    Microstructure and mechanical properties of repair welds of low-pressure sand-cast Mg-Y-RE-Zr alloy by tungsten inert gas welding

    2022-07-14 08:55:56XinTongGuohuaWuLiangZhangYingxinWangWencaiLiuWenjiangDing
    Journal of Magnesium and Alloys 2022年1期

    Xin Tong, Guohua Wu, Liang Zhang, Yingxin Wang, Wencai Liu, Wenjiang Ding

    National Engineering Research Center of Light Alloy Net Forming and State Key Laboratory of Metal Matrix Composites, School of Materials Science and Engineering, Shanghai Jiao Tong University, Shanghai 200240, China

    Abstract The sand castings of Mg-Y-RE-Zr series alloys are widely utilized in the large scales and complex shapes in the aerospace industry,as a result of which there are always some cast defects in the products.In this study, the feasibility of repair welding of sand-cast Mg-4Y-3RE-0.5Zr alloy by tungsten inert gas (TIG) welding was scrutinized with different welding currents from 150 to 210 A.The results indicated that defect-free repaired joints with good appearance could be acquired at 170 and 190 A.Interestingly, the grain size of the fusion zone (FZ) was refined initially and then increased with the linear increment of welding current.Because at the higher heat inputs, although the cooling rate of the molten pool was reduced, substantial constitutional supercooling for the grain refinement was attained after the Zr particles were transformed into Zr solutes.The tensile strength of the repaired joint at 170 A was 195MPa with the maximum joint efficiency of 87.8%, and the elongation reached to 124.4% of the sand-cast base material (BM).However, serious grain coarsening and continuous eutectic structures generated in heat-affected zone (HAZ) above 190 A resulted in the weakening of the joint due to the brittle intergranular fracture.

    Keywords: Sand-cast Mg-Y-RE-Zr alloy; Repair welding; Microstructure; Tensile properties; Fracture behavior.

    1.Introduction

    Developing the lightweight magnesium (Mg) alloys with excellent performances has long been a significant target of the aerospace industry, where reducing the weight of components is of crucial importance[1,2].Compared with traditional Mg alloys, Mg-rare earth (Mg-RE) alloys have attracted considerable attention for their higher specific strength, better corrosion resistance, and especially the desirable creep resistance up to the high temperature of 523K [3-5].In particular,the Mg-Y-RE-Zr series alloys have become the most famous commercial Mg-RE alloys and been widely applied in aviation and aerospace fields [6,7].

    From the practical needs of aerospace engineering, the large-scale and complex-shaped components are mostly produced by low- or differential-pressure sand casting process [8-10].However, because of the slow filling rate, long solidification time, and intricate mould cavity of the sand casting process, typical defects such as sand inclusions,shrinkage porosities, and microcracks can be produced during solidification procedure [11,12].Moreover, because RE elements exhibit even stronger tendencies to be oxidized than Mg (the oxidation tendency is Y>Gd>Nd>Mg) [13], it is much easier to generate oxidation slags in Mg-Y-RE-Zr alloy castings with the high Y contents.Actually, some of these defects are inevitable in complex castings even processed in the modified gating and cooling systems [14].So it is essential to develop an economical repair welding technique with easy accessibility for Mg-Y-RE-Zr series sand castings.

    Because of the utility and economy, TIG welding has been widely adopted to Mg alloys at the industrial level[15].Moreover, TIG welding can be performed manually, so it exhibits unique advantages for repairing inner structures and camberedsurfaces in comparison to some advanced welding technologies such as friction stir welding (FSW) [16], diffusion welding(DW)[17],and laser beam welding(LBW)[18].Recently,Meng et al.[14]proved the feasibility of TIG welding for repairing of as-cast Mg-6Gd-3Y-0.5Zr alloy,and the maximum tensile strength of the T6 treated joint reached up to 295MPa.Turowska and Adamiec [19]analyzed the microstructure of the TIG welds of WE43 alloy just under a fixed welding parameter and evaluated their mechanical properties at elevated temperatures.

    However,the existing papers primarily investigated the butt joints of Mg-RE alloys [20,21], while the repair welding is usually applied for refilling some small holes after removing the local defects.Thus there may be a more severe tensile stress field and a higher cooling rate within the weld pool of repaired joints.It is unclear whether these differences have effects on the performance of repaired casting.On the other hand, most of the published works were focused on the welding of deformed Mg-RE alloys or these series alloys fabricated by permanent mould casting [22], which are quite different from the engineering application.The coarser grain size as well as the continuous eutectic structure in the sand-cast alloy is more easily to generate overburning and hot crack under the high temperature of TIG welding [17].Thus,optimized welding parameters in the previous researches may not be suitable for the sand-cast Mg-Y-RE-Zr alloy.

    Liu et al.[23]concluded that, because of the high heat input of TIG welding, the grain size of FZ in TIG welded AZ31B alloy is the largest in comparison to other advanced welding methods.But for the welded Mg-Y-RE-Zr alloys,in addition to the weld heat input, also Zr can significantly affect the grain size [24-26].In Mg alloys, there are two different existence forms of Zr: Zr solute (Zrs) and Zr particle(Zrp).Zrpprovides the heterogeneous site for nucleation of the primaryα-Mg due to their similar lattice constants, while Zrsprovides substantial constitutional supercooling to restrict grain growth.The Interdependence Model [27,28]illustrated that both Zrpand Zrsare required to achieve the grain refinement, but a major contribution was provided by Zrs[29,30].So in the casting process, long holding time and repeated stirring are necessary to dissolve Zr in the Mg melt to achieve better grain refinement [30].

    Similarly, the resulting Zr phases in Mg-Y-RE-Zr alloys will be influenced by the heat input induced by the TIG welding process.In other words, the grain size of FZ in this series alloy may be determined by the combined effects of the cooling rate and the existence forms of Zr.Qin et al.[31]prepared dissimilar joints between AZ61 and ZK60 (Zr content>0.45wt%) Mg alloys by TIG welding, and the grain size in FZ first decreased and then increased with the linear increase of the welding current.The authors attributed this finding to the synergistic effect of the cooling rate and the heat input but without consideration of the Zr.However, up to now, there is no further research on the effect of Zr existence forms on the microstructure of Mg-RE-Zr alloys during the welding process, and the repair welding of sand-cast Mg-Y-RE-Zr alloy has not been paid much attention to.

    Given these facts, in the present study, the repair welding of sand-cast Mg-4Y-3RE-0.5Zr alloy was performed by TIG welding under different welding currents.The qualities of the repaired castings were evaluated in terms of the microstructure evolutions and mechanical properties of the formed joints.We believe that these results will broaden our understanding of the repair welding of sand-cast Mg-RE-Zr alloys and further their applicability to the aerospace industry.

    2.Experimental procedure

    2.1.Preparation of the low-pressure sand-cast alloy

    In this research, the low-pressure sand-cast Mg-4Y-2Nd-1Gd-0.5Zr alloy was chosen for repair welding experiments.The base material was fabricated by melting commercial pure Mg (>99.95%), Mg-30Y, Mg-90Nd, Mg-90Gd and Mg-30Zr (wt%) master alloys in an electric resistance furnace protected by a mixed atmosphere of CO2(99 vol%) and SF6(1 vol%).After refined at 740°C for 10min, the melt was filled into a sand mould preheated to 200°C to obtain the alloy plates.The actual composition detected by Inductively Coupled Plasma-Atomic Emission Spectroscopy (ICP-AES)was listed in Table 1.Detailed information regarding the testing of the content of dissolved Zr (Zrs) can be found elsewhere [30,32].

    Table 1The actual composition of the sand-cast Mg-4Y-2Nd-1Gd-0.5Zr alloy analysed by ICP-AES (wt%).

    2.2.Repair welding process

    The plates were cut into rectangular specimens with dimensions of 70mm×60mm×10mm for welding experiments.Afterwards, a blind hole (Ф 15 mm×H 5 mm) was processed by a pneumatic milling cutter at the centre of the plate for AC-TIG repair welding(Rehm INVERTIG.PRO digital 450 AC/DC).The chemical composition of the filler rod is shown in Table 1.Prior to welding, all the surfaces of the workpiece and the filler rod were ground with 400 # grit SiC paper and degreased in acetone for removing the surface attachments.In order to reduce the experimental error, all the experiments were performed via a set of self-designed welding jig and wire feeder.Fig.1 illustrates the schematic of the process procedure,and detailed information about the welding parameters are provided in Table 2.

    Table 2The primary process parameters of the repair welding.

    2.3.Characterization

    X-ray computer tomography was used to detect the welding defects within the repaired joint.Cross-sections ofthe repaired plates were mechanically ground, polished, and etched in a solution of 4.2g picric acid, 10mL acetic acid,10mL water and 70mL ethanol for 12s.Macrostructure observation of the cross-section of the joint was carried out by a stereoscopic microscope (Stemi 305).Microstructure characterization was performed by an optical microscope (OM, Carl Zeiss Axivoert 40) and scanning electron microscope (SEM,NOVA NanoSEM 230) equipped with an energy-dispersive spectroscope (EDS).The grain sizes of the repair welded alloys were calculated by the image analysis software Image-Pro Plus 6.0.The phase composition was identified by X-ray Diffraction (XRD, Rigaku Ultima IV) with Cu Kαradiation.A differential scanning calorimeter (DSC, METTLER 1100LF) was used to measure the phase transition in FZ.The range of testing temperature was from 50 °C to 650 °C with a heating rate of 10 °C/min under a shielding atmosphere of Ar gas.Corresponding DSC data were processed by a software Netzsch Proteus Thermal Analysis to calculate the temperature and heat flow of the phase transition.

    Fig.1.Schematic of (a) low-pressure sand casting process, (b) repair welding process, (c) repair welded joint, and (d) sampling location and geometry of the tensile specimen.

    The hardness profiles were attained through cross-sections of the joints via a Vickers hardness tester (VH, HV-300) with a load of 49N for 15 s.Tensile specimens were cut in the horizontal direction 1mm from the upper surfaces of the cast plates after welding, and Fig.1d shows the sampling location and geometry of the tensile specimen.Before the tensile test, the fusion zone was marked on the surfaces of these tensile samples for determining the fracture location after the failure.The tensile properties of the joints were measured at a constant strain rate of 1mm/min on a tensile machine(Zwick/Roell Z100) at room temperature.

    Fig.2.X-ray flaw detections of the repair welded joints fabricated with a welding current of (a) 150 A, (b) 170 A, (c) 190 A, and (d) 210 A.

    3.Results

    3.1.Macrostructural analysis

    Fig.2 shows the analyses of the X-ray computer tomography of the representative repaired joints fabricated with different welding currents.The forming defects of the repaired weld can be easily recognized by the X-ray with a penetration direction from the upper surface of the cast workpiece.From Fig.2a, there was incomplete fusion at the edge of circular weld with 150 A.With the increasing welding current, no obvious welding defects could be found at the welding current of 170 and 190 A.However, an aggregate welding porosity in size of ~2mm appeared in the weld at 210 A, as shown in Fig.2d.Moreover, it can be seen that the contrast of all the welds was darker in comparison to those of the BM under the X-ray inspection.

    The macrosection of the repair welded joints are shown in Fig.3.Although the dimensions of these blind holes before repairing were the same, the shapes and sizes of the welds were significantly different after welding with different welding currents.As the welding current increased, both of the penetration depth as well as the processed width were increased due to the increasing heat input.Meanwhile, the aspect ratios between the penetration depth and processed width of the repair welds also increased with the increase of welding current.Some key transition zones such as FZ, HAZ, and BM labeled in Fig.3 are the consequence of steep temperature variation in various regions.

    3.2.Microstructural analysis

    The microstructure of the sand-cast Mg-4Y-2Nd-1Gd-0.5Zr alloy is shown in Fig.4.The microstructure primarily consists of equiaxedα-Mg matrix surrounded by eutectic structure (Fig.4a), which is proved to be a dendrite growth mode.A small number of divorced eutectics can also be observed in the triple junction of grain boundaries.The average grain size of theα-Mg matrix was approximately 50μm.As depicted in the SEM images and corresponding elemental distribution maps (Fig.4b and c), the lamellar eutectic structures in network shape distributing along grain boundaries were mainly rich in Y, Nd, Gd, and Zr elements.

    Fig.5 exhibits the optical microstructures of FZ, HAZ of the joints performed at different welding currents.Different transition zones presented different organizational characteristics.Compared with the BM, the grain sizes in FZ were obviously refined, while grain sizes in HAZ near FZ were increased.The quantitative calculation of grain sizes of HAZ and FZ within different joints are shown in Fig.6, and the grain size (48μm) of the sand-cast alloy is shown as a horizontal black line for comparison.With the lowest welding current, the grain size of HAZ was just increased by 5μm compared with that of the BM.With the increase of the repair welding current, the grain sizes of the HAZ increased obviously, and reached the maximum value (79μm) at 210 A.In addition, the eutectic phases distributing along the grain boundaries became more and more continuous with coarser morphologies.However, the grain size of the center of FZfirstly decreased and then increased with the increasing welding current, achieving its minimum value (13μm) at 170 A.It is worth noting that at the lowest welding current of 150 A,some black particle aggregated at the grain boundaries in the FZ which were significantly different from those eutectic phases.But with the increase of the welding current, the number of black clusters decreased gradually.

    Fig.3.Macrographs of the repair welded joints repaired with a welding current of (a) 150 A, (b) 170 A, (c) 190 A, and (d) 210 A.

    Fig.4.(a) Optical and (b) SEM micrographs of low-pressure sand-cast alloy.(c) Corresponding EDS maps of SEM micrograph in (b).

    Fig.7 displays the SEM microstructures and corresponding EDS maps of the transition interface between HAZ and FZ of these joints.As the welding current increased, the eutectics presented in HAZ in the upper-left region of these SEM images became coarser, which was consistent with the analyses in Fig.5.At the same time, some bright white particles in the FZ in the lower-right region, which have been detected as the black clusters in the optical observation in Fig.5, were mainly rich in Zr and Y elements according to the EDS maps.The number of these bright white particles in the FZ also gradually decreased with the increase of welding current under SEM mode.Compared with the elemental distribution of the transition interface of 150 A (Fig.7a), Zr and Y elements were more evenly distributed in that of 210 A, as shown in the EDS maps in Fig.7d.

    Fig.8a-d show the SEM microstructures in the center of FZ.The bright white particle clusters also existed with the lowest welding current, which was in good agreement with the observation in Fig.7.From the images at high magnification and corresponding EDS analysis in Fig.8e and f, it can be concluded that these flocculent clusters should be Zr-Y phases.Except for these clusters, the eutectic structure was fewer in the FZ with the lower welding current (Fig.8a).However, with the increase of the current, semi-continuous corrosion pits appeared along the grain boundaries, which should be produced after the erosion of the eutectics during the etch process.This indicated that the eutectics were more likely to appear in FZ with a higher welding current.

    XRD patterns of the sand-cast alloy and FZ of the joints repaired with different welding currents are shown in Fig.9.After repair welding process, the phases detected in FZ were the same as that in the sand-cast state.All of the samples were composed ofα-Mg solid solution, Mg24(Gd, Y)5,Mg12Nd, Mg14Nd2Y, and Mg5(Gd, Y) intermetallic compounds (Fig.9a), indicating that there were no new phases generated in the welding process.However, theα-Mg matrix in FZ formed with different welding currents exhibited different positions of diffraction peaks.Taking the three strongest peaks ofα-Mg in Fig.9a as examples, all the diffraction angles of the peaks were lower than the standard values(Fig.9b).As the welding current increased, the peak positions ofα-Mg in FZ first shifted to left gradually, reaching the minimum values at 190 A.And then the peaks shifted to the right slightly when the welding current continuously increased to 210 A.It can be known from the Bragg’s law that the interplanar spacing ofα-Mg matrix in FZ increased first and then decreased with the increasing welding current.

    Fig.5.Optical microstructures of HAZ (a, c, e, g) and FZ (b, d, f, h) formed with different welding currents: (a, b) 150 A, (c, d) 170 A, (e, f) 190 A, and(g, h) 210 A.

    Fig.6.The calculation results of grain sizes of the HAZ and FZ within different joints.

    The DSC analyses of the BM and FZ are provided in Fig.10.According to the previous researches and Mg-REphase diagrams, the two endothermic reactions occurred at~540°C (labeled as B) and ~630°C (labeled as C) can be speculated to be the eutectic decomposition and the melting ofα-Mg matrix, respectively [3].Not only the cast alloy but also the FZ prepared at 210 A had eutectic decomposition in the DSC curves.Interestingly, another endothermic reaction with a wider temperature range started at ~350 °C (labeled as A) just in the four DSC curves of FZ.Table 3 shows the calculated heat flow value of the peaks A and B as well as the melting temperature ofα-Mg matrix in these curves.It can be seen that the melting temperature ofα-Mg first decreased and then increased with the increase of welding current, showing a minimum melting point (637.7°C) at the current of 190 A.

    Table 3Calculated heat flow value of the peaks A and B as well as the melting temperature of α-Mg.

    Fig.7.SEM micrographs and corresponding EDS maps of the transition zones between HAZ and FZ formed with different welding currents: (a) 150 A, (b)170 A, (c) 190 A, and (d) 210 A.

    Fig.8.SEM micrographs of the FZ formed with different welding currents: (a) 150 A, (b) 170 A, (c) 190 A, and (d) 210 A.(e) SEM image and corresponding EDS maps of the particle cluster in FZ with the welding current of 150 A.(f) is the EDS point analysis in (e).

    Fig.9.(a) XRD spectra of the BM and FZ in the joints with different welding currents.(b) XRD spectra with the scanning angle from 31° to 37° in (a).

    Fig.10.DSC analysis of the FZ in the joints repaired with different welding currents.

    Fig.11.Vickers hardness distributions of repair welded joints from FZ to BM.

    3.3.Vickers hardness and tensile properties

    Fig.11 shows the Vickers hardness profiles of the repaired joints.The hardness of the sand-cast alloy (69 HV) is exhibited as a horizontal black line for comparison.The Vickers hardness of the FZ in four repaired joints was higher than that of the sand-cast alloy.The average Vickers hardness of the FZ of the joint repaired with 150 A was 75 HV, and then realized the maximum value of 77HV at 170 A, which was 11.6% higher than that of the sand-cast state.However, as the current further increased to the maximum current of 210 A,the Vickers hardness was reduced apparently to 72 HV.Further, it can be seen that the widths of the FZ and HAZ were all increased gradually with the increasing current, and the larger the welding current, the more severe the softening of the HAZ.

    As shown in Fig.12a, the tensile tests were conducted to investigate the effects of welding current on the tensile properties of the repair welded joints.The comparison of 0.2% tensile yield strength (YS), ultimate tensile strength (UTS), and elongation (EL) values between the repaired joints (columns)as well as the sand-cast alloy (horizontal dotted lines) are shown in Fig.12b.With the increase of the welding current,the UTS of the repaired joints first increased from 178MPa(150 A) to the maximum value of 195MPa (170 A) withthe highest joint efficiency of 87.8% and then it decreased to 149MPa at 210 A.The YS values also showed the similar trend.What is more, the EL of the joints repaired at 170 A was 5.1%, which was unexpectedly higher than that of the sand-cast alloy by 24.4%.However, as the welding current increased to 210 A, the EL of the repaired joint was sharply reduced to 1.4%.

    Fig.12.(a) Engineering stress-strain curves and (b) tensile properties of the BM and repair welded joints repaired with different welding currents.

    Fig.13.(a) Fracture locations of the repair welded joints.(b-h) Tensile fractures of the BM and joints repaired with different welding currents: (b) BM, (d)150 A, (e) 170 A, (f) 190 A, (g, h) 210 A.(c) is the magnified view of the square region in (b) and (i) is EDS point analysis of the cluster in (d).

    3.4.Fracture behavior

    Fig.13a shows the failure locations of the repaired joints.It can be observed that the joints fabricated with the minimum (150 A) and maximum (210 A) currents all failed in FZ,while the joints of 170 and 190 A failed at HAZ.Fig.13b shows the SEM image of the typical fracture features of the sand-cast alloy at room temperature.The fracture surface exhibited a mixed characteristic of transgranular and intergranular fractures with some fractured eutectics structures, coarse dimples,and cleavage planes.The magnified view of the fractured eutectics structures with a lamellar shape is presented in Fig.13c.

    Due to the different failure locations, the tensile fracture surface of 150 A (Fig.13d, failed at FZ) shows much finer structure characteristics in comparison to those of 170 A and190 A (Fig.13e and f, all failed at HAZ).The fracture surface of the joint with 150 A consisted of many coarse dimples and tear ridges, with the main fracture characteristic of quasicleavage.Notably, some bright white clusters were observed at the torn grain boundary, the EDS point analysis (Fig.13i)proved that they were Zr-Y particles which have also been observed in OM (Fig.5) and SEM (Fig.8) images in the FZ repaired at 150 A.Although both the joints with 170 A and 190 A were broken at HAZ, their fracture morphologies were significantly different.The fracture surface of the joint formed with 170 A was characterized by some fractured eutectics structures, cleavage planes, and a small number of dimples, which showed a similar fracture mode with the BM in Fig.13b.However, the joint of 190 A exhibited a relatively flat fracture surface comprised of more fractured eutectic structures and river patterns, suggesting the main fracture characteristic of brittle cleavage fracture.As can be seen in Fig.13g, the macro fracture surface of the joint fabricated with 210 A could be divided into two regions with different fracture characteristics, distinguished by the yellow dotted line.The upper left region containing an aggregate welding porosity shows a finer fracture structure than the lower right region, which demonstrated that the upper left region located in FZ while the lower right region was HAZ.It can be speculated that the cracks may initiate near the welding porosity in FZ, then propagate toward HAZ in the lower right corner as indicated by the yellow arrows, and finally resulting in the fracture failure, which was in accordance with the lowest elongation of 1.4%.

    Fig.14 exhibits optical micrographs of the longitudinal sections of these ruptured tensile samples.As mentioned above,the failure modes of the BM(Fig.14a)and the joint repaired at 170 A(Fig.14c)all showed the coexistence of transgranular and intergranular fracture.Fig.14b and d present the initiation and propagation process of the cracks, it can be seen that the cracks initiated in the eutectic structures along grain boundaries and then propagated toward the interior of the grain.However, because of the much coarser grains surrounded by continuous eutectics in HAZ of the joint repaired with 190 A, the crack primarily grown along the brittle eutectics, as shown in Fig.14f.Obviously, the tensile failure in FZ of the joints with 150 A (Fig.14g) and 210 A (Fig.14h)is mainly transgranular fracture.It is worth noting that some of the cracks in Fig.14g was generated near the clusters at grain boundary which have been detected in Fig 13d, indicating that these clusters may be detrimental to the mechanical properties of the repaired joint.

    4.Discussion

    In addition to the heat input, the grain size of FZ was also affected by the existence of Zr which has been considered as a dominant grain refiner for a range of commercial magnesium alloys [24-26].Therefore, it is necessary to detect the existence forms of Zr in FZ fabricated with different welding currents.Table 4 exhibits the compositions including the content of Zrsof FZ in the repaired joints.It can beseen that with the increase of welding current, the ratio of the content of solute Zr to the total Zr content increased and became closer to 1.This is because the temperature of the molten pool was higher with a larger welding current, so the diffusion rate of Zr atoms from the surface of Zr particles into the liquid phase was increased simultaneously.Secondly,as the heat was conducted from the molten pool to the BM during repair welding, and the larger the current, the higher the temperatures of BM and FZ, resulting in a lower cooling rate of the molten pool [31,33].After the extinction of the arc, the residence time of the molten pool at high temperature would be prolonged, therefore it provided a more sufficient time for the Zr diffusion.Thirdly,the disturbance effect of the arc also played a significant role in the dispersion of the Zr particles; the agglomerated Zr particles could be dispersed by the stronger arc force with a higher welding current, which can further facilitate the dissolution of the clusters.As a result, it can be seen from Figs.5, 7, and 8 that the number density of Zr clusters decreased apparently as the welding current increased from 150 to 210 A.That is, with the increasing welding current, the content of Zrpin FZ gradually decreased, while the content of Zrsincreased.

    Table 4Actual compositions of FZ in the four joints analysed by ICP-AES (wt%).

    XRD results in Fig.9 show that the three strongest peaks of theα-Mg matrix gradually shifted to lower diffraction angle values with the increasing welding current from 150 to 190 A.This suggests that the Zr clusters were dissolved to be Zrsin a higher welding current, and then Zrswas retained in the matrix under the condition of rapid cooling of the molten pool, leading to the formation of a supersaturated solid solution in FZ.According to Bragg’s law, the lattice distortion and crystal plane spacing of theα-Mg matrix increased with the increasing welding current, so the corresponding diffraction angle decreased.However, when the current was further increased to 210 A, the BM was heated to a higher temperature, thus it started to have negative impacts on the cooling rate of FZ.During the relatively slow solidification procedure with the highest welding current, theα-Mg dendrites in FZ could continuously discharge solute atoms into the intergranular residual liquid,which increased the content of alloying elements in the liquid phase [3].Eventually, the semi-continuous eutectic structures were obtained along theα-Mg grain boundaries, as confirmed by the corrosion pits at the grain boundaries in Fig.8.Due to the consumption of the solute elements in eutectic structures, the solid solubility of the matrix was reduced, leading to a decrease in the interplanar spacing and an increase of the diffraction angle value in XRD analysis.

    Fig.14.Optical micrographs of the longitudinal section of the fracture surface of BM and joints repaired with different welding currents: (a) BM, (c) 170 A,(e) 190 A, (g) 150 A, (h) 210 A.(b), (d) and (f) is the magnified view of the square region in (a), (c) and (e), individually.

    Based on the DSC analyses in Fig.10 and the corresponding quantitative calculation in Table 3, only the sample cut from FZ of 210 A showed an obvious heat flow at ~540°C.This indicated that except for the FZ of 210 A, the number of the eutectics was very low in the other three samples fabricated with lower currents.On the other hand, the melting point of theα-Mg matrix with the welding current from 150 to 190 A showed a decreasing tendency, indicating that the solid solubility of the matrix was gradually increased with the increasing current [34].That is, more alloying elements were dissolved into the matrix in FZ with the lower three currents rather than used to form eutectic structures, which wasconsistent with the XRD analyses.As the current further increased to 210 A, the solid solubility in the matrix was then reduced on account of the formation of eutectic structures,thus resulting in a slight increase in the melting point of the matrix.The endothermic peaks (like peak A) that occurred before eutectic decomposition also have been detected in the DSC of some solution-treated alloys, which could be ascribed to the dissolution of the precipitates [35,36].Due to the rapid cooling of the molten pool, a large number of solute elements could be dissolved into theα-Mg matrix in FZ, leading to the formation of the non-equilibrium microstructures [37].Similarly, during the heating process of the DSC test, theβ1andβphases precipitated first and then were dissolved at a higher testing temperature, resulting in the formation of endothermic peak A [35].In contrast, the relatively slow cooling rate of the sand-cast alloy resulted in the lower solid solubility of the matrix, thus there was no reaction peak before the eutectic decomposition.

    Fig.15.Mechanism schematics of the microstructure formation in molten pools formed with different welding currents: (a-c) 150 A, (d-f) 170 A, (g-i)210 A.

    Fig.15 illustrated the mechanism schematics of the microstructure evolution in the molten pools.Because of the minimum heat input with the welding current of 150 A, a large number of Zr particles cannot be dissolved to produce the constitutional supercooling effect due to the low temperature of the molten pool.On the other hand, the size of the Zr particle as a heterogeneous nucleus is also a key factor for the grain refinement [30,34].It was difficult for the Zr cluster with a large size to act as the effective heterogeneous nucleus in the molten pool.These above two factors all reduced the refinement effect of Zr in the repaired weld.With the growth ofα-Mg dendrites,these Zr clusters would be pushed towards the grain boundaries after solidification of FZ, as shown in Figs.8a and 15c.

    As exhibited in Fig.15d-f, as the welding current increased to 170 A, some of the Zr clusters were dissolved into the liquid phase and transformed to be Zrs.A large number of previous works have demonstrated that Zrsprovided constitutional supercooling for the nucleation ofα-Mg dendrites on undissolved Zrpand actually a major contribution to grain refinement was provided by Zrs[30,32].The refinement effectiveness of solute elements is determined by its growthrestriction factorQwhich can be expressed as [32]:

    where the subscriptirepresents different alloy,miandkiis the slope of the liquidus and the solute partition coefficient of the corresponding binary phase diagram, respectively.Cimeans the solute content of the binary alloy.Alloying elements with higherQvalue have better grain refinement effect through constitutional supercooling.The values ofm(k?1) for Y and Zr used for this calculation were 1.7 and 38.3[32,38],thus Zr showed a much better refinement effect than Y.As a result,the grain size in FZ decreased from 20μm to 13μm when the welding current increased from 150 to 170 A.

    However, although increasing the welding current would lead to a more complete dissolution of the residual Zr particles, the higher heat input applied to FZ reduce the cooling rate of the molten pool, as mentioned above.At this point,the lower cooling rate became the dominated factor of the grain size, which led to the coarsening of the grain and even the formation of the eutectic structures along the grain boundaries at 210 A, as shown in Figs.8d and 15i.Furthermore,aggregate welding porosity also appeared in FZ, due to the air indraft in the molten pool at higher temperatures.

    Due to the higher cooling rate of the weld, FZ in the repaired joint possessed a smaller grain size with a higher solid solubility of the matrix than those of the BM [19,22].The resulting strong grain boundary strengthening and solid solution strengthening lead to the higher hardness of the repaired weld in comparison to that of the BM [39,40].As the current was increased to 170 A, Zr clusters in the molten pool with a higher temperature were transformed into Zrsto refine the grain size to the minimum (13μm), so the hardness of FZ was increased from 75 HV (at 150 A) to 77 HV (at 170 A).However, the cooling rate of FZ decreased with the further increase in the current, and the grains began to coarsen.Especially in the FZ formed with 210 A, the eutectic structures formed along the grain boundaries decreased the solid solubility of theα-Mg matrix, which would weaken the above two strengthening mechanisms.Therefore, the hardness of FZ fabricated with 210 A was drastically reduced to 72 HV.

    During the repair welding process, the grain coarsening occurred in the regions near the molten pool to reduce the interfacial energy, resulting in the formation of HAZ [31,41].Moreover, when the temperature of the HAZ was above the melting point of the low-melting eutectics, these eutectics along the grain boundaries were melted locally and then solidified again.In addition, the eutectic structures in HAZ would become more continuous due to the lower volume fraction of the grain boundaries after the grain coarsening, as shown in Fig.5.Previous researchers believed that this microstructure with the characteristic of coarse grains surrounded by continuous eutectics possessed lower intergranular bonding strength,weakening the hardness of HAZ [14].From the DSC analysis in Fig.10, the critical temperature for the decomposition of the eutectics was 540°C.As the welding current increased,the area of the BM affected by heating effect became larger,leading to a wider HAZ.Therefore, as the welding current was increased from 150 to 210 A, the width of the HAZ was increased from 1mm to 2.5mm, and the minimum hardness in HAZ was also reduced from 67 HV to 62 HV.

    The joint of 150 A contained incomplete fusion defects in the repaired weld, as demonstrated in the X-ray flaw detections in Fig.2a.Some Zr clusters were also exposed to the fracture surface in Fig.13d, confirming the poor bonding force between the cluster and the matrix.These two factors deeply deteriorated the mechanical properties of the joint repaired with 150 A;the EL of this joint was only 2.5%,and the tensile fracture located in the FZ(Fig.13a).The joint repaired at 210 A also exhibited a similarly poor UTS of 149MPa and even lower EL of 1.4% owing to the welding porosity with a large size generated in the FZ during the welding (Fig.13g).

    Well-formed repair welded joints have been obtained by proper heat inputs at 170 and 190 A; there were no obvious welding defects inspected from the X-ray detections, thus the mechanical properties of the repaired joints were higher than those of the others.Moreover,the number of Zr clusters in FZ of 170 A and 190 A were significantly reduced, resulting in the lower probability of crack initiation in FZ.To investigate the reason of different fracture locations in the repaired welds of 170 and 190 A, grain boundary strengthening in the three regions were estimated by Hall-Petch relationship [42]:

    whereσ0is the friction stress free from grain boundary contributions,kyis the stress concentration factor, anddis the average grain diameter.The constantkyfor this alloy was estimated to be 250MPa μm1/2[7].Taking the joint of 170 A for an example, the contribution of grain boundary strengthening in FZ, HAZ, and BM was 35.7MPa, 30.8MPa, and 69.3MPa,respectively.It can be seen that HAZ may be the weakest region in the whole joint due to the presence of coarser grains surrounded by continuous eutectics.This is the reason why both the joints of 170 and 190 A were fractured in the HAZ and the joint of 190 A even showed a slightly lower mechanical performance than that of the 170 A.Moreover, many researches illustrated that continuous eutectics can function as crack initiation sites during tensile tests [3, 7], seriously reducing the ductility of the sample.Although the UTS of the repaired joint with 170 A was only 87.8% of the sand-cast BM, the EL of the joint was surprisingly higher than the BM by 24.4%.The improvement of the EL could be attributed to that the fine grains in FZ restrained the crack initiation during the tensile process by affording more deformation before the fracture failure.

    As shown in Fig.13b and c, the sand-cast alloy exhibited fractured eutectic structures, which was consistent with the optical microstructure of the longitudinal section of the fracture surface (Fig.14a and b).This reconfirmed the poor combination between the eutectic structures and theα-Mg grains[7, 34, 43].The joints repaired with 150 and 210 A were all broken in FZ due to the welding defects.Compared with the sand-cast BM, the microstructure of FZ showed fewer eutectic structures thus stronger intercrystalline bonding force.Therefore, the longitudinal section of the fracture surface of150 and 210 A all exhibited obvious transgranular fracture characteristics (Fig.14g and h).It is worth noting that the Zr clusters, which may act as crack initiators, deteriorated the ductility of the repaired joint [30].So these cracks in the FZ of 150 A tended to initiate near the Zr clusters at the grain boundaries, and then gradually propagated into the interior of grains, which was different from the failure procedure in the joint of 210 A.

    Although both the joints of 170 and 190 A were failed at HAZ, the grain coarsening occurred in HAZ of the 170 A was not as severe as that of the 190 A, and the eutectic structure in HAZ of 170 A was semi-continuous.Therefore, the failure mode in the repaired joint of 170 A was similar to that of the sand-cast alloy with a mixed feature of transgranular and intergranular fracture.When the welding current was increased to 190 A,coarser grains surrounded by more continuous eutectics in HAZ were attained by the higher heat input[31].The cracks initiated at the interface between the eutectics and matrix, and then mostly developed along the continuous eutectics, leading to the main characteristic of intergranular fracture (Fig.14e and f) [3, 7].Therefore, there were much more fractured eutectics and river patterns appeared in the fracture surface with a relatively flat morphology (Fig.13f).The continuous brittle eutectics in HAZ were also the main reason for the cracks to propagate to the HAZ from FZ in the joint of 210 A, as mentioned in Fig.13g.

    5.Conclusions

    This research verified the feasibility of repair welding in sand-cast Mg-4Y-2Nd-1Gd-0.5Zr alloy by TIG welding,and the qualities of the repaired joints were evaluated in terms of the microstructure evolutions and mechanical properties.The following conclusions can be drawn:

    1.Some welding defects of incomplete fusion and welding porosity were generated in the fabricated welds with the current of 150 and 210 A, respectively, while the defectfree repaired joints with good appearance could be acquired at 170 and 190 A.

    2.With the welding current increased of from 150 to 210 A,the mechanical properties of the TIG repair welds of sandcast Mg-4Y-2Nd-1Gd-0.5Zr alloy frist increased and then decreased, showing a maximum tensile strength of 195MPa with the joint effciiency of 87.8% at 170 A, and the elongation reached 124.4% of the original sand-cast alloy.

    3.Although there was no obvious grain coarsening that occurred in the HAZ of the repaired joint fabricated with 150 A, not only incomplete fusion defects existed in the weld, but also some Zr clusters were observed along the grain boundaries, which deteriorated the mechanical properties of the repaired joint.

    4.The grain size of FZ in Mg-4Y-2Nd-1Gd-0.5Zr alloy was determined by the combination of the cooling rate and the existence forms of Zr.Although increasing the welding current could reduce the cooling rate of the molten pool,it also facilitated the transformation of Zr particles to Zr solute which provided constitutional supercooling for the grain refinement.Thus the minimum grain size (13μm)was obtained in the FZ of 170 A.

    5.Obvious grain coarsening and continuous eutectic structures occurred in HAZ above the welding current of 190 A,resulting in the intergranular fracture in HAZ.A small number of eutectics also be detected in the FZ as the welding current further increased to 210 A.

    Declaration of Competing Interest

    The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

    Acknowledgments

    This research was supported by the National Natural Science Foundation of China (Nos.51775334 and 51821001),the National Key Research & Development Program of China(No.2016YFB0701205) and the National Science and Technology Innovation Special Zone Project (No.002-002-01).

    午夜福利视频精品| 这个男人来自地球电影免费观看 | 亚洲性久久影院| a级毛色黄片| 人妻少妇偷人精品九色| 国产高清有码在线观看视频| 一级片'在线观看视频| 精品国产乱码久久久久久小说| a级毛片在线看网站| 大片电影免费在线观看免费| 又大又黄又爽视频免费| 久久久亚洲精品成人影院| 亚洲国产精品一区二区三区在线| 天堂中文最新版在线下载| 亚洲成人av在线免费| 欧美老熟妇乱子伦牲交| 久久久a久久爽久久v久久| 亚洲av在线观看美女高潮| 麻豆成人午夜福利视频| 久久国产亚洲av麻豆专区| 视频中文字幕在线观看| 黑人猛操日本美女一级片| 一级片'在线观看视频| 久久久久精品久久久久真实原创| 欧美日韩在线观看h| 亚洲精品久久久久久婷婷小说| 亚洲激情五月婷婷啪啪| 一区二区三区精品91| 一个人看视频在线观看www免费| 少妇被粗大的猛进出69影院 | 高清视频免费观看一区二区| 熟女av电影| 午夜影院在线不卡| 久久精品国产亚洲av天美| 日韩一区二区三区影片| 最近2019中文字幕mv第一页| 亚洲av免费高清在线观看| 欧美丝袜亚洲另类| 蜜桃久久精品国产亚洲av| 麻豆乱淫一区二区| 日韩一区二区三区影片| 亚洲精品第二区| 国产日韩欧美视频二区| 纯流量卡能插随身wifi吗| 国产精品蜜桃在线观看| 国产精品蜜桃在线观看| 在线观看www视频免费| 最近2019中文字幕mv第一页| 亚洲欧美日韩另类电影网站| 国产精品久久久久久精品古装| 99热全是精品| 亚洲图色成人| 黄色欧美视频在线观看| 精品亚洲乱码少妇综合久久| 国产成人aa在线观看| 自线自在国产av| 国产在线男女| 成人亚洲精品一区在线观看| 亚洲精品久久久久久婷婷小说| 最近最新中文字幕免费大全7| 一级毛片电影观看| 一本大道久久a久久精品| 久久久久国产精品人妻一区二区| 亚洲国产成人一精品久久久| 丁香六月天网| 久久鲁丝午夜福利片| 日韩欧美 国产精品| 国产真实伦视频高清在线观看| 我的女老师完整版在线观看| 国产高清国产精品国产三级| 日日爽夜夜爽网站| 亚洲四区av| 久久精品夜色国产| 99热这里只有精品一区| 久久av网站| 寂寞人妻少妇视频99o| 如日韩欧美国产精品一区二区三区 | 国产欧美日韩综合在线一区二区 | 能在线免费看毛片的网站| 人妻系列 视频| 纯流量卡能插随身wifi吗| av专区在线播放| www.av在线官网国产| 国产精品一区二区在线观看99| 国产精品.久久久| 99视频精品全部免费 在线| 国产精品偷伦视频观看了| 在线观看三级黄色| 亚洲色图综合在线观看| 下体分泌物呈黄色| a级毛色黄片| 国产淫片久久久久久久久| 老司机影院成人| 狂野欧美白嫩少妇大欣赏| 精品99又大又爽又粗少妇毛片| 赤兔流量卡办理| 黑丝袜美女国产一区| 亚洲欧美精品专区久久| 777米奇影视久久| 久久久久久久久久久丰满| 99热6这里只有精品| 亚洲图色成人| 尾随美女入室| 人妻夜夜爽99麻豆av| 欧美精品一区二区免费开放| 一级毛片 在线播放| 视频区图区小说| 精品久久国产蜜桃| 18禁在线无遮挡免费观看视频| 免费在线观看成人毛片| 日本91视频免费播放| 麻豆成人av视频| 成人毛片60女人毛片免费| 26uuu在线亚洲综合色| 色哟哟·www| 精品久久久精品久久久| 国产精品嫩草影院av在线观看| 午夜精品国产一区二区电影| 蜜桃在线观看..| 亚洲av日韩在线播放| 2022亚洲国产成人精品| 精华霜和精华液先用哪个| 国产精品免费大片| 人妻人人澡人人爽人人| 亚洲精品第二区| 欧美丝袜亚洲另类| av线在线观看网站| 日韩欧美一区视频在线观看 | 一边亲一边摸免费视频| 国产成人a∨麻豆精品| 一级av片app| a级片在线免费高清观看视频| 日本黄大片高清| 日韩制服骚丝袜av| 天堂8中文在线网| 在线免费观看不下载黄p国产| 国产一区有黄有色的免费视频| h日本视频在线播放| 黄片无遮挡物在线观看| 色哟哟·www| 国产老妇伦熟女老妇高清| 国产深夜福利视频在线观看| 不卡视频在线观看欧美| 国产极品天堂在线| 男女边吃奶边做爰视频| 免费观看的影片在线观看| 亚洲精品乱码久久久v下载方式| 国产日韩欧美在线精品| 夫妻性生交免费视频一级片| 国产精品福利在线免费观看| √禁漫天堂资源中文www| 美女cb高潮喷水在线观看| 晚上一个人看的免费电影| 伦精品一区二区三区| 国产黄色免费在线视频| 国产精品免费大片| 国产精品嫩草影院av在线观看| av线在线观看网站| 国产精品.久久久| 亚洲天堂av无毛| 久久人人爽av亚洲精品天堂| 国产 精品1| 精品久久久噜噜| 久久久久久久久久久免费av| 婷婷色综合大香蕉| 日韩强制内射视频| 简卡轻食公司| 亚洲第一av免费看| 免费观看在线日韩| 日韩大片免费观看网站| 王馨瑶露胸无遮挡在线观看| 婷婷色av中文字幕| 人妻一区二区av| 只有这里有精品99| 亚洲精品国产成人久久av| 男人爽女人下面视频在线观看| 观看免费一级毛片| 色94色欧美一区二区| 日韩不卡一区二区三区视频在线| 中文字幕av电影在线播放| 另类精品久久| 国产精品不卡视频一区二区| 国产永久视频网站| 九色成人免费人妻av| 曰老女人黄片| 美女中出高潮动态图| 男女免费视频国产| 国产精品人妻久久久影院| 精品少妇内射三级| 妹子高潮喷水视频| 亚洲精品一二三| 日韩一本色道免费dvd| 国产国拍精品亚洲av在线观看| 国产老妇伦熟女老妇高清| 国产免费又黄又爽又色| 欧美三级亚洲精品| 女人精品久久久久毛片| 久久韩国三级中文字幕| 熟妇人妻不卡中文字幕| 欧美激情极品国产一区二区三区 | 91精品一卡2卡3卡4卡| 这个男人来自地球电影免费观看 | 大片电影免费在线观看免费| 日韩亚洲欧美综合| 91成人精品电影| 国产精品久久久久久久电影| 色婷婷av一区二区三区视频| 18禁在线无遮挡免费观看视频| av线在线观看网站| 久久久久国产网址| 亚洲天堂av无毛| 日日爽夜夜爽网站| 极品教师在线视频| 久久久久久久久久成人| 亚洲精品自拍成人| 亚洲精品国产色婷婷电影| 久久人人爽人人片av| 亚洲国产精品999| 色视频www国产| 精品视频人人做人人爽| 久久久久久久久久久久大奶| 久久午夜综合久久蜜桃| 国产一级毛片在线| 久久精品国产亚洲av涩爱| 少妇人妻一区二区三区视频| 91在线精品国自产拍蜜月| 特大巨黑吊av在线直播| 国产精品.久久久| 久久精品久久久久久噜噜老黄| 亚洲情色 制服丝袜| 青春草国产在线视频| 久久av网站| 日本色播在线视频| 日日摸夜夜添夜夜爱| 国产深夜福利视频在线观看| 99精国产麻豆久久婷婷| 色吧在线观看| 日韩亚洲欧美综合| 午夜免费观看性视频| 日韩av在线免费看完整版不卡| 亚洲欧洲精品一区二区精品久久久 | 熟女电影av网| 亚洲成人av在线免费| av免费在线看不卡| 国产精品嫩草影院av在线观看| 久热这里只有精品99| 这个男人来自地球电影免费观看 | 久久久久视频综合| 简卡轻食公司| 亚洲精品乱码久久久v下载方式| 欧美+日韩+精品| 一区二区av电影网| 国产亚洲精品久久久com| 80岁老熟妇乱子伦牲交| 免费人妻精品一区二区三区视频| 偷拍熟女少妇极品色| 极品教师在线视频| 免费av不卡在线播放| 大码成人一级视频| 色婷婷久久久亚洲欧美| 午夜免费观看性视频| 91aial.com中文字幕在线观看| 亚洲,一卡二卡三卡| 亚洲国产精品国产精品| 你懂的网址亚洲精品在线观看| 免费久久久久久久精品成人欧美视频 | 国产午夜精品一二区理论片| 街头女战士在线观看网站| 亚洲色图综合在线观看| av在线app专区| 国产免费一级a男人的天堂| 国产一区亚洲一区在线观看| 精品一区二区三区视频在线| 另类亚洲欧美激情| 成人黄色视频免费在线看| 18禁在线无遮挡免费观看视频| 免费少妇av软件| 亚洲精品久久久久久婷婷小说| 亚洲色图综合在线观看| 国产色爽女视频免费观看| 男女边摸边吃奶| 高清不卡的av网站| 国产日韩欧美亚洲二区| 国产免费一级a男人的天堂| 99九九线精品视频在线观看视频| 久久久久久久国产电影| 一级毛片黄色毛片免费观看视频| 少妇的逼好多水| 国产中年淑女户外野战色| 日本黄色日本黄色录像| 国产成人免费观看mmmm| 国产精品99久久99久久久不卡 | 成人美女网站在线观看视频| 婷婷色麻豆天堂久久| 啦啦啦中文免费视频观看日本| 涩涩av久久男人的天堂| 国产黄色免费在线视频| 久久韩国三级中文字幕| 国产色婷婷99| 久久久亚洲精品成人影院| 日本爱情动作片www.在线观看| 亚洲国产毛片av蜜桃av| 亚洲精品久久久久久婷婷小说| 国产免费视频播放在线视频| 狠狠精品人妻久久久久久综合| tube8黄色片| 欧美精品人与动牲交sv欧美| 人人妻人人添人人爽欧美一区卜| 日日啪夜夜爽| 在线观看av片永久免费下载| 久久人人爽av亚洲精品天堂| 极品教师在线视频| 亚洲成人av在线免费| 大码成人一级视频| 欧美3d第一页| 91午夜精品亚洲一区二区三区| 国产成人91sexporn| 美女cb高潮喷水在线观看| 精品人妻一区二区三区麻豆| 午夜视频国产福利| 91午夜精品亚洲一区二区三区| av网站免费在线观看视频| 日本猛色少妇xxxxx猛交久久| 婷婷色综合www| 午夜影院在线不卡| 亚洲欧美精品自产自拍| 日韩av免费高清视频| 99久久精品国产国产毛片| 日韩一区二区视频免费看| 国产精品国产三级专区第一集| 亚洲色图综合在线观看| 精品亚洲成国产av| av网站免费在线观看视频| 啦啦啦中文免费视频观看日本| 极品少妇高潮喷水抽搐| 国产免费福利视频在线观看| kizo精华| 国产在线男女| 国产成人91sexporn| 韩国av在线不卡| 久久久久久久久久人人人人人人| 成人特级av手机在线观看| 在线亚洲精品国产二区图片欧美 | 在线天堂最新版资源| 午夜激情久久久久久久| 在线 av 中文字幕| 伦精品一区二区三区| 国产精品秋霞免费鲁丝片| 色视频www国产| 亚洲精品自拍成人| 少妇 在线观看| 亚洲国产精品一区二区三区在线| 99久国产av精品国产电影| 色网站视频免费| 美女福利国产在线| 国产精品一区二区在线观看99| 国精品久久久久久国模美| 亚洲,欧美,日韩| 91久久精品国产一区二区三区| 久久国产精品男人的天堂亚洲 | 国产黄色免费在线视频| 99热6这里只有精品| 22中文网久久字幕| 丝袜脚勾引网站| 寂寞人妻少妇视频99o| 一级毛片我不卡| 看十八女毛片水多多多| 亚洲高清免费不卡视频| 亚洲无线观看免费| 美女xxoo啪啪120秒动态图| 欧美高清成人免费视频www| 少妇的逼好多水| 欧美97在线视频| 国产一区亚洲一区在线观看| 成人综合一区亚洲| 有码 亚洲区| 一级毛片aaaaaa免费看小| 亚洲自偷自拍三级| 青春草视频在线免费观看| 精品午夜福利在线看| 亚洲国产毛片av蜜桃av| 国产亚洲91精品色在线| 大又大粗又爽又黄少妇毛片口| 成人国产av品久久久| 国产日韩欧美亚洲二区| 成人国产av品久久久| 午夜免费观看性视频| 2018国产大陆天天弄谢| 久久久精品免费免费高清| 久久久国产一区二区| 大又大粗又爽又黄少妇毛片口| 在线观看三级黄色| av专区在线播放| 男女边吃奶边做爰视频| 欧美高清成人免费视频www| 亚洲欧洲精品一区二区精品久久久 | 99热全是精品| 欧美精品一区二区免费开放| 欧美日韩亚洲高清精品| 又大又黄又爽视频免费| 亚洲av在线观看美女高潮| 精品久久久久久电影网| 丝袜喷水一区| 一级片'在线观看视频| 亚洲三级黄色毛片| √禁漫天堂资源中文www| 精品视频人人做人人爽| 激情五月婷婷亚洲| 日韩在线高清观看一区二区三区| 一级毛片久久久久久久久女| 精品少妇黑人巨大在线播放| 亚洲色图综合在线观看| 夫妻性生交免费视频一级片| 免费观看的影片在线观看| 亚洲欧美一区二区三区黑人 | 日韩av不卡免费在线播放| 最近2019中文字幕mv第一页| 蜜臀久久99精品久久宅男| 99热全是精品| 成人黄色视频免费在线看| 晚上一个人看的免费电影| 欧美日韩精品成人综合77777| 免费看日本二区| 亚洲天堂av无毛| 在线亚洲精品国产二区图片欧美 | 国产成人a∨麻豆精品| 国产精品一区二区在线观看99| videossex国产| 全区人妻精品视频| 曰老女人黄片| 久久久亚洲精品成人影院| 午夜福利影视在线免费观看| 久久久久国产网址| 亚洲国产精品一区三区| av专区在线播放| 亚洲国产精品专区欧美| 欧美 日韩 精品 国产| 交换朋友夫妻互换小说| 国产在视频线精品| 国产精品.久久久| 成人漫画全彩无遮挡| 精品久久久噜噜| 亚洲美女视频黄频| 欧美3d第一页| 婷婷色麻豆天堂久久| 国产精品久久久久成人av| 亚洲国产日韩一区二区| 久久综合国产亚洲精品| 午夜免费男女啪啪视频观看| 午夜久久久在线观看| 久久久国产欧美日韩av| 亚洲欧洲国产日韩| 国产精品伦人一区二区| 欧美亚洲 丝袜 人妻 在线| 精品一区二区三区视频在线| 免费观看av网站的网址| 一区二区三区乱码不卡18| 成年人免费黄色播放视频 | 妹子高潮喷水视频| 国产精品国产三级专区第一集| 超碰97精品在线观看| 只有这里有精品99| 99热这里只有精品一区| 大码成人一级视频| 蜜桃在线观看..| 国产高清有码在线观看视频| 99视频精品全部免费 在线| 国产淫片久久久久久久久| 最新的欧美精品一区二区| 欧美 日韩 精品 国产| 亚洲综合色惰| 一级毛片aaaaaa免费看小| 一级二级三级毛片免费看| www.av在线官网国产| 一级毛片我不卡| 91久久精品电影网| 日本黄色片子视频| 精品一区二区免费观看| 大又大粗又爽又黄少妇毛片口| 久久午夜综合久久蜜桃| 国产黄片美女视频| 成年人午夜在线观看视频| 最新的欧美精品一区二区| 中文字幕制服av| 一级毛片 在线播放| 久久狼人影院| 美女xxoo啪啪120秒动态图| 国产黄片美女视频| 女性被躁到高潮视频| 蜜臀久久99精品久久宅男| 精品99又大又爽又粗少妇毛片| 爱豆传媒免费全集在线观看| 国产一区二区三区综合在线观看 | 成人18禁高潮啪啪吃奶动态图 | 免费观看av网站的网址| 免费在线观看成人毛片| 精品国产一区二区久久| 亚洲三级黄色毛片| 校园人妻丝袜中文字幕| 国产精品久久久久久久电影| 麻豆乱淫一区二区| 亚洲美女视频黄频| 久久这里有精品视频免费| 亚洲精品久久午夜乱码| 国产精品久久久久久久电影| 亚洲va在线va天堂va国产| 人体艺术视频欧美日本| 一本久久精品| 99国产精品免费福利视频| 亚洲欧美精品自产自拍| 久久久久久伊人网av| av在线老鸭窝| 久久久久久伊人网av| 国产精品蜜桃在线观看| 精品久久久久久久久亚洲| 国产精品久久久久久精品古装| 国产精品福利在线免费观看| 亚洲国产欧美日韩在线播放 | 性色avwww在线观看| h日本视频在线播放| 在线观看三级黄色| 日本91视频免费播放| 成人国产麻豆网| 亚洲欧美日韩另类电影网站| 色94色欧美一区二区| 青春草亚洲视频在线观看| 免费黄频网站在线观看国产| 一本色道久久久久久精品综合| av在线app专区| 少妇人妻 视频| 亚洲精品乱码久久久v下载方式| 亚洲欧洲国产日韩| 特大巨黑吊av在线直播| 日韩精品有码人妻一区| 亚洲精品国产av蜜桃| 欧美日韩视频精品一区| 久久精品久久久久久久性| 日本色播在线视频| 亚洲人成网站在线播| 久久久久精品久久久久真实原创| 特大巨黑吊av在线直播| 亚洲精品亚洲一区二区| 国产 精品1| 在线看a的网站| 成年人午夜在线观看视频| 肉色欧美久久久久久久蜜桃| 亚洲va在线va天堂va国产| 久久国产精品大桥未久av | 欧美高清成人免费视频www| 日韩强制内射视频| 秋霞伦理黄片| 国产精品欧美亚洲77777| 国产淫语在线视频| 精品午夜福利在线看| 亚洲国产毛片av蜜桃av| 爱豆传媒免费全集在线观看| 免费少妇av软件| 日韩三级伦理在线观看| 国产免费又黄又爽又色| 国产亚洲91精品色在线| 久久久精品免费免费高清| 黑人猛操日本美女一级片| 在线播放无遮挡| 午夜免费鲁丝| 少妇高潮的动态图| 久久99热这里只频精品6学生| 久久国产精品大桥未久av | 亚洲av成人精品一二三区| 秋霞伦理黄片| 啦啦啦视频在线资源免费观看| 国产成人精品无人区| 极品教师在线视频| 一级片'在线观看视频| 大香蕉久久网| 中文乱码字字幕精品一区二区三区| 日韩中字成人| 日韩一区二区视频免费看| 少妇猛男粗大的猛烈进出视频| 在线观看av片永久免费下载| 亚洲国产精品国产精品| 国产精品一区二区在线不卡| 欧美区成人在线视频| 另类精品久久| 日韩三级伦理在线观看| 免费大片黄手机在线观看| 亚洲欧美一区二区三区国产| 亚洲国产av新网站| 97超碰精品成人国产| 亚洲欧美清纯卡通| 五月伊人婷婷丁香| 午夜视频国产福利| 18禁在线无遮挡免费观看视频| 只有这里有精品99| 国产色爽女视频免费观看| 免费观看性生交大片5| 天天躁夜夜躁狠狠久久av| 99久久人妻综合| 久久综合国产亚洲精品| 人妻夜夜爽99麻豆av| 久久久久久久国产电影| 噜噜噜噜噜久久久久久91| 欧美区成人在线视频| 另类精品久久| 一级a做视频免费观看| 国产男女超爽视频在线观看| 99热这里只有是精品在线观看| 亚洲av福利一区| 欧美激情极品国产一区二区三区 | 春色校园在线视频观看| 午夜av观看不卡| 精品久久久噜噜| av卡一久久| 黄片无遮挡物在线观看| 精品一区二区三卡| 18禁在线无遮挡免费观看视频|