    CNT toughened aluminium and CFRP interface for strong adhesive bonding

    2022-10-09 07:25:18GngHnBoTnFiChngBinhuWngKwongLongXiozhiHu
    Namo Materials Science 2022年3期

    Gng Hn ,Bo Tn ,Fi Chng ,Binhu Wng ,Y-Kwong Long ,Xiozhi Hu,*

    a Department of Mechanical Engineering,University of Western Australia,Perth,WA,6009,Australia

    b Department of Chemical Engineering,University of Western Australia,Perth,WA,6009,Australia

    c Shaoxing Baojing Composite Materials Co.,Ltd,Shaoxing,312073,PR China

    d School of Materials Science and Engineering,Southwest University of Science and Technology,Mianyang,621000,PR China

    e Key Laboratory of Road Construction Technology and Equipment,MOE,Chang'an University Xi'an,710064,PR China

    Keywords:Shear bond strength Interfacial toughening CNT Resin pre-coating (RPC)Chemical surface treatment Aluminium/CFRP Laminate

    ABSTRACT This study presents a simple technique for strengthening the adhesive-bond strength between aluminium (Al)substrate and carbon fibre reinforced polymer (CFRP) utilising resin pre-coating (RPC) with carbon nanotubes(CNTs).The CNT-containing RPC solution with 90 wt%acetone and 10 wt%resin(without hardener)was applied onto Al substrates,where micro-/nano-vertical channels had been created by chemical or mechanical surface treatments to accommodate CNTs.RPC was able to fill all micro-/nano-cavities over the Al substrate surface,then CNTs were pulled into those vertical micro-channels by the capillary action generated from acetone evaporation.Normal epoxy adhesive (resin +hardener) was applied after the CNT-containing RPC treatment.CNTs bridging across the interface between the adhesive joint and Al substrate and sealing of micro-/nano-cavities by RPC effectively enhanced the interfacial shear bond strength between the Al substrate and CFRP by 30–100%depending on the Al substrate surface profiles.Al substrates with two different chemical treatments were compared in this study for the effectiveness of CNT interfacial reinforcement.Results from a steel substrate after sandblasting were also included for comparison.

    1.Introduction

    Carbon nanotube(CNT)as a key focus of nano-materials science has been studied for many years[e.g.[1,2]].Nowadays,it is expected to see more and more industrial applications of this unique nano-material.CNT typically with a nano-sized diameter and micro-scale length from 1 to 10 μm is a perfect choice for strengthening narrow adhesive joints between carbon-fibre reinforced polymers(CFRP)and aluminium(Al)alloy substrates,and interfaces in laminar CFRP structures commonly employed in the aviation and automotive industries[3].

    The relatively weak interface between the Al substrate and ultra-thin adhesive joint (followed by CFRP) is always a concern for the adhesive bond strength of Al/CFRP structures.Typical epoxy adhesive bonding between Al and CFRP may involve different substrate preparations(cleaning,chemical treatment,sandblasting or primer coating),followed by the final adhesive bonding.While the interfacial bond strength has been improved by those commonly used substrate preparation methods,the reality is that there is still no“Z-direction”reinforcement across the interface between the Al substrate and adhesive joint.It is perceivable fibre bridging across the interface between the Al substrate and adhesive joint will be beneficial for eliminating any potential premature adhesive failure along the interface.Particularly,it has been proven that Z-pin and stitching [e.g.[4–6]] are effective against delamination or interfacial cracking in laminar CFRP.Although Z-pin and stitching cannot be adopted directly for adhesive bonding between Al and CFRP,quasi-Z-directional fibre bridging against interfacial cracking can still be realised by suitable substrate preparations.Keeping the simplicity of common adhesive bonding,this study explores a plausible technique for interfacial fibre bridging or CNT “Z-pin” in conjunction with pre-made micro-/nano-sized cavities or channels in Al substrates using either chemical or mechanical methods [7–9].

    The simple CNT-containing resin pre-coating (RPC) technique,presented in this study,can be conveniently applied in any laboratory for small test samples and adopted on-site for large structures after chemical or mechanical preparations of substrates.This simple and quick intermediate RPC step is beneficial as it does not cause any noticeable delay and complication for the process of adhesive bonding.Yet,the shear bond strength has been consistently increased by 30%–100%,depending on the substrate surface profiles.In this study,Al substrates prepared by two different chemical treatments and a steel substrate prepared by sandblasting are used to confirm the CNT-PRC adhesive bonding method.

    Fig.1.(a)Top view of chemically treated Al(CHEM1)substrate surface with vertical channels.The viscous epoxy adhesive may not fill in the micro-cavity tips.(b)FIB exposed the side view,showing depths of the vertical channels are around 10–20 μm,and the micro-channels have been filled all the way to the tips by the unique RPC process.

    2.CNT “Z-pins” across Al substrate with micro-channels positioned by capillary action

    2.1.CNT dispersion in resin pre-coating (RPC) solution

    For practical applications of CNTs interfacial toughening for strong adhesive bonding,the following three conditions need to be satisfied.(1)There should be a simple method for CNT dispersion,which can be carried out with minimum equipment requirements and could be easily adopted on-site.(2)Applications of CNT for adhesive bonding should be simple so that engineers without any special research skills can still use the well-studied nano-material for real structures.(3) CNT toughening has to be noticeably effective,e.g.,consistently improving the adhesive bond strength by at least 20–50% or higher,whether it is done by an experienced researcher in the laboratory or a practical engineer working on site.This study intends to provide tentative solutions for the above three conditions.

    Firstly,the dispersion of CNT in an acetone-diluted resin solution(e.g.90 wt% of acetone and 10 wt% of resin without hardener) is simple,which can be done by simple mechanical stirring for a few minutes.A“perfect CNT dispersion” in this resin pre-coating (RPC) solution is unnecessary for common adhesive bonding,so 5–10 min of mechanical dispersion is more than sufficient.Furthermore,the CNT-containing RPC solutions can be pre-made and tailored for specific requirements.Acetone evaporation from the CNT-containing RPC solution is fast,and the mechanical properties of the remaining resin are not affected[10].

    Secondly,the CNT-containing acetone-rich RPC solution can be conveniently coated over Al substrates through either spraying or brushing.That is instead of mixing CNT in a viscous epoxy adhesive(resin and hardener mixture),the CNT-coating or distribution over the Al substrate surface is done using the low viscous RPC solution(90 wt%of acetone and 10 wt%of resin without hardener).The RPC process has two distinct roles;(1)to fill all micro-/nano-surface and sub-surface cavities and channels and wet the entire substrate surface,and (2) to pull CNT into those micro-channels from the capillary action during the acetone evaporation process.Note that the RPC solution contains 90 wt%acetone and only 10 wt%resin.

    Thirdly,it has been tested and confirmed that even RPC by itself is effective for the adhesive bond strength improvement for metal substrates with various surface conditions[11–13].Fibre bridging from CNT just makes the RPC method even more effective for additional bond strength improvement [8,9].All the relevant studies on adhesive bond strengths with various substrates show that the interfacial bonding strength improvements are at least around 30% or higher.Considering CNT-coating over Al substrates can be easily done using the RPC solution,the proposed CNT-containing RPC method is simple,beneficial and fully justified in applications.

    Fig.2.(a)original surface,and then(b)and(c)Top view of phosphoric acid anodised Al(CHEM2)with porous structures with 50–200 nm diameters.Based on the micro-surface features,CNT “Z-pins” are most likely less effective for CHEM2 in comparison to CHEM1.

    Fig.3.Height profiles of CONTROL,CHEM1 and CHEM2,where the maximum x-scale range =1000 μm and maximum y-scale range =40 μm.

    It should also be mentioned that it has been proven mathematically that fibre bridging can still be effective against the opening mode(Mode-I) crack propagation in CFRP even if short or micro-length fibres at the ply interface are not perpendicular to the crack face[14].For shear bond strengths(Mode-II),perfectly vertical“Z-pins”are even less important,or necessary.As long as the micro-cavities are deep enough to accommodate CNT“Z-pins”,creating perfectly vertical micro-/nano-channels on the Al substrates is not required.

    2.2.Two Al substrates prepared by two different chemical treatments

    To concentrate on the effectiveness of CNT interfacial toughening,three different surface profiles(Al substrates with two different chemical treatments,and one steel substrate with sandblasted surface finish) are examined and compared in this study.That is the main emphasis of this study is on the surface microstructures and their effects on CNT interfacial toughening.

    Two chemical treatments of the Al substrate (6060 T5 aluminium),sulfuric acid,sulfuric acid-oxalic acid and sulfuric acid-oxalic acid-iron sulphate(CHEM1)[15]in Fig.1,and phosphoric acid electrolyte(20 wt%) (CHEM2) in Fig.2 are considered in this study.The material details and detailed chemical treatment process are described in Section 3.

    The top surface view of the CHEM1 treated Al substrate surface is shown in Fig.1(a),and the side surface exposed by focus ion beam(FIB)is shown in Fig.1(b).The depth of those vertical channels varies from around 10 to 20 μm while their tip width is around 1 μm.That is those micro-channels are big enough to accommodate various CNTs with diameters from 10s of nano-meters(typical multi-wall CNT)to one or two hundred nano-meters (e.g.helical CNT).The top outer alumina surface layer of the chemically-treated Al substrate is strong,so the surface features are perfect for accommodating potential CNT“Z-pins”.It should be mentioned that the tips of those micro-channels have been filled completely by the epoxy adhesive using the RPC process as shown in Fig.1 (b),while this may not be possible with direct applications of regular viscous epoxy adhesives.

    The surface profile from CHEM2 in Fig.2 is very different to that in Fig.1.Instead of deep vertical micro-channels,the surface features in Fig.2 are fairly smooth but having many micro-/nano-pore structures.Those shallow micro-/nano-pore structures from CHEM2 vary between 50 and 500 nm,which may not be as effective as CHEM1 surface features as far as vertical CNT Z-pins are concerned.Clearly,the differences in the surface profiles between the Al substrates in Figs.1 and 2 can provide useful information on the effectiveness of CNT interfacial toughening within the epoxy adhesive joint.

    Surface variations or height differences of peak valley (Pt) for different Al surfaces,including CONTROL,anodised by CHEM1 and CHEM2,are measured and shown in Fig.3.The height difference for the untreated Al is 11.55 μm while it is 18.78 μm for CHEM1 and 14.28 μm for CHEM2,respectively.It is more meaningful to consider those Pt numbers in Fig.3 together with the local surface conditions,i.e.whether the peaks and deepest valleys are close to each other.If they are close to each other as for the CHEM1 condition,it is more likely to put CNT Z-pins into those vertical micro-channels.

    Fig.4.(a)For comparison,a normal sandblasted steel surface[16],and(b)all micro-cavities have been filled after RPC.The substrate wettability is improved since the surface remains wet (thin resin coating only and no hardener).Air entrapment in sub-surface micro-cavities is avoided in final adhesive bonding.

    Fig.5.(a) CNT was well dispersed in RPC solution around 1 wt% (compared to the net resin).All surface-modified metals,including anodised Al and sandblasted steel,were soaked into CNT-containing RPC solution for 30s.(b) The CNT-containing RPC solution is applied onto the chemically treated Al substrate surface.During the process of acetone evaporation,CNTs are pulled into the microchannels.Standard epoxy adhesive(resin +hardener) is applied on the Al substrate normally for adhesive bonding.(c)The CNT-containing RPC solution can also be applied onto a sandblasted Al substrate with micro-cavities for similar CNT-bridging effects along the interface between the Al substrate and adhesive joint.Broken sand particles embedded in the metal substrate are also fully coated by the RPC process.

    For comparison,a mild steel substrate with a sandblasted surface finish[16]is shown in Fig.4(a).The smooth surface in Fig.4(b)is“wet”,covered by the ultra-thin resin coating left by the RPC process.Changing the acetone/resin ratio,e.g.from the current 90 wt%acetone and 10 wt%resin to 95 wt% acetone and 5 wt% resin,will produce a thinner resin coating after the complete evaporation of acetone.However,as exposed by the FIB micrograph in Fig.1(b),the most important RPC feature underneath the smooth surface of Fig.4 (b) is that all micro-cavities have been filled by resin,and there are no micro-air pockets even at the tips of those micro-/nano-cavities.It may not be the case for a normal epoxy adhesive bonding since some degree of air entrapment at the tips of micro-/nano-cavities may not be avoidable.

    Fig.6.“Helical” CNTs on the Al-substrate of CHEM1,where “one” ends of CNTs in both (a) and (b) were pulled into the deep cavities (1) by the capillary action generated from the acetone evaporation process from the RPC solution.Some CNTs,e.g.one helical CNT in (a),remain the surface (2).

    2.3.Capillary action and position of CNT “Z-pins” into micro-cavities on Al substrate

    The CNT-containing resin pre-coating (RPC) solution is acetone rich(e.g.90 wt%acetone and 10 wt%resin)so that resin(without hardener)tends to fill in and remain within the surface and sub-surface microcavities after the complete acetone evaporation.This capillary actiondriven resin flow also takes CNTs into those micro-cavities.Fig.5 illustrates how CNTs are positioned into those vertical micro-channels or micro-cavities generated from anodising and sandblasting.Depending on the acetone/resin ratio,the RPC process can be repeated if necessary.Fig.6 shows“helical”CNT examples on the CHEM1 Al substrate surface of Fig.1,where “one” ends of some helical CNTs have been pulled into micro-cavities by the capillary action generated from the acetone evaporation process from the RPC solution.

    It should be mentioned again that a perfect CNT dispersion is not necessary for typical adhesive bonding,and it is sufficient to perform simple mechanical stirring in the RPC solution for a few minutes.Then the CNT-containing RPC solution is ready to apply over the chemically or mechanically treated Al substrate surfaces as illustrated in Fig.5.After the complete evaporation of acetone,the normal epoxy adhesive(resin +hardener mixture) can be applied.There is no need to further mix CNT with the viscous epoxy adhesives.

    3.Materials details and chemical surface treatments/characterisations

    3.1.Chemical anodising of Al substrates and sandblasting of steel

    The Al substrate samples (6065 T5) were anodised by similar procedures where the chemically alkaline etching was designed as the pretreatment,and electrochemically anodising was intended as the primary processing step.All major raw materials and their properties are listed in Table 1.

    Table 1 Main raw materials and their properties.

    Pre-treatments were necessary before the anodising treatment of Al substrates.Al alloy samples were ultrasonic cleaned in acetone for 30 min to remove any surface contaminants.Then they were put into a 10 wt%NaOH solution for 10 min to remove poorly soluble substrates.After etching by the NaOH solution,the Al samples were cleaned by deionised water.Then Al substrates were soaked into 10 wt% HNO3solution for 5 min to neutralise and remove NaOH residua.Anodising treatment on Al was designed to create surface structures.CHEM1 applied 20 wt% sulfuric acid dopted 0.5 wt% oxalic acid as the electrolyte while CHEM2 used 20 wt%phosphoric acid.Both CMEM 1&2 were treated under 12 V for 60 min.Different from Al,steel substrates (Fig.4) were sandblasted using GMA Premium Blast (Perth,Australia) garnet with a grit size of 30–60 μm at a compressed air pressure of 5 bar after pre-ultrasoniccleaned by acetone.

    Fig.7.(a)The load and displacement curves of each group closest to the average of 6 tests(Al substrate with deep vertical micro-channels as in Fig.1).Besides the maximum shear load,the critical displacement and energy are also enhanced significantly for the CNT +RPC combinations.(b)The average shear strength from 6 SLS tests.The combinations of CNT +RPC (resin pre-coating) are the most effective.

    Fig.8.Shear failure surfaces with different features linked to surface treatments.

    All treated metal substrates were soaked in CNT-contained resin precoating solution(weight ratio of acetone to resin to CNT was 89:10:1)for 30 s.CNTs remained in micro-valleys after acetone was completely evaporated.All CNT-rich and resin pre-coated metals were designed to be adhesively bonded with CFRP.The adhesive mixing ratio (adhesive to hardener) was 1:1.When joints were cured at room temperature,they were stored in the oven (60°C) for 3 days,ensuring adhesive mixtures were cured completely.

    3.2.Characterisation of samples

    Instron 5982 universal testing machine,Instron Corp.,USA,was applied to test single-lap shear stresses of adhesively connected joints according to ASTM 5868 [22].The operational parameters were set to 100 kN tensile fixture,a steady rate of 1 mm/min,and automatically recorded every 0.1 s for load and crosshead displacement.

    Morphologies and microstructure of pretreated aluminium and anodised aluminium were investigated using a scanning electron microscope(FEI Verios XHR SEM,Thermo Fisher Scientific Inc.,USA)by the Everhart-Thornley detector(ETD)at 20 kV/0.8 nA while 10 kV/0.4 nA for steel substrates.Internal pore feature was examined by focused ion beam(FIB,FEI Helios 650,Thermo Fisher Scientific Inc.,USA)with a high voltage of 5.0 kV and current of 0.34 nA.The Ga +beam with a depth of 30 μm was applied to cut and polish.

    Contact angles with water droplets on both treated and untreated Al before PRC were measured by an OCA20 contact angle meter (Data-Physics Instruments GmbH,Germany)with a water drop size of 2 μL.

    Fig.9.Shear strengths from 5 tests per group from samples made from CFRP and the Al substrate with relatively flat surface cavities as shown in Fig.2.CNT +RPC is still the most effective,but the increase of 73.5%is noticeably less than the 134.2% enhancement from the Al substrate with deep vertical microchannels in Fig.1.

    Fig.10.Cross-section views of contact angles for “CONTROL” group,CHEM1 anodised Al (Fig.1) and CHEM2 anodised Al (Fig.2) before RPC.

    Surface height profiles were evaluated by an Altisurf 520 profilometer(Altimet SAS,France).The CCS Prima confocal displacement sensor(CL3,Schmitt Industries,Inc.,Portland) was selected to set spot size,normal and lateral resolution as 4 μm,25 nm and 2 μm.An area of 2 mm× 2 mm in both x and y directions were detected.

    4.Experimental results

    4.1.Chemically treated Al substrates with CNT reinforcement applied by RPC

    The single-lap shear (SLS) test samples of adhesive bonded Al and CFRP were prepared and tested from the two Al substrates with distinctly different surface profiles generated from two different chemical surface treatments,as shown in Figs.1 and 2.The test results are shown in Fig.7 and Fig.9,respectively.The adhesive joint thickness is 0.76 mm,and the adhesive-bonded area is 25.4 × 25.4 mm2.The Al plates have the measurements of 101.6 × 25.4 × 3 mm3and the CFRP plates have the dimensions of 101.6× 25.4× 2 mm3.

    The “CONTROL” condition inFig.7(b) with the average shear strength of 9.6 MPa is for common adhesive bonding after acetone cleaning of both Al substrate and CFRP plate.“CHEM1”represents the Al substrate with vertical micro-channels,which is then bonded to CFRP normally.The average shear strength of 13.36 MPa is a 39.2% increase from the CONTROL condition.“CHEM1+RPC” with the average shear strength of 18.62 MPa for adhesive bonding after RPC(resin pre-coating)on both Al substrate and CFRP,i.e.the increase from 13.36 to 18.62 MPa(39.4% increase) is due purely to the effect of RPC.This shear strength increase implies that normal viscous epoxy adhesive cannot completely fill in the micro-channels of Al substrate shown in Fig.1.The last two groups in Fig.7(b)with average shear strengths of 20.55 and 22.48 MPa are results with the combination of CNT +RPC.CFRP of the last group was roughened slightly using#120 SiC sandpaper,followed by RPC.The largest 134.2%increase from the base CONTROL condition is significant.

    The typical shear failure modes corresponding to the substrate conditions in Fig.7 are shown in Fig.8.CONTROL has a typical adhesive failure along with the interface between Al substrate and adhesive joint.CHEM1+RPC has a mixture of adhesive failures at the interfaces on the Al substrate and CFRP sides and some degree of cohesive failure.That is,because of RPC,the interface between the Al substrate and adhesive joint is no longer the dominant weakest link in the adhesive-bonded composite structure.With the CNT reinforcement (for the CHEM1+RPC+CNT condition),the primary failure mode is shifted towards the interface between CFRP and adhesive joint.Failure inside CFRP has occurred and is clearly visible in Fig.8.With RPC over CFRP after slight roughening by#120 SiC sandpaper,the CNT-reinforced adhesive joint and its two interfaces with both Al substrate and CFRP are so strong that failure could only occur inside the CFRP substrate through delamination or tearing failures of carbon fibres.

    Shear strengths from samples made from CFRP and the Al substrate with relatively flat surface cavities in Fig.2 are shown in Fig.9.The CONTROL (only acetone cleaning) and CHEM2 (Al substrate with chemical treatment) have almost identical shear strengths,11.20 and 11.50 MPa,respectively.These similar shear strengths are probably as expected since both CONTROL and CHEM2 Al substrates have similar surface roughness,as can be seen from Fig.2(a)and(b).

    Fig.11.Epoxy adhesive-bonded steel substrates with 8 tests per group: Polished (using #120 SiC paper),SB (sandblasting),SB/RPC (SB +resin precoating),SB/RPC/CNT (SB +RPC +CNT,two separate tests with 8 samples per group).The highest enhancement from the CNT-PRC toughening is 93.4%from the polished surface,and is 34.5% from the sandblasted surface.

    The CHEM2+RPC condition in Fig.9 shows the significant shear strength increase of 53.5% to 17.35 MPa,which confirms the ability of RPC to penetrate into those surface and sub-surface micro-cavities over the chemically treated Al substrate.The shear strength (CHEM2-+RPC+SAND) is increased further to 18.65 MPa (or 65.1%) by slight roughening of CFRP by #120 SiC sandpaper.The final two groups with CNT reinforcements show similar trends with average values of 18.80 and 19.60 MPa,respectively.The best result with 73.5%improvement is significantly less than 134.2% in Fig.7,proving the effectiveness of vertical micro-channels and CNT“Z-pins”across the Al substrate surface.

    Contact angles for the CONTROL group,CHEM1 anodised Al,and CHEM2 anodised Al are described in Fig.10.Acetone ultrasonic cleaned Al substrates(CONTROL)witnesses a higher contact angle at 115°since contaminants still remained on Al's surface,leading to weak bonding strength between Al and adhesive.Sulfuric-oxalic acid anodised Al decreases contact angles to 68°since anodising treatment achieves increased wettability.Phosphoric acid anodised Al (CHEM2) has a slightly higher contact angle(78°)than sulfuric-oxalic acid anodised one(CHEM1).Low surface roughness contributes to this low wettability.

    4.2.Sandblasted steel substrate with CNT reinforcement applied by RPC

    For the purpose of comparison,the effects of CNT +RPC interfacial reinforcements on shear strengths of adhesive bonded mild steel substrates [16] are shown in Fig.11.Eight samples were tested for each group shown in Fig.11.The adhesive joint thickness is around 50 μm,and the adhesive-bonded area is 25×13 mm2.The mild steel plates have measurements of 40×25×3 mm3.

    The shear strength between the two polished steel substrates (using#120 SiC paper) is 16.23 MPa and is 23.33 MPa for the sandblasted surface.RPC has further enhanced the shear strength to 28.18 MPa.Two separate tests(8 samples per group)with CNT-toughened adhesive joints produced the best and almost identical results of 31.07 and 31.39 MPa.Those results in Fig.11 for the steel substrate clearly show that normal adhesive bonding after sandblasting can still be improved by RPC +CNT,which is similar to the two Al substrate cases in Figs.7 and 9.A recent study [17] on adhesive bonding between CFRP and Al substrate with a sandblasting surface finish also shows that RPC alone can further enhance the shear strength by 35.1%.

    Fig.12.Three major failure modes of adhesive bonded Al and CFRP interface:(a)adhesive failure along the Al substrate surface,(b)cohesive failure in the adhesive joint (possibly with partial failure along CFRP surface),and (c) structural failure inside CFRP away from the CNT-toughened adhesive joint,which is possible if the adhesive joint is optimised and fully toughened.

    5.Discussions

    5.1.Effectiveness of CNT-toughening with RPC and relevant shear failure modes

    The most considerable shear strength improvement is 134%,74%,and 93%for the three different substrate surfaces prepared chemically or mechanically.These results show that the CNT-containing RPC process is effective.Since CNT dispersion in the RPC solution is simple,and the CNT +RPC process can be conveniently used on-site and applied by engineers without special training and without the need for any special equipment,the unique interfacial toughening method proposed in this study has the potential to be adopted on-site for large-area adhesive bonding between Al substrate and CFRP.

    Fig.13.(a)Micro-roughness and cavities over Al and CFRP substrate surfaces[18],and(b)vertical micro-channels in Al substrate created by chemical treatment as in Fig.1(b).Resin pre-coating (RPC) has filled all micro-cavities,which may be difficult using normal epoxy adhesive due to relatively high viscosity.

    The change or shift in the shear failure modes displayed in Fig.8 by the optical photos of test samples can be summarised by the illustrations in Fig.12.The commonly known two failure modes are:(1)the adhesive failure or failure along the interface between the substrate and adhesive joint,and(2)the cohesive failure or failure within the adhesive joint.The substrate surface treatments are designed to suppress adhesive failure.The CNT interfacial reinforcement can effectively prevent premature failures from either“the adhesive or cohesive mode”.

    It is noticed that CNT +RPC can be so effective that neither adhesive nor cohesive failure is possible.In this case,the third failure mode,or(c)structural failure within CFRP,is generated.That is,the adhesive joint is no longer the weakest link in laminar Al-CFRP structures.This probably is the optimum adhesive bonding scenario,which can be expected for structural applications.

    Besides establishing“Z-pins”by injecting CNTs into surface-modified metal interface structures,a similar setup by dispersing CNTs in epoxy matrix[23]can realise the same function of“Z-pins”.Functionalised CNT on matrix interface can connect to those micro-structures on adherend surfaces to realise “Z-pins” establishment.Adhesives strengthened by nanoparticles (e.g.,GNPs and CNTs [26,27]) can significantly improve the bulk strength of adhesive matrix and adhesive bond strength,up to the scale of 20–30 MPa.Again,CNT and micro-length or short fibres do not have to be vertical to strengthen the thin adhesive joint.The best content of CNT varies by surface roughness and micro-structures dimensions of adherents.Typically,optimum adhesive properties can be achieved with around 1–2 wt%CNTs[25].

    5.2.RPC -optimisation of adhesive bonding area and strength

    A comprehensive review of adhesive bonding between Al substrate and CFRP published recently[18] provides a good overview of the current technologies utilised for adhesive bonding of these two vastly different materials.The general illustration of Al and CFRP substrates[18] is shown in Fig.13(a),where micro-cavities exist on both Al and CFRP substrates.

    While the “perfect” adhesive bonding condition along the surface profiles,as illustrated in Fig.13(a),is highly idealised,it has actually been achieved by the simple RPC method described in this study.The SEM-FIB micrograph in Fig.13(b) or part of Fig.1(b) shows the perfect adhesive bonding profile inside those vertical micro-channels created by the chemical surface treatment [15].The CNT “Z-pins” positioned into those vertical micro-channels by RPC provides the crack-bridging mechanism along the surface reference lines in Fig.13(a).It should also be mentioned that the RPC method adopted for the three adhesive bonding cases has also been tested on other substrates,including rock,wood and bamboo composites[19–21].

    Last but not least,there is one more positive aspect of RPC,which is desirable for adhesive bonding.After filling and sealing all micro-and nano-pores (e.g.micro-porous structures shown in Fig.2 and TiO2nanotubes formed on the titanium alloy [24]),RPC also improves the wettability of the substrate.This is because the ultra-thin resin coating(without hardener) left over the substrate surface remain “wet” after evaporation of acetone.The comparison of the SEM micrographs of the steel surfaces shown in Fig.4(a)and(b)clearly shows the difference due to RPC.For the three types of surface profiles from CHEM1,CHEM2 and sandblasting,RPC is invariably effective.It is highly likely that RPC may also be useful even to the fine nanostructures reported in Ref.[24].

    6.Conclusions

    As summarised in Fig.13 and discussed in the review article[16],the thin adhesive joint between Al and CFRP substrates is typically un-reinforced,and micro-cavities exists on both substrates (that can be purposely prepared).This study compared two chemically treated Al substrates and one steel substrate prepared by sandblasting.The CFRP surface can be conveniently roughened by sandpapers if necessary.

    This study examined the effectiveness of CNT-bridging across the thin adhesive joint between the Al and CFRP substrates.Filling of all microcavities over both substrate surfaces is ensured by the unique resin precoating (RPC) process,using the acetone-rich resin solution,e.g.acetone 90 wt% and resin 10 wt% (without hardener).CNTs are pulled into those micro-cavities and across the “surface reference lines” in Fig.13 by the capillary action generated by acetone evaporation so that CNT “Z-pins” or CNT-bridging across the thin adhesive joint becomes possible.Clearly,the effectiveness of CNT-bridging depends on the surface profiles of both Al and CFRP substrates.The highest shear bonding strength improvements for the three cases in this study are over 130%,70% and 90%,respectively,and they are all with CNT interfacial toughening.It can be concluded that the CNT-containing RPC solution has significantly improved the adhesive bond strength between the Al substrate and CFRP,and the method can be easily used on other substrates such as rock,concrete,wood and bamboo composites.

    Declaration of competing interest

    There are no conflicts to declare.

    Acknowledgement

    XZ Hu would like to thank Chang'an University of China for a visiting professor grant (2018-2020) for research collaboration between Chang'an University and University of Western Australia.

    又粗又硬又长又爽又黄的视频| 99久久精品热视频| 亚洲天堂国产精品一区在线| av在线播放精品| 精品久久久久久电影网| 精品不卡国产一区二区三区| 丝袜喷水一区| 97热精品久久久久久| 日本色播在线视频| 欧美不卡视频在线免费观看| 国产高清三级在线| 国产一级毛片在线| 高清av免费在线| 国产精品av视频在线免费观看| 在线a可以看的网站| 蜜桃久久精品国产亚洲av| 好男人在线观看高清免费视频| 一区二区三区乱码不卡18| 欧美性猛交╳xxx乱大交人| 777米奇影视久久| 亚洲精品久久久久久婷婷小说| 国产高清三级在线| 久久精品国产亚洲网站| 一区二区三区乱码不卡18| 午夜亚洲福利在线播放| 婷婷六月久久综合丁香| 亚洲成人精品中文字幕电影| 国产av在哪里看| 人体艺术视频欧美日本| 三级经典国产精品| 内射极品少妇av片p| 国产激情偷乱视频一区二区| 联通29元200g的流量卡| 国产高清三级在线| 国产免费视频播放在线视频 | 亚洲国产精品专区欧美| 美女脱内裤让男人舔精品视频| 国产成人午夜福利电影在线观看| 午夜精品在线福利| 欧美激情在线99| 床上黄色一级片| 免费播放大片免费观看视频在线观看| 日本午夜av视频| 国产精品福利在线免费观看| 男人舔奶头视频| 91午夜精品亚洲一区二区三区| 国产免费福利视频在线观看| 人人妻人人澡人人爽人人夜夜 | 综合色丁香网| 久久99蜜桃精品久久| 国产黄片美女视频| 乱码一卡2卡4卡精品| 又爽又黄无遮挡网站| 国产91av在线免费观看| 欧美成人精品欧美一级黄| 日韩亚洲欧美综合| 少妇猛男粗大的猛烈进出视频 | 五月玫瑰六月丁香| 亚洲精品成人久久久久久| 三级国产精品欧美在线观看| 99re6热这里在线精品视频| 免费少妇av软件| 欧美高清性xxxxhd video| 国产片特级美女逼逼视频| 一区二区三区免费毛片| 嫩草影院新地址| 国产高潮美女av| 内射极品少妇av片p| 国产午夜精品论理片| 老女人水多毛片| 蜜桃亚洲精品一区二区三区| 三级毛片av免费| 午夜免费激情av| 一区二区三区四区激情视频| 听说在线观看完整版免费高清| 有码 亚洲区| 国产国拍精品亚洲av在线观看| 搡女人真爽免费视频火全软件| 国产有黄有色有爽视频| 欧美日韩综合久久久久久| 看免费成人av毛片| 国产又色又爽无遮挡免| 成人综合一区亚洲| 国产免费又黄又爽又色| 97超碰精品成人国产| kizo精华| 又黄又爽又刺激的免费视频.| 性色avwww在线观看| 亚洲高清免费不卡视频| 国产亚洲av嫩草精品影院| 久99久视频精品免费| 狂野欧美白嫩少妇大欣赏| 韩国高清视频一区二区三区| 99热这里只有是精品在线观看| 狠狠精品人妻久久久久久综合| 99久久精品一区二区三区| 国产有黄有色有爽视频| 久久99蜜桃精品久久| 少妇丰满av| 日本与韩国留学比较| 91午夜精品亚洲一区二区三区| 高清午夜精品一区二区三区| 欧美区成人在线视频| 一个人看视频在线观看www免费| 久久这里有精品视频免费| 丝袜喷水一区| videos熟女内射| 亚洲国产成人一精品久久久| 国产精品国产三级国产专区5o| 亚洲国产色片| 高清欧美精品videossex| 91在线精品国自产拍蜜月| 激情 狠狠 欧美| 国产亚洲午夜精品一区二区久久 | av在线蜜桃| av福利片在线观看| 国产成人一区二区在线| 国产伦精品一区二区三区四那| 亚洲在线自拍视频| 欧美成人午夜免费资源| 又爽又黄无遮挡网站| 亚洲精品成人av观看孕妇| 国产中年淑女户外野战色| 在线 av 中文字幕| 免费观看的影片在线观看| 好男人视频免费观看在线| 日韩欧美精品免费久久| 欧美激情在线99| 91在线精品国自产拍蜜月| 一级毛片久久久久久久久女| 国产精品精品国产色婷婷| 午夜激情久久久久久久| 99久久中文字幕三级久久日本| 亚洲怡红院男人天堂| 在线观看一区二区三区| av国产免费在线观看| 少妇人妻一区二区三区视频| 亚洲激情五月婷婷啪啪| 国产成人精品久久久久久| 亚洲精品aⅴ在线观看| 国产免费福利视频在线观看| av.在线天堂| 亚洲色图av天堂| 波野结衣二区三区在线| 国产精品一区二区三区四区免费观看| 国产探花极品一区二区| 亚洲,欧美,日韩| 中文字幕av成人在线电影| 99久久精品热视频| 免费播放大片免费观看视频在线观看| 免费播放大片免费观看视频在线观看| 婷婷色综合大香蕉| 3wmmmm亚洲av在线观看| av免费观看日本| 亚洲怡红院男人天堂| 久久这里只有精品中国| 九九久久精品国产亚洲av麻豆| 在线观看一区二区三区| 又大又黄又爽视频免费| 美女黄网站色视频| 国产精品一及| 97超视频在线观看视频| 国产亚洲av嫩草精品影院| 日日干狠狠操夜夜爽| av在线播放精品| 久久韩国三级中文字幕| 成年人午夜在线观看视频 | 亚洲图色成人| 日本三级黄在线观看| 丝袜喷水一区| 欧美一级a爱片免费观看看| 亚洲av中文字字幕乱码综合| 免费av观看视频| 十八禁网站网址无遮挡 | 内射极品少妇av片p| 国产精品一区二区在线观看99 | 亚洲国产精品sss在线观看| av国产免费在线观看| 九九久久精品国产亚洲av麻豆| 日日撸夜夜添| 久久人人爽人人爽人人片va| or卡值多少钱| 免费看美女性在线毛片视频| 一级毛片久久久久久久久女| 亚洲精品久久午夜乱码| 校园人妻丝袜中文字幕| 丰满少妇做爰视频| 男插女下体视频免费在线播放| 国产亚洲av嫩草精品影院| 成年人午夜在线观看视频 | 秋霞伦理黄片| 久久久久久久久中文| 高清视频免费观看一区二区 | 91久久精品国产一区二区三区| 久久精品久久精品一区二区三区| 亚洲欧美日韩卡通动漫| 国产精品久久视频播放| 男人和女人高潮做爰伦理| 成年人午夜在线观看视频 | 精品久久久噜噜| 亚洲人成网站在线观看播放| av在线亚洲专区| www.av在线官网国产| 欧美日韩综合久久久久久| 成人毛片60女人毛片免费| 国产黄频视频在线观看| 成人国产麻豆网| 亚洲av福利一区| 亚洲精品国产成人久久av| 日本爱情动作片www.在线观看| 美女cb高潮喷水在线观看| 国产老妇伦熟女老妇高清| 97精品久久久久久久久久精品| 亚洲成人一二三区av| 色尼玛亚洲综合影院| 精品一区二区三卡| 人妻一区二区av| av福利片在线观看| 亚洲国产高清在线一区二区三| 日韩av不卡免费在线播放| 少妇人妻一区二区三区视频| 日本wwww免费看| 久久久精品94久久精品| 亚洲av电影在线观看一区二区三区 | 精品久久久久久久久久久久久| 小蜜桃在线观看免费完整版高清| 熟妇人妻久久中文字幕3abv| 国产白丝娇喘喷水9色精品| 日本黄大片高清| 久久99蜜桃精品久久| 国产男人的电影天堂91| 一级片'在线观看视频| 久久久精品欧美日韩精品| 欧美日韩国产mv在线观看视频 | 精品国产一区二区三区久久久樱花 | 亚洲经典国产精华液单| 91久久精品电影网| av免费观看日本| 亚洲av福利一区| 少妇裸体淫交视频免费看高清| 毛片女人毛片| 国产91av在线免费观看| 中文字幕久久专区| www.av在线官网国产| 欧美xxⅹ黑人| 91aial.com中文字幕在线观看| 亚洲怡红院男人天堂| 国产成人福利小说| 观看美女的网站| 久久韩国三级中文字幕| 简卡轻食公司| 极品教师在线视频| 国产一区有黄有色的免费视频 | 中文字幕av成人在线电影| 日产精品乱码卡一卡2卡三| 国产成人91sexporn| 国产午夜精品久久久久久一区二区三区| 男人舔奶头视频| 五月玫瑰六月丁香| 观看美女的网站| 欧美xxxx黑人xx丫x性爽| 麻豆成人午夜福利视频| 中文字幕制服av| 大又大粗又爽又黄少妇毛片口| 国产在线男女| 欧美日韩综合久久久久久| 日产精品乱码卡一卡2卡三| 国产精品一及| 狂野欧美激情性xxxx在线观看| 精品久久久久久久末码| 97精品久久久久久久久久精品| av线在线观看网站| 真实男女啪啪啪动态图| 亚洲国产精品国产精品| 中文字幕人妻熟人妻熟丝袜美| 久久草成人影院| 成人综合一区亚洲| 久久鲁丝午夜福利片| 日本黄大片高清| 草草在线视频免费看| 成人午夜高清在线视频| 在线免费十八禁| 九九爱精品视频在线观看| av专区在线播放| 成人亚洲欧美一区二区av| 日产精品乱码卡一卡2卡三| xxx大片免费视频| 日日干狠狠操夜夜爽| 国产美女午夜福利| 国产综合懂色| 国产成人freesex在线| 免费高清在线观看视频在线观看| 亚洲综合色惰| 舔av片在线| 亚洲精品日本国产第一区| 精品99又大又爽又粗少妇毛片| a级一级毛片免费在线观看| 国产有黄有色有爽视频| 久久国产乱子免费精品| 亚洲av福利一区| 69av精品久久久久久| 国产老妇伦熟女老妇高清| 亚洲精品乱码久久久v下载方式| 国产精品99久久久久久久久| 精品国产露脸久久av麻豆 | 欧美另类一区| 99久久精品国产国产毛片| 久久精品国产亚洲av天美| 一个人看视频在线观看www免费| 午夜福利网站1000一区二区三区| 久久久久精品久久久久真实原创| 青春草亚洲视频在线观看| 国产淫片久久久久久久久| 日本一本二区三区精品| 成年版毛片免费区| 欧美日韩在线观看h| 久久久久久国产a免费观看| 禁无遮挡网站| 国产在线一区二区三区精| 国产白丝娇喘喷水9色精品| 黄片无遮挡物在线观看| 久久久久久久午夜电影| 亚洲av免费高清在线观看| 精品久久久久久久久久久久久| 久久鲁丝午夜福利片| 只有这里有精品99| 国产成人精品婷婷| 精品久久久久久久末码| 国产精品蜜桃在线观看| 欧美日本视频| 国内少妇人妻偷人精品xxx网站| 美女国产视频在线观看| 国产综合精华液| 国产精品国产三级国产专区5o| 国产欧美日韩精品一区二区| 亚洲av二区三区四区| 亚洲欧美日韩无卡精品| 淫秽高清视频在线观看| 能在线免费观看的黄片| 午夜精品一区二区三区免费看| 伦理电影大哥的女人| 欧美日韩在线观看h| 女人十人毛片免费观看3o分钟| 国产精品国产三级国产专区5o| 观看免费一级毛片| 白带黄色成豆腐渣| 久久99蜜桃精品久久| 嫩草影院精品99| 美女高潮的动态| 亚洲精华国产精华液的使用体验| 欧美精品一区二区大全| 午夜激情久久久久久久| 最后的刺客免费高清国语| 18禁动态无遮挡网站| 国产白丝娇喘喷水9色精品| 街头女战士在线观看网站| 久久久久久国产a免费观看| 精品欧美国产一区二区三| 欧美日本视频| 欧美日韩精品成人综合77777| 听说在线观看完整版免费高清| 最近2019中文字幕mv第一页| 免费看不卡的av| 成人毛片a级毛片在线播放| 国产成年人精品一区二区| 大香蕉97超碰在线| 亚洲av成人精品一区久久| 夫妻性生交免费视频一级片| 日本与韩国留学比较| 观看美女的网站| 免费看日本二区| 99re6热这里在线精品视频| 中文欧美无线码| 亚洲精品久久午夜乱码| 欧美丝袜亚洲另类| 熟妇人妻久久中文字幕3abv| 午夜福利在线在线| 色哟哟·www| 国产高清三级在线| 插逼视频在线观看| 热99在线观看视频| 少妇猛男粗大的猛烈进出视频 | 最近的中文字幕免费完整| 免费观看精品视频网站| 欧美日韩一区二区视频在线观看视频在线 | 在线 av 中文字幕| 免费少妇av软件| 久久精品人妻少妇| 激情五月婷婷亚洲| 久久精品夜色国产| 日韩一区二区视频免费看| 精品人妻偷拍中文字幕| 舔av片在线| 天堂俺去俺来也www色官网 | 1000部很黄的大片| 国产国拍精品亚洲av在线观看| 亚洲四区av| 精品国内亚洲2022精品成人| 久久久亚洲精品成人影院| 国产亚洲午夜精品一区二区久久 | 春色校园在线视频观看| 观看免费一级毛片| 永久免费av网站大全| 青春草亚洲视频在线观看| 国产91av在线免费观看| 伦精品一区二区三区| 国产一区二区三区av在线| 一个人免费在线观看电影| 一级av片app| 99久久九九国产精品国产免费| 久久久久精品久久久久真实原创| 18禁在线无遮挡免费观看视频| 亚洲av电影不卡..在线观看| 国产成人精品福利久久| 我的女老师完整版在线观看| 2021少妇久久久久久久久久久| 欧美一级a爱片免费观看看| 22中文网久久字幕| 观看美女的网站| 免费黄网站久久成人精品| 免费av不卡在线播放| 亚洲一级一片aⅴ在线观看| 亚洲四区av| 欧美高清成人免费视频www| 哪个播放器可以免费观看大片| 毛片女人毛片| 小蜜桃在线观看免费完整版高清| 亚洲欧美精品专区久久| 国产免费视频播放在线视频 | 91av网一区二区| 国产精品久久久久久av不卡| 真实男女啪啪啪动态图| 久久精品人妻少妇| 校园人妻丝袜中文字幕| 亚洲精品一区蜜桃| 免费观看在线日韩| 亚洲精品国产成人久久av| 91精品国产九色| 国产有黄有色有爽视频| 中文天堂在线官网| 国产伦一二天堂av在线观看| 男人舔奶头视频| 日韩av在线大香蕉| 国产精品麻豆人妻色哟哟久久 | 精品久久久精品久久久| 国产伦精品一区二区三区四那| 亚洲欧美精品专区久久| 美女内射精品一级片tv| 精品国内亚洲2022精品成人| 汤姆久久久久久久影院中文字幕 | 青春草国产在线视频| 国产成人精品福利久久| 美女黄网站色视频| 麻豆乱淫一区二区| 三级经典国产精品| 久久久国产一区二区| 干丝袜人妻中文字幕| 老司机影院毛片| 国产精品日韩av在线免费观看| 国产69精品久久久久777片| 国产免费福利视频在线观看| 午夜亚洲福利在线播放| 久久久a久久爽久久v久久| 男女啪啪激烈高潮av片| 18禁在线无遮挡免费观看视频| 国产午夜精品论理片| 国产精品日韩av在线免费观看| 亚洲天堂国产精品一区在线| 22中文网久久字幕| 大片免费播放器 马上看| 波多野结衣巨乳人妻| 99久久精品热视频| 久久精品国产亚洲网站| 大话2 男鬼变身卡| 亚洲精品久久午夜乱码| 日韩电影二区| 五月伊人婷婷丁香| 乱系列少妇在线播放| 精品酒店卫生间| 一级a做视频免费观看| 精品99又大又爽又粗少妇毛片| 男的添女的下面高潮视频| 日韩av在线大香蕉| 国产午夜精品一二区理论片| 七月丁香在线播放| 如何舔出高潮| 中文字幕av成人在线电影| 亚洲精品影视一区二区三区av| 久久久精品免费免费高清| 少妇丰满av| 日韩欧美精品v在线| 高清欧美精品videossex| 大香蕉久久网| 中国国产av一级| 真实男女啪啪啪动态图| 五月伊人婷婷丁香| 最近的中文字幕免费完整| 天堂中文最新版在线下载 | 两个人的视频大全免费| 69人妻影院| 九九爱精品视频在线观看| 亚洲精品久久久久久婷婷小说| 午夜免费激情av| 99re6热这里在线精品视频| 亚洲av免费在线观看| 中文字幕制服av| 亚洲精品乱码久久久久久按摩| 国产亚洲av嫩草精品影院| 色综合色国产| 一级二级三级毛片免费看| 黄色欧美视频在线观看| 亚洲欧美成人综合另类久久久| 日本黄色片子视频| 国产精品综合久久久久久久免费| videossex国产| 欧美高清成人免费视频www| 爱豆传媒免费全集在线观看| 九九爱精品视频在线观看| 哪个播放器可以免费观看大片| 最近的中文字幕免费完整| 人体艺术视频欧美日本| 久久6这里有精品| 亚洲精华国产精华液的使用体验| 亚洲av免费在线观看| 国产久久久一区二区三区| 精品人妻视频免费看| 99热6这里只有精品| 亚洲欧美一区二区三区黑人 | 国产高潮美女av| 最近手机中文字幕大全| 免费av不卡在线播放| 日日摸夜夜添夜夜爱| 成年女人在线观看亚洲视频 | 免费电影在线观看免费观看| 午夜福利成人在线免费观看| 亚洲精品日韩在线中文字幕| 春色校园在线视频观看| 免费大片黄手机在线观看| 久久综合国产亚洲精品| 成人午夜精彩视频在线观看| 色吧在线观看| 99热这里只有精品一区| 亚洲精品自拍成人| 久久久色成人| 三级男女做爰猛烈吃奶摸视频| 美女cb高潮喷水在线观看| 欧美不卡视频在线免费观看| 一级二级三级毛片免费看| 中国美白少妇内射xxxbb| 亚洲av电影在线观看一区二区三区 | 日韩伦理黄色片| 女人被狂操c到高潮| 国产黄频视频在线观看| 成年人午夜在线观看视频 | 在线观看一区二区三区| 成年免费大片在线观看| 国产永久视频网站| 国产片特级美女逼逼视频| 欧美xxⅹ黑人| 99久久精品国产国产毛片| 一级毛片黄色毛片免费观看视频| 欧美xxxx黑人xx丫x性爽| 亚洲av二区三区四区| 午夜老司机福利剧场| 国产免费福利视频在线观看| 韩国av在线不卡| 亚洲成人精品中文字幕电影| 一级av片app| 精华霜和精华液先用哪个| 亚洲美女搞黄在线观看| 99久久精品热视频| 久久久久精品性色| 男的添女的下面高潮视频| 亚洲欧美一区二区三区国产| 婷婷色麻豆天堂久久| 成年免费大片在线观看| 亚洲精品日韩av片在线观看| 久久久久久久大尺度免费视频| 久久99热这里只有精品18| 亚洲天堂国产精品一区在线| 免费不卡的大黄色大毛片视频在线观看 | 九草在线视频观看| 亚洲婷婷狠狠爱综合网| 欧美日韩一区二区视频在线观看视频在线 | 国产男女超爽视频在线观看| 亚洲国产最新在线播放| 久久久久久久久久人人人人人人| 丰满少妇做爰视频| 寂寞人妻少妇视频99o| 乱系列少妇在线播放| 自拍偷自拍亚洲精品老妇| 欧美日韩亚洲高清精品| 日韩制服骚丝袜av| 国产一区有黄有色的免费视频 | 亚洲欧美中文字幕日韩二区| 91久久精品电影网| 国产中年淑女户外野战色| 亚洲成人精品中文字幕电影| 国产精品蜜桃在线观看| 五月伊人婷婷丁香| 亚洲精品一区蜜桃| 777米奇影视久久| 国产又色又爽无遮挡免| 午夜亚洲福利在线播放| 亚洲欧美日韩东京热| 插阴视频在线观看视频| 一区二区三区高清视频在线| 51国产日韩欧美| 少妇人妻一区二区三区视频| 国产91av在线免费观看| 国产黄频视频在线观看| 国产精品美女特级片免费视频播放器| 亚洲真实伦在线观看| 一级av片app| 91午夜精品亚洲一区二区三区|