DRXed grains were given in Fig.18.A relatively similar trend for evolution of size and fraction of DRXed grains is realized.Deformation along RD yielded the largest grain size and DRX fraction,while the minimum grain size and DRX fraction were obtained for ND and TD samples respectively.This observation is rationalized with high Schmid factor for slip in twinned areas of ND and both twinnwd and untwinned areas of TD,and resulting intensive dynamic recovery which limits the size of new grains.The lower softening fraction in pretwinned TD sample compared to RD is attributed to the extended recovery prior to DRX,considering the slip dominated fl w.Accordingly,a lower work hardening is developed before the peak stress,due to high Schmid factor for non-basal slips.This,in turn,may result in a lower softening ration in TD sample.

    Fig.19.(a,b)Quaternion misorientation graphs and(c and d)misorientation distributions of the material with pre-existing twins deformed at 250 °C along ND and RD,respectively.

    At 350 °C temperature,yield strength along different directions converge to about the same level.The CRSSs for nonbasal slip systems decrease at higher temperatures[35],so that they may contribute more homogenously to deformation of samples with different orientation.Accordingly,the contribution of twinning is diminished at such high temperatures.However,in case of pretwinned samples the stability of pretwins may be preserved at low strains leading to a minor anisotropy.The mean grain size and DRX fraction as well as the fl w softening fraction of the samples at 350 °C were included in Fig.18.Though the softening fraction was remarkably reduced at 350 °C,but there still is a slight anisotropy in the microstructure characteristics of the experimental material.Nevertheless,keeping in mind the overall microstructure evolutions one can infer that pretwins could mitigate anisotropy in microstructure evolutions in the experimental alloy.A slight increase in softening fraction with temperature in pre-twinned TD sample may be justifie considering the prevalence of non-basal slip in twinned and untwinned regions,where increasing the temperature to 350 °C can boost the activity of nonbasal slips with further straining.The latter may accelerate the progression of DRX and thereby greater fl w softening fraction.

    To explore more details of anisotropy in microstructure evolutions,EBSD analysis were performed for the pretwinned material deformed at 250 °C along ND and RD.Fig.19a and b display the quaternion misorientation figur relative to the typical as-rolled texture component(0002)<11-20>.In the present study,although there is a significan difference in deformation mechanisms and DRX progression,no distinct difference in fina texture was observed.The majority of deformed and DRXed grains tend to align perpendicular(~90°)to the〈a〉direction of basal planes.The latter observation together with necklace like DRX structure signify the dominance of discontinuous DRX mechanism[33].Boundaries corresponding to extension,contraction and double twin relationship can be traced by the relative frequencies around 86°,56° and 38° grain boundaries.Distribution axes for different twin-related misorientations were included in Fig.19.A higher frequency for low angle boundaries(2-15°)indicates the occurrence of more extended dynamic recovery,corresponding to higher average Schmid factor along RD.A frequency peak at 86° and related high misorientation axis density clustering at the〈11-20〉for ND and RD samples is observed while no noticeable extension twins with lenticular morphologies is seen.It suggests that a portion of the DRXed grains satisfy the twin orientation relationship,which is an evidence for active contribution of twin recrystallization.It can be also deduced that pretwins would retain after early deformation,which confir our speculation on the cessation of detwinning at 250 °C.Deformation along RD gave rise to development of distribution peak around 30°with the range of 20-50°.Moreover,the recrystallized regions contained abundant traces of 40° misoriented boundaries.However,the rotation axes of the 30-40° boundaries are mainly concentrated around〈0001〉,excluding the possibility of{10-11}-{10-12}double twinning related boundaries.Boundaries which satisfy 30°[0001]correspond to the areas of the dynamically recrystallized grains,indicating that the formation of the 30°[0001]misorientation is associated with dynamic recrystallization.The formation of this type of grain boundaries was explained as a result preferential nucleation and growth of the recrystallized grains[43].The higher mobility and stability due to specifi slip configuratio in this misorientation were also discussed that stabilize such boundaries[44].

    4.Conclusions

    ?A fl w softening was realized during deformation of ND sample at 150 °C,which is ascribed to formation of shear regions.

    ?The anisotropy in fl w stress did not remarkably decrease with increasing temperature to 250 °C,while a sharp decrease in fl w stress anisotropy was realized as the temperature was raised to 350 °C.

    ?The occurrence of twinning during deformation of RD and TD samples at 250 °C postponed the development of DRX and thereby fl w softening.

    ?The largest grain size and DRX fraction at 250 °C was obtained after deformation of DR.sample,while the minimum grain size and DRX fraction were obtained for ND one.

    ?Pre-existing twins could reduce the anisotropy of material in respect of fl w stress as well as DRX progression,where TD sample showed the lowest DRX fraction at 250 °C.

    ?A different misorientation distribution was realized after deformation of pretwinned material along ND and RD directions.

    Acknowledgment

    This work was supported in part by the National Science Center(Poland)under grant No.2018/31/B/ST8/00942.

    久久精品国产鲁丝片午夜精品| 欧美另类一区| 国产精品一区二区性色av| 久久久久久久久久成人| h日本视频在线播放| 中文字幕av成人在线电影| 国产精品av视频在线免费观看| 九色成人免费人妻av| 亚洲国产最新在线播放| 极品教师在线视频| 国产色婷婷99| 少妇高潮的动态图| 久久99精品国语久久久| 久久久国产一区二区| 好男人视频免费观看在线| 一级黄片播放器| 七月丁香在线播放| 这个男人来自地球电影免费观看 | 国产日韩欧美亚洲二区| a级一级毛片免费在线观看| 欧美高清成人免费视频www| 国产精品国产av在线观看| av线在线观看网站| 亚洲图色成人| videos熟女内射| 在线观看免费视频网站a站| 联通29元200g的流量卡| 人妻一区二区av| 欧美激情国产日韩精品一区| 亚洲最大成人中文| 99re6热这里在线精品视频| 伦精品一区二区三区| 国产在线视频一区二区| 成人亚洲欧美一区二区av| 伊人久久精品亚洲午夜| 成人高潮视频无遮挡免费网站| 伦理电影大哥的女人| 91久久精品电影网| 99久久中文字幕三级久久日本| 久久 成人 亚洲| 狂野欧美白嫩少妇大欣赏| 欧美丝袜亚洲另类| 下体分泌物呈黄色| 欧美精品亚洲一区二区| 建设人人有责人人尽责人人享有的 | 国产精品三级大全| 午夜福利在线在线| 永久网站在线| 午夜福利在线在线| 菩萨蛮人人尽说江南好唐韦庄| 国国产精品蜜臀av免费| 久久6这里有精品| 国产精品嫩草影院av在线观看| 热99国产精品久久久久久7| 天堂俺去俺来也www色官网| 国产日韩欧美亚洲二区| 亚洲精品中文字幕在线视频 | 大码成人一级视频| 免费av中文字幕在线| 91在线精品国自产拍蜜月| 2021少妇久久久久久久久久久| 涩涩av久久男人的天堂| 伊人久久精品亚洲午夜| 国内揄拍国产精品人妻在线| 春色校园在线视频观看| 国产淫语在线视频| 自拍偷自拍亚洲精品老妇| 国国产精品蜜臀av免费| 91精品国产九色| 人妻制服诱惑在线中文字幕| av免费在线看不卡| 精品人妻熟女av久视频| 小蜜桃在线观看免费完整版高清| 久久99精品国语久久久| 大片免费播放器 马上看| av黄色大香蕉| 人体艺术视频欧美日本| 国国产精品蜜臀av免费| 欧美 日韩 精品 国产| 看免费成人av毛片| 亚洲一级一片aⅴ在线观看| 国产精品久久久久成人av| 国产一区有黄有色的免费视频| 日本-黄色视频高清免费观看| 一级毛片 在线播放| 美女cb高潮喷水在线观看| 久久国产精品男人的天堂亚洲 | 国产无遮挡羞羞视频在线观看| 91精品一卡2卡3卡4卡| 在线观看免费日韩欧美大片 | 成人影院久久| 中文字幕制服av| 久久女婷五月综合色啪小说| 七月丁香在线播放| 男人和女人高潮做爰伦理| 成人一区二区视频在线观看| 欧美日韩在线观看h| 最近中文字幕高清免费大全6| 中文字幕亚洲精品专区| 天堂中文最新版在线下载| 九色成人免费人妻av| 亚洲欧美日韩另类电影网站 | 精品久久久久久久久av| 男人狂女人下面高潮的视频| 久久久久国产网址| www.色视频.com| 国产在视频线精品| 亚洲精华国产精华液的使用体验| 成人国产麻豆网| 欧美成人一区二区免费高清观看| av视频免费观看在线观看| 免费高清在线观看视频在线观看| 六月丁香七月| 日本欧美视频一区| 国产午夜精品久久久久久一区二区三区| 综合色丁香网| 新久久久久国产一级毛片| 永久网站在线| 黄色怎么调成土黄色| 成年av动漫网址| 九九在线视频观看精品| 亚洲精品国产色婷婷电影| 久久精品久久久久久久性| 大香蕉久久网| 2018国产大陆天天弄谢| 久热久热在线精品观看| 身体一侧抽搐| 日本av手机在线免费观看| 99热这里只有精品一区| 亚洲av欧美aⅴ国产| 在线观看国产h片| 男人狂女人下面高潮的视频| 三级国产精品欧美在线观看| 久久99热这里只频精品6学生| 国产深夜福利视频在线观看| 中文天堂在线官网| 日日摸夜夜添夜夜爱| 极品少妇高潮喷水抽搐| 亚洲欧美日韩另类电影网站 | 国产男人的电影天堂91| 免费看日本二区| 大陆偷拍与自拍| 欧美精品国产亚洲| 久久99热6这里只有精品| 夜夜爽夜夜爽视频| kizo精华| 黄色日韩在线| 日本与韩国留学比较| a级毛片免费高清观看在线播放| 国产人妻一区二区三区在| 国产色爽女视频免费观看| 黑丝袜美女国产一区| 99久久精品热视频| 一边亲一边摸免费视频| 欧美xxxx黑人xx丫x性爽| 在线免费观看不下载黄p国产| 女的被弄到高潮叫床怎么办| 国产av一区二区精品久久 | 成人毛片60女人毛片免费| 亚洲内射少妇av| 热re99久久精品国产66热6| 成人免费观看视频高清| 黑人猛操日本美女一级片| 晚上一个人看的免费电影| 大陆偷拍与自拍| 欧美少妇被猛烈插入视频| 嘟嘟电影网在线观看| 成人亚洲欧美一区二区av| 夫妻午夜视频| 精品人妻一区二区三区麻豆| 国产黄频视频在线观看| 六月丁香七月| 国产毛片在线视频| 亚洲精品乱久久久久久| 欧美成人精品欧美一级黄| 在线天堂最新版资源| 成人特级av手机在线观看| 搡女人真爽免费视频火全软件| 能在线免费看毛片的网站| 日韩欧美一区视频在线观看 | 少妇裸体淫交视频免费看高清| 久久精品国产鲁丝片午夜精品| 91久久精品电影网| 久久6这里有精品| 国产免费又黄又爽又色| 又大又黄又爽视频免费| 最近的中文字幕免费完整| 国产在线视频一区二区| 亚洲国产欧美人成| 中文在线观看免费www的网站| 午夜日本视频在线| 久久国内精品自在自线图片| 精品酒店卫生间| 777米奇影视久久| 一级av片app| 肉色欧美久久久久久久蜜桃| 深爱激情五月婷婷| av专区在线播放| 亚洲成人中文字幕在线播放| 日韩 亚洲 欧美在线| 大香蕉久久网| 美女xxoo啪啪120秒动态图| 伊人久久国产一区二区| 欧美日韩在线观看h| 国产精品久久久久成人av| 国产伦在线观看视频一区| 丰满人妻一区二区三区视频av| 久久精品国产亚洲网站| 午夜福利网站1000一区二区三区| 91精品伊人久久大香线蕉| 国产欧美日韩精品一区二区| 亚洲一级一片aⅴ在线观看| 美女高潮的动态| 你懂的网址亚洲精品在线观看| 国产精品精品国产色婷婷| av黄色大香蕉| 深夜a级毛片| 99久国产av精品国产电影| 亚洲久久久国产精品| 亚洲国产欧美在线一区| 欧美 日韩 精品 国产| 国产精品一区二区性色av| 亚洲色图综合在线观看| 日日摸夜夜添夜夜添av毛片| 亚洲自偷自拍三级| 亚洲精品中文字幕在线视频 | 各种免费的搞黄视频| 国产精品人妻久久久影院| av天堂中文字幕网| 在线观看三级黄色| 少妇熟女欧美另类| 五月开心婷婷网| 亚洲精品色激情综合| 在线免费观看不下载黄p国产| 高清视频免费观看一区二区| av播播在线观看一区| 久久国产亚洲av麻豆专区| 在线观看人妻少妇| 2022亚洲国产成人精品| 日韩成人av中文字幕在线观看| 久久精品国产亚洲av天美| 免费观看av网站的网址| 丰满乱子伦码专区| 91狼人影院| 97在线视频观看| 久久精品国产a三级三级三级| 中文天堂在线官网| 国产亚洲精品久久久com| 亚洲在久久综合| 国产精品免费大片| av黄色大香蕉| 在线观看一区二区三区| 男人狂女人下面高潮的视频| 日产精品乱码卡一卡2卡三| 国产精品久久久久成人av| 久久久久国产网址| 综合色丁香网| kizo精华| 大码成人一级视频| 老师上课跳d突然被开到最大视频| av在线观看视频网站免费| 久久久色成人| 国产精品久久久久久久电影| 六月丁香七月| 国产精品.久久久| 成人漫画全彩无遮挡| 99热这里只有是精品50| 久久精品久久久久久噜噜老黄| 99热6这里只有精品| 插逼视频在线观看| 日韩成人av中文字幕在线观看| 秋霞伦理黄片| av免费在线看不卡| 国产乱人偷精品视频| 欧美日韩视频精品一区| 久久精品久久久久久久性| 亚洲av二区三区四区| 国产成人精品婷婷| 天堂俺去俺来也www色官网| 国产精品一区二区在线观看99| 亚洲自偷自拍三级| 少妇熟女欧美另类| 女性生殖器流出的白浆| 五月玫瑰六月丁香| 亚洲va在线va天堂va国产| 青春草视频在线免费观看| 国产爱豆传媒在线观看| 亚洲国产精品一区三区| 国产精品久久久久久精品古装| 久久国产精品大桥未久av | 日日摸夜夜添夜夜爱| 久久亚洲国产成人精品v| 九色成人免费人妻av| 精品亚洲成国产av| 久久久久久伊人网av| 如何舔出高潮| 91aial.com中文字幕在线观看| 国产美女午夜福利| 久久久久久九九精品二区国产| 美女cb高潮喷水在线观看| 亚洲成色77777| 精品少妇久久久久久888优播| 小蜜桃在线观看免费完整版高清| 久久久国产一区二区| 免费黄频网站在线观看国产| 丰满人妻一区二区三区视频av| 欧美高清性xxxxhd video| 国产一区二区三区av在线| 狂野欧美白嫩少妇大欣赏| 国产精品一区二区性色av| 能在线免费看毛片的网站| 五月开心婷婷网| 视频中文字幕在线观看| 伦精品一区二区三区| 国产精品爽爽va在线观看网站| 男女无遮挡免费网站观看| 亚洲av男天堂| 老师上课跳d突然被开到最大视频| 亚洲av成人精品一二三区| 欧美丝袜亚洲另类| 一区二区三区精品91| 亚洲人与动物交配视频| 亚洲精品自拍成人| 97精品久久久久久久久久精品| 亚洲欧美精品自产自拍| 五月天丁香电影| 你懂的网址亚洲精品在线观看| 亚洲成人手机| 一个人看的www免费观看视频| av国产精品久久久久影院| 日韩在线高清观看一区二区三区| 国产视频首页在线观看| 熟女av电影| a级毛片免费高清观看在线播放| 国产淫语在线视频| 多毛熟女@视频| 大又大粗又爽又黄少妇毛片口| 我的女老师完整版在线观看| 最近最新中文字幕大全电影3| 美女国产视频在线观看| 亚洲av在线观看美女高潮| 日韩伦理黄色片| 如何舔出高潮| 日韩精品有码人妻一区| 直男gayav资源| 国产精品av视频在线免费观看| 在线亚洲精品国产二区图片欧美 | 亚洲av日韩在线播放| 中文字幕精品免费在线观看视频 | 在线免费观看不下载黄p国产| 男的添女的下面高潮视频| 久久久久网色| 成人毛片a级毛片在线播放| 久久国内精品自在自线图片| av在线蜜桃| 色婷婷久久久亚洲欧美| av网站免费在线观看视频| 女性被躁到高潮视频| 日本-黄色视频高清免费观看| 成年av动漫网址| 成人黄色视频免费在线看| 干丝袜人妻中文字幕| 中文欧美无线码| 麻豆精品久久久久久蜜桃| 午夜日本视频在线| 建设人人有责人人尽责人人享有的 | www.色视频.com| 99久久人妻综合| 久久99热这里只有精品18| 国产在线一区二区三区精| 99久久精品热视频| av在线老鸭窝| 一级片'在线观看视频| 男人添女人高潮全过程视频| 欧美国产精品一级二级三级 | 这个男人来自地球电影免费观看 | 亚洲欧美一区二区三区国产| 国产极品天堂在线| 亚洲av综合色区一区| 国产精品无大码| 超碰97精品在线观看| 亚洲熟女精品中文字幕| 精品99又大又爽又粗少妇毛片| 少妇被粗大猛烈的视频| av黄色大香蕉| 欧美精品国产亚洲| 午夜免费男女啪啪视频观看| 偷拍熟女少妇极品色| 99国产精品免费福利视频| 久久精品久久精品一区二区三区| 亚洲成色77777| 日韩欧美精品免费久久| 人妻夜夜爽99麻豆av| 简卡轻食公司| 自拍偷自拍亚洲精品老妇| 亚洲av综合色区一区| 哪个播放器可以免费观看大片| 特大巨黑吊av在线直播| 日本vs欧美在线观看视频 | 日本黄大片高清| 在线免费十八禁| 天天躁夜夜躁狠狠久久av| 国产中年淑女户外野战色| freevideosex欧美| 晚上一个人看的免费电影| 久久久久精品久久久久真实原创| 精品亚洲成a人片在线观看 | 国产成人一区二区在线| 欧美zozozo另类| 久久国产精品大桥未久av | 国产色婷婷99| 国产精品三级大全| kizo精华| 久久 成人 亚洲| 亚洲成人av在线免费| 18禁裸乳无遮挡免费网站照片| 欧美xxⅹ黑人| 狂野欧美白嫩少妇大欣赏| 国产精品国产三级专区第一集| 国产无遮挡羞羞视频在线观看| 美女主播在线视频| 中文在线观看免费www的网站| xxx大片免费视频| a级一级毛片免费在线观看| 中国国产av一级| 国产一区二区三区综合在线观看 | 中文字幕av成人在线电影| 亚洲精品成人av观看孕妇| 国产精品福利在线免费观看| 欧美 日韩 精品 国产| 国产伦精品一区二区三区视频9| 尤物成人国产欧美一区二区三区| 自拍欧美九色日韩亚洲蝌蚪91 | 汤姆久久久久久久影院中文字幕| 久久久久久久大尺度免费视频| 少妇人妻久久综合中文| 日韩视频在线欧美| 亚洲av电影在线观看一区二区三区| 伊人久久精品亚洲午夜| 亚洲国产最新在线播放| 国产爱豆传媒在线观看| 婷婷色av中文字幕| 菩萨蛮人人尽说江南好唐韦庄| 亚洲国产毛片av蜜桃av| 欧美国产精品一级二级三级 | av国产免费在线观看| 九九爱精品视频在线观看| 十分钟在线观看高清视频www | 日本黄色日本黄色录像| 精品久久久久久久末码| 日韩欧美 国产精品| 国产精品国产三级国产专区5o| 国产 一区精品| 久久久久久人妻| 一本色道久久久久久精品综合| 一级毛片aaaaaa免费看小| 青春草亚洲视频在线观看| 岛国毛片在线播放| 中文字幕精品免费在线观看视频 | 九九爱精品视频在线观看| 久久久久视频综合| 91精品一卡2卡3卡4卡| 高清不卡的av网站| 午夜福利在线观看免费完整高清在| 久久久久精品性色| 久久久亚洲精品成人影院| 超碰97精品在线观看| 一区二区av电影网| 精品一品国产午夜福利视频| 日本爱情动作片www.在线观看| 看十八女毛片水多多多| 女性被躁到高潮视频| 自拍偷自拍亚洲精品老妇| 亚洲精品乱码久久久v下载方式| 精品午夜福利在线看| 另类亚洲欧美激情| 午夜福利视频精品| 纵有疾风起免费观看全集完整版| 天堂俺去俺来也www色官网| 一区二区av电影网| 久久这里有精品视频免费| 日韩成人av中文字幕在线观看| av福利片在线观看| 国产精品一区www在线观看| 国产 一区精品| 中文在线观看免费www的网站| 多毛熟女@视频| 亚洲国产日韩一区二区| 亚洲av免费高清在线观看| 亚洲精品,欧美精品| 直男gayav资源| 日本猛色少妇xxxxx猛交久久| 高清视频免费观看一区二区| 一本久久精品| 久久久午夜欧美精品| 国产91av在线免费观看| 亚洲内射少妇av| 精品少妇黑人巨大在线播放| 美女cb高潮喷水在线观看| freevideosex欧美| 日日啪夜夜爽| 亚洲精品国产色婷婷电影| 看十八女毛片水多多多| 国产 精品1| 观看av在线不卡| tube8黄色片| 狂野欧美激情性xxxx在线观看| 看十八女毛片水多多多| 乱系列少妇在线播放| 少妇被粗大猛烈的视频| 国产淫语在线视频| 久久6这里有精品| 高清黄色对白视频在线免费看 | 久久精品国产亚洲av涩爱| 丰满少妇做爰视频| 久久久午夜欧美精品| 直男gayav资源| 一级毛片电影观看| 波野结衣二区三区在线| 水蜜桃什么品种好| 久久精品久久久久久噜噜老黄| 青春草视频在线免费观看| 精品少妇久久久久久888优播| av.在线天堂| 欧美丝袜亚洲另类| 中国三级夫妇交换| 国产毛片在线视频| 高清欧美精品videossex| 国产黄频视频在线观看| 国产色爽女视频免费观看| 一级二级三级毛片免费看| 插逼视频在线观看| 久久精品久久久久久久性| 中国三级夫妇交换| 欧美+日韩+精品| 免费观看的影片在线观看| 黄片无遮挡物在线观看| 国产成人精品一,二区| 黄色怎么调成土黄色| 寂寞人妻少妇视频99o| 91精品国产九色| 啦啦啦在线观看免费高清www| 国产在线视频一区二区| 麻豆成人午夜福利视频| 少妇丰满av| 久久久精品免费免费高清| 久久 成人 亚洲| 国产乱人视频| 亚洲图色成人| 国产成人a∨麻豆精品| 男女啪啪激烈高潮av片| 久久久久久久久久久丰满| 国产高清国产精品国产三级 | 亚洲精品成人av观看孕妇| 日本vs欧美在线观看视频 | 亚洲熟女精品中文字幕| 男人添女人高潮全过程视频| 国产免费视频播放在线视频| 男女边摸边吃奶| 极品少妇高潮喷水抽搐| 久久人人爽av亚洲精品天堂 | 国产黄色视频一区二区在线观看| 国产精品秋霞免费鲁丝片| 国产av一区二区精品久久 | 国产成人精品福利久久| 亚洲欧美一区二区三区国产| www.色视频.com| 久久av网站| 日韩亚洲欧美综合| 免费播放大片免费观看视频在线观看| 国产日韩欧美在线精品| 校园人妻丝袜中文字幕| 亚洲av欧美aⅴ国产| 亚洲av在线观看美女高潮| 在线观看国产h片| 日本-黄色视频高清免费观看| 晚上一个人看的免费电影| 国产亚洲午夜精品一区二区久久| 亚洲成色77777| 韩国高清视频一区二区三区| 777米奇影视久久| 女性生殖器流出的白浆| 人妻系列 视频| 亚洲一级一片aⅴ在线观看| 不卡视频在线观看欧美| 国产精品一区www在线观看| 精品一区二区免费观看| 伦精品一区二区三区| 精品一区二区三区视频在线| 九九久久精品国产亚洲av麻豆| 亚洲无线观看免费| 色婷婷久久久亚洲欧美| 国产精品秋霞免费鲁丝片| 尾随美女入室| 精品一区二区三区视频在线| 久久99热这里只有精品18| 伦精品一区二区三区| 下体分泌物呈黄色| 日日撸夜夜添| 一个人看视频在线观看www免费| 乱系列少妇在线播放| 99久久中文字幕三级久久日本| 亚洲欧美日韩东京热| 精品人妻熟女av久视频| av免费在线看不卡| 黄色配什么色好看| 午夜激情福利司机影院| 亚洲自偷自拍三级| h日本视频在线播放| 热re99久久精品国产66热6| 麻豆国产97在线/欧美| 最近中文字幕2019免费版| 欧美成人精品欧美一级黄| 精品一区在线观看国产| 国产成人精品久久久久久|