    Study of galvanic corrosion and mechanical joint properties of AZ31B and carbon-fiber-reinforce polymer joined by friction self-piercing riveting?

    2022-07-13 08:24:50YongChaeLimJiheonJunDonovanLeonardYuanLiJianChenMichaelBradyZhiliFeng
    Journal of Magnesium and Alloys 2022年2期

    Yong Chae Lim,Jiheon Jun,Donovan N.Leonard,Yuan Li,Jian Chen,Michael P.Brady,Zhili Feng

    Materials Science and Technology Division,Oak Ridge National Laboratory,One Bethel Valley Road,Oak Ridge,TN 37831,USA

    Abstract A new testing methodology was developed to quantitively study galvanic corrosion of AZ31B and thermoset carbon-fiber-reinforce polymer spot-joined by a friction self-piercing riveting process.Pre-define areas of AZ31B in the joint were exposed in 0.1 M NaCl solution over time.Massive galvanic corrosion of AZ31B was observed as exposure time increased.The measured volume loss was converted into corrosion current that was at least 48 times greater than the corrosion current of AZ31B without galvanic coupling.Ninety percent of the mechanical joint integrity was retained for corroded F-SPR joints to 200 h and then decreased because of the massive volume loss of AZ31B.

    Keywords: Multi-material joining;Carbon fiber-reinforce polymer;AZ31B;Friction self-piercing riveting;Galvanic corrosion;Mechanical joint strength.?This manuscript has been authored by UT-Battelle,LLC,under contract DE-AC05-00OR22725 with the US Department of Energy (DOE).The US government retains and the publisher,by accepting the article for publication,acknowledges that the US government retains a nonexclusive,paid-up,irrevocable,worldwide license to publish or reproduce the published form of this manuscript,or allow others to do so,for US government purposes.DOE will provide public access to these results of federally sponsored research in accordance with the DOE Public Access Plan(http://energy.gov/downloads/doe-public-access-plan).

    1.Introduction

    Metal-to-composite hybrid structures represent a new concept for achieving higher specific strength (strength divided by density)for multi-material lightweight vehicles[1,2].Their use enables greater fuel efficiency and lower greenhouse gas emissions.Higher-specific-strengt alloys,such as magnesium (Mg) alloys and high-strength aluminum (Al) alloys,and advanced/ultra-high-strength steels are being considered as new materials for lighter vehicle structures.Also,carbonfiber-reinforce polymer(CFRP)has been identified as a candidate engineering composite material with design flexibility and tailorable mechanical properties [3,4].Among these materials,Mg alloys and CFRP have the highest potential for lightweight applications because of their higher specific strength [1].

    However,the physical and chemical incompatibility of metals and polymer composites is a technical obstacle preventing the integration of such lightweight hybrid structures into unified body-in-white autobody assemblies that can meet joint performance and safety requirements.Extensive research and development efforts have been made to identify suitable processes for joining metal/composite material pairs to form assemblies.Joining techniques that have been tried include conventional fusion welding (laser welding,resistance spot welding)[5,6],solid-state joining[7-10],ultrasonic welding [11],mechanical fastening [12,13],and adhesive bonding [14].Recently,a combination of the friction stir process(FSP) and self-piercing rivet (SPR) joining methods,called“friction self-piercing riveting” (F-SPR),has been proposed to join low-ductility materials such as Mg alloys and highstrength Al alloys [15-17].This unique spot-joining process uses the friction heat from FSP and mechanical interlocking enabled by SPRs.Essentially,it involves a rivet that spins as it penetrates into stacked materials.The rotating rivet produces localized frictional heat as it interacts with the surrounding metal substrates.The generated friction heat increases the local ductility of the Mg alloy sheet to effectively avoid cracking problems.Most recently,the F-SPR process was further expanded to join a thermoset CFRP (TS-CFRP) to the Mg alloy AZ31B [18].

    Another critical concern is galvanic corrosion in dissimilar material joints,particularly when Mg alloys are joined with noble metals.Accelerated Mg corrosion as a result of galvanic coupling can be indirectly assessed by comparing the corrosion potentials of individual joint components [19] or measuring the galvanic current between Mg and other components in simplified electrode configuration [20-23].However,these indirect methods cannot fully emulate the galvanic corrosion of Mg in actual dissimilar material joints with more complex geometries.Another approach to evaluate Mg corrosion in dissimilar joints is to measure the corrosion mass loss [21,24].Note that mass loss is the result of general and galvanic corrosion of Mg and other components in the joints,so Mg corrosion dominated by the galvanic effect may not be directly assessed.Therefore,a novel experimental design should be considered to permit the evaluation of Mg galvanic corrosion in specific dissimilar joints.

    In the present work,a new methodology to study corrosion behavior was developed for the Mg alloy AZ31B joined to a TS-CFRP by F-SPR.In this method,a pre-define AZ31B area in the F-SPR joint produced measurable corrosion loss during immersion in 0.1 M NaCl solution.Galvanic corrosion of AZ31B driven by a steel rivet head was quantitatively estimated by corrosion volume measurement and further analyzed by corrosion potential and galvanic current measurements.Optical microscopy was used to measure the corrosion volume of AZ31B in the corroded F-SPR joints.X-ray tomography and scanning electron microscope (SEM) equipped with energy-dispersive spectroscopy (EDS) were also employed to characterize the corroded F-SPR joints.Lap shear tensile testing was used to evaluate the mechanical strength of post-immersion (corroded) F-SPR joints,and fractographical characterization was also conducted to investigate the failure mode(s).

    2.Materials and experimental methods

    2.1.Materials

    In this work,TS-CFRP (Clearwater Composites,Minnesota,USA) with a G-83 prepreg laminate reinforced with 50 wt.% of unidirectional carbon fiber (T700,Toray) was used as a top sheet.The stacking sequence of the carbon fiber layers was [0°/90°] with nine plies,resulting in a total thickness of 1.9 mm.An AZ31B sheet 2.36 mm thick (Buymetal.com) was employed as the bottom material.Japanese Industrial Standard G3507-2 carbon steel(SWCH18A) was used to fabricate the hexagonally shaped rivet head (9.525 mm width).The rivet stem diameter and leg length were 5.3 and 6 mm,respectively.A detailed drawing and dimensions of the steel rivet and pip die can be found in previous work [18].Inductively coupled plasma-optical emission spectrometry (ICP-OES) and combustion techniques were employed to characterize the chemical makeup of individual materials for the present work;the results are summarized in Table 1.A summary of the mechanical and corrosion properties of each material are provided in Table 2 [18].

    Table 1Elemental compositions of AZ31B and steel rivet in weight percent for metallic elements and Si and in ppm for O and N.The compositions (wt.%) were analyzed by ICP-OES and combustion techniques.

    Table 2Summary of mechanical and corrosion properties of thermoset CFRP,AZ31B,and steel rivet at room temperature (18).

    Table 3Summary of F-SPR parameters.

    Water jet cutting was used to cut sheet materials into coupons with dimensions of 25.4 mm width and 101.6 mm length for lap shear coupons.Then,reagent acetone and alcohol were used to clean the surfaces of the AZ31B,and the TS-CFRP coupons were sonicated with an ethanol solution.Finally,all coupons were dried at room temperature before F-SPR joining.

    2.2.Description of F-SPR process and joint fabrication

    A description of the F-SPR process can be found in the authors’ previous work [18],and a brief description of the joining process is provided as follows.First,an external plunging axial force is used to drive a spinning rivet into a stacked workpiece.During this process,frictional heat is locally generated between the rivet and the bottom sheet metal (i.e.,AZ31B),leading to improved local ductility of the AZ31B.Finally,the rivet leg flare out in the AZ31B based on the supporting die geometry,leading to mechanical interlocking in the workpiece.Fig.1 illustrates a lap shear joint configuration with a 25.4 mm overlap size.Based on previous F-SPR trials,the joining process parameters summarized in Table 3 were selected with the highest lap shear failure load (?5 kN)[18].The lap shear joint specimens were used for the subsequent corrosion study.

    Fig.1.A schematic of the lap shear joint configuration The unit is mm.

    2.3.Corrosion testing

    2.3.1.Corrosion exposure of pre-define AZ31B in F-SPR joint

    To enable a quantitative assessment of Mg corrosion,a new testing method was applied to the F-SPR joints to expose the rivet head and pre-define side sections of the AZ31B for the 0.1 M NaCl immersion test.A specific tape masking technique was applied to the F-SPR specimens and to the AZ31B side surfaces for corrosion exposure,as illustrated in Fig.2a.The AZ31B area on one pre-define side surface was 2.3×10 mm2.An F-SPR lap joint during immersion testing is schematically depicted in Fig.2b.After tape masking was applied,the active surfaces in contact with the solution were the two exposed sides of AZ31B (marked in Fig.2b),the steel rivet,and the carbon fiber exposed on the sides of the CFRP.Also note that the solution was drawn into the narrow gap between the AZ31B and the CFRP by capillary force during immersion,allowing corrosion exposure of the joining section inside the gap.To measure the corrosion potential(Ecorr) of an immersed F-SPR joint,a saturated calomel electrode (SCE) was placed adjacent to the overlap section of the joints.During immersion,the AZ31B side surfaces formed a corrosion volume as a result of anodic dissolution of the alloy by galvanic impact.The anodic dissolution of Mg from this pre-define area is similar to the experimental concept used for one-dimensional artificia pits in stainless steels in which a quantifiabl corrosion volume and depth were produced [25,26].A similar method was also adopted to investigate galvanic corrosion of AZ31B and CFRP joined by steel bolting [27].A side view of the corrosion volume formed on the AZ31B exposure surfaces is presented in Fig.2c.After immersion testing,all F-SPR joints were cleaned ultrasonically in a deionized water bath and rinsed by reagent ethanol and water to remove corrosion products.

    The corrosion volume of AZ31B was calculated by the sheet thickness (2.3 mm) and the corroded area estimated by an image analysis software.The calculated corrosion volume was then converted to the anodic charge using the charge balance,density,and molar mass of Mg,+2,-1.77 g·cm-3and 24.3 g·mol-1,respectively,and Faraday constant of 96,485 C·mol-1.The anodic current was also determined from the anodic charge divided by the immersion time.Meantime,the electrode area of AZ31B during the immersion increased as the corrosion volume grew,so a nominal surface area (described in the appendix) was used to estimate the anodic current density.

    Fig.2.Schematic descriptions of (a) the location of the AZ31B side surfaces for 0.1 M NaCl solution exposure and (b) the immersion testing with Ecorr measurement.(c) A photo image of corroded AZ31B in an F-SPR joint after 25 h of immersion.

    Fig.3.Preparation and immersion testing of dummy lap specimens:(a) AZ31B mating surface with the location of the circular insulation tape,(b) a photo of AZ31B and CFRP mating surfaces after the application of insulation tapes,and (c) a schematic of galvanic current measurement from a dummy lap specimen.

    Fig.4.Immersion testing of a dummy lap specimen:(a) measured anodic current and Ecorr for 100 h and (b) a photo of the AZ31B mating surface after testing and cleaning.The mating surface clearly showed the corrosion volume and depth formed from the two exposed sides..(For interpretation of the references to colour in this figure legend,the reader is referred to the web version of this article.)

    In addition to the corrosion volume measurement,dummy lap specimens,which mimicked the actual F-SPR joints but with no connection between the AZ31B and the riveted CFRP,were used for galvanic current measurement.To prepare the dummy lap specimens,the F-SPR joints were cut to separate the AZ31B and riveted CFRP sheets,and then circular(?=12.7 mm) and 25.4 mm wide insulating tapes were applied on the mating surfaces of the AZ31B and CFRP,respectively,as described in Fig.3a and 3b.The separated AZ31B and CFRP were then re-assembled and tape-masked to expose the same AZ31B side surfaces and rivet head used in the immersion testing of the actual F-SPR joints depicted in Fig.2a.The AZ31B and CFRP in the dummy lap specimens were connected individually to a potentiostat in zero current ammeter mode,and a reference SCE was placed near the overlap section to monitor the Ecorrof the dummy lap specimen,as shown schematically in Fig.3c.With the dummy lap samples,it was possible to measure the galvanic current between the rivet head and the AZ31B sheet in the same geometrical configuration as in the actual F-SPR joints.These dummy lap specimens also formed a corrosion volume,enabling the estimation of anodic current by using the same procedure stated previously in this section.All immersion testing was conducted at room temperature with loose plastic covers,as illustrated in Fig.2b and Fig.3c,to allow access of air but minimize the evaporation of the 0.1 M NaCl solution.

    2.4.Metallographic preparation

    The post-corrosion F-SPR samples were firs mounted in epoxy and then cut into halves to obtain cross-sections using a diamond saw.The cross-sectioned samples were ground by silicon carbide papers with 600,800,1200 grits and then polished using diamond suspensions of 3 μm,1 μm,and 0.5 μm.

    2.5.Characterization of post-corroded samples

    A digital optical microscope(Dino-Lite Edge,Taiwan)was used to characterize the post-corrosion F-SPR samples.DinoXcope software was used to measure the corrosion depth and volume for the corrosion-tested samples.

    X-ray tomography was employed to study the postcorrosion F-SPR joints in three different viewing orientations as a nondestructive evaluation method.X-ray scans were acquired using a Zeiss Metrotom 800,operated at 180 kV with a 220 uA beam current.This tungsten source x-ray microscope achieved ?15 um resolution using a 1 mm thick copper filte.X-ray data were analyzed using a VGStudio Max 3.3 created by Visual Graphics GmbH.

    SEM coupled with EDS (TESCAN Mira3) was used to characterize the cross-sectional view of the corroded F-SPR joint.An accelerating voltage of 20 kV was set during SEM.The elements Mg,Fe,O,and C were mapped with a scanning time of 4 min at the interfaces in the post-corroded samples.

    2.6.Static lap shear tensile testing of F-SPR specimens

    An MTS tensile machine was used to evaluate the joint strength of post-corrosion F-SPR coupons.Lap shear tensile testing was performed with a constant cross-head speed of 10 mm min-1at room temperature.To minimize bending of the specimen during lap shear tensile testing,spacers (25.4 by 25.4 mm) were used to hold the lap shear coupons to align them vertically between the grips.

    3.Results and discussion

    3.1.Corrosion characterization

    The anodic current and Ecorrof a dummy lap specimen are presented in Fig.4 along with a photo image showing the mating surface of the specimen after immersion testing.For 100 h of immersion testing,Ecorrgradually increased with time and was higher than the reported Ecorrof AZ31B alone,?1.55 VSCEin 0.1 M NaCl [28-31],indicating that the AZ31B in the dummy lap specimen was galvanically polarized.Meanwhile,the measured anodic current increased for an initial 25 h and then decreased gradually to ?2.2 mA afterward.The immersion testing of dummy lap specimens was conducted three times,once for 50 h and twice for 100 h.The average measured anodic currents and initial/fina Ecorrvalues aresummarized along with the corrosion-volume-calculated anodic currents in Table 4.The measured anodic current is about 53% of the corrosion volume-based anodic current.This is the case because Mg anodic dissolution is balanced by a H2reduction reaction not only on the steel rivet but also on the Mg itself [32],indicating that the evolution of H2on the Mg surface accounted for the remaining 47% of anodic Mg dissolution.In the three measurements,the initial Ecorrvalues were similar,but the final Ecorrvalues were slightly higher for 100 h than 50 h.

    Table 4Summary of measured Ecorr and average anodic currents as well as the corrosion-volume-calculated anodic currents from three dummy lap specimens.

    Fig.5.Sequence of optical images for post-corrosion F-SPR joint (backside view) with different exposure times in 0.1 M NaCl solution;(a) 25 h,(b) 50 h,(c) 100 h,(d) 200 h,(e) 350 h,and (f) 500 h.Red dot line was added in the center of rivet joint to indicate how corrosion of AZ31B progressively reduces effective cross-sectional area at the rivet joint.(For interpretation of the references to colour in this figure legend,the reader is referred to the web version of this article.)

    Fig.5 shows the examples of the corrosion volume formed on F-SPR joints for 25-500 h of immersion testing,during which galvanic corrosion of AZ31B (red dotted box) caused greater Mg loss with increasing exposure time.Overall,corrosion of AZ31B started from the pre-define exposure location and propagated into the joint.Red dot line was added in the center of rivet joint to show the degree of corrosion progression in AZ31B.Up to 200 h of exposure time,the loss of AZ31B found did not extend to the center of rivet joint as indicated by red dot line in Fig.5a-d.Therefore,effective cross-sectional area at the rivet joint was not as different from the non-corroded specimen.However,after 350 h testing,reduction of effective cross-sectional area at the rivet joint was observed in Fig.5e-f.For example,5?5.6 mm of corrosion depth was found from edge of coupon to the center of rivet joint at 500 h.This loss of AZ31B at the joint effectively decreased the joint integrity as described in the following section.

    The increasing corrosion volumes of AZ31B from the exposed F-SPR joints are plotted in Fig.6a as a function of exposure time.In addition,the anodic current and current density,calculated from the corrosion volume data and plotted in Fig.6b,decreased with immersion time.The calculated current density at 500 h was about 45% of the current density at 25 h,indicating that the dissolution rate of Mg at the corroding interface decreased as the corrosion volume and depth increased.The reduction in Mg dissolution was presumably caused by an increased solution ohmic drop as the corroded volume of AZ31B was occupied by solid phase corrosion products.The measured Ecorrduring the immersion testing of the F-SPR joints is summarized in Table 5.The initial Ecorrranged from -1.43 to -1.45 VSCE,similar to the values measured from the dummy lap specimens (see Table 4).Ecorrincreased with time to 200 h but there was no further increase afterward,as seen from theΔEcorrvalues.The values of final Ecorrwere similar between 350 and 500 h.The increase in Ecorris again considered to occur as a result of the increased ohmic drop from the buildup of solid corrosion products.

    Fig.6.F-SPR joint immersion testing results:(a) corrosion volume and (b) calculated anodic current and current density as a function of immersion time.

    Table 5Summary of measured Ecorr from F-SPR joint immersion testing.

    For 50 and 100 h immersion testing,the anodic currents for the F-SPR joints in Fig.6b were higher than the current calculated from the corrosion volume of the dummy specimens(Table 4),but their Ecorrvalues were not notably different from each other (Table 4 and Table 5).With the similar Ecorrof AZ31B in the F-SPR joints and dummy specimens,it is reasonable to assume the following:

    where ?is the overpotential applied to AZ31B,I is galvanic current between AZ31B and the steel rivet,R is the total resistance for the galvanic current flow,and the subscripts 1 and 2 indicate that the values are for F-SPR joints and dummy samples,respectively.With higher anodic currents for AZ31B in the F-SPR joint,?1and I1should be greater than ?2and I2,meaning that R2must have been greater than R1to satisfy Eq.(1).Both R1and R2must have very similar solution resistance components,implying that the solid path resistance component was greater in the dummy samples.This inference is reasonable,as the solid conduction path in the dummy samples was through carbon fiber and electric wires without direct contact between the AZ31B and the steel rivet(as was the case in the F-SPR joints).

    The corrosion current density data from this work and from the literature are compared for AZ31B and unalloyed Mg in Fig.7.The lowest value of the corrosion current density,?7.2 mA·cm-2,in this work was about 48 times greater than the highest current density value from the literature,?0.15 mA·cm-2,giving a quantitative measure of the lower-limit galvanic influence for AZ31B in the F-SPR joint configuration.More generally,it can be said that AZ31B galvanically coupled with a bare steel rivet in F-SPR lap joints corrodes 2-3 orders more than in the same alloy without galvanic polarization [31,33,34].Meanwhile,the corrosion current densities of unalloyed Mg were slightly lower than those of AZ31B in the compared literature data [35-37].

    3.2.Characterizations of corroded F-SPR joints

    Fig.8 shows X-ray tomographic images for an F-SPR joint after 500 h of corrosion,at three different viewing orientations.Fig.8a depicts massive galvanic corrosion of Mg (yellow dotted lines),which is correlated with a joint that underwent corrosion for 500 h (Fig.5f).A cross-sectional view of the corroded F-SPR joint is shown in Fig.8b and 8c in different viewing planes (z-y and x-z planes).In Fig.8b,it is seen that both edges of the AZ31B (yellow dotted boxes) significantly corroded as the area was directly exposed to 0.1 M NaCl.However,there is no obvious corrosion of the steel rivet and the AZ31B at the left side (red dotted circle,labeled “1′′)and the right side of the joint (orange dot circle,labeled “2′′).This result could be due to the limited corrosion solution infiltration into the joint area because of the tight gap tolerance between the TS-CFRP and AZ31B.Also,mechanical interlocking between the flare rivet leg and the bottom AZ31B sheet is observed in Fig.8b and 8c.The interlocking distance was approximated 0.5 mm from our recent work [18].This interlocking distance is the most important joint strength factor because it governs the locking strength between the rivet and the bottom sheet.Detailed characterization was conducted using SEM with EDS at the left side of the joint (red dotted circle) and is discussed in the following section.

    Fig.7.Comparison of corrosion current for AZ31B under galvanic influence in F-SPR joints (this work) and with no galvanic influence (31,33,34).The corrosion current of unalloyed Mg without galvanic impact (35-37) is also included.Five literature corrosion currents were measured in 0.1 M NaCl open to air at room temperature,but one data (37),converted from 0.3 mm?y-1 for high purity Mg in concentrated NaCl solutions,was deduced from multiple literature..(For interpretation of the references to colour in this figure legend,the reader is referred to the web version of this article.)

    Fig.8.X-ray tomographic images for 500 h corroded F-SPR joint at different viewing orientations:(a) x-y plane,(b) y-z plane,(c) x-z plane.

    A cross-section of the F-SPR joint after 500 h of corrosion was characterized by SEM with element maps at the left side of the joint interface (TS-CFRP -steel rivet -AZ31B),as previously shown in Fig.8b (red dotted circle).In Fig.9a,the SEM image clearly shows the joint interface with three materials:TS-CFRP,steel rivet,and AZ31B.First,part of the AZ31B was embedded into the TS-CFRP layer when the steel rivet plunged into the AZ31B.Second,there was no obvious corrosion of the steel rivet,potentially because of the limited electrolyte access into the joint.This findin agrees with the observation from x-ray tomography in Fig.8b and 8c.Next,carbon fiber dripped into the joint interface between the steel rivet and the AZ31B because of the joining process (i.e.,rotating and plunging motion of the rivet),producing a quite complex joint interface with intermixed materials.Finally,no significant corrosion of AZ31B was observed at the joint interface.There is physical contact between the steel rivet and the AZ31B;however,the limited access of the corrosion solution into the joint,due to the tight gap between the AZ31B and TS-CFRP,practically limited the formation of a galvanic circuit at the joint interface.Note that another type of mechanical fastener,an SPR similar to that used in the current joining process,has the capability to achieve watertight joints by tightly clamping the materials during the joining process[38].On the other hand,the exposure areas on both sides of the AZ31B,as preciously shown in Fig.5 and Fig.8a,were significantly corroded as a result of galvanic coupling and direct exposure to the 0.1 M NaCl solution.

    Fig.9.SEM images with element maps for 500 h corroded F-SPR joints.(a) SEM image at the joint interface as shown in Fig.8b,(b) overlay image of single elements (C,Fe,Mg,and O),(c) element map for C,(d) element map for Fe,(e) element map for Mg,and (f) element map for O.

    3.3.Mechanical joint strength for post-corroded F-SPR joints and fractography

    The mechanical joint integrity of the F-SPR joint under different corrosion exposure times was evaluated by lap shear tensile testing.Fig.10 summarizes the averaged peak failure load at different testing times.The average lap shear failure load for an uncorroded F-SPR joint was around 5 kN[18].In general,nearly 90% of the averaged peak fracture load was retained during testing for up 200 h.Then,the joint strength started to decrease from 350 h of exposure time,and 83.4% of the strength of the untested F-SPR joint remained.Finally,65%of the original F-SPR joint strength was retained at 500 h.This decrease of joint strength can be related to the reduction of effective cross-sectional area at the rivet joint as illustrated in Fig.5.However,Fig.9 shows no significant corrosion at the joint interface.Therefore,the fracture surfaces of the F-SPR joint were evaluated.

    Fig.10.Summary of mechanical joint strength for post-corroded F-SPR joints at different exposure times.

    A summary of fractography images at the mating joints is provided in Fig.11.As the corrosion exposure time increases,both edges of the AZ31B show greater corrosion loss.However,as shown in Fig.11a-d,the failure mode of the F-SPR joints for up to 200 h was not changed from that of the uncorroded F-SPR joints (i.e.,AZ31B pullout,indicated by the yellow arrow in Fig.11a,due to the strong mechanical interlocking between the flare rivet leg and the AZ31B.This is because the loss of AZ31B did not impact the effective cross-sectional area at the rivet joint (red dot line in Fig.5)up to 200 h as discussed previously.A white corrosion product (black arrow) on the AZ31B and TS-CFRP surfaces was seen at the edges,but no significant amount of corrosion product was found at the joint.The white corrosion products must be the mixture of Mg oxide and hydroxides that were commonly found on corroded AZ31B [39-41].Again,the tight gap between the TS-CFRP and AZ31B was considered to have limited the infiltration of the corrosion solution into the joint.Thus,no significant joint strength reduction was found until after 200 h of exposure time.However,cracking (red arrow) was observed away from the joint after 350 and 500 h exposure time,as seen in Fig.11e and 11f.This cracking is related to massive galvanic corrosion of AZ31B at the joint,resulting in a great reduction in the effective cross-sectional area at the joint.Also,localized corrosion of AZ31B may have created several crack initiation sites during the lap shear tensile testing and resulted in crack propagation into the joint area.Thus,after 350 h of immersion in the solution,the FSPR joint strength started to degrade because the effective joint volume of the AZ31B was greatly reduced.

    The present works provides a unique methodology to quantitively study the galvanic corrosion of Mg alloy with the other materials (e.g.,steel rivet and CFRP) in the actual dissimilar material joints.This protocol can be used to investigate the impacts of coating and other mitigations efforts to improve the galvanic corrosion resistance,directed to the AZ31B,the CFRP,and the steel rivet.

    Fig.11.Fractography of post-corroded F-SPR joints at different corrosion testing times after lap shear tensile testing.(a) 25 h,(b) 50 h,(c) 100 h,(d) 200 h,(e) 350 h,and (f) 500 h.Yellow dotted boxes at both edges of the AZ31B are corroded areas.The rivet joint is indicated by a yellow arrow.White corrosion product (black arrow) is seen at the joint.Cracking (red arrow) on AZ31B was seen for 350 h and 500 h exposure times..(For interpretation of the references to colour in this figure legend,the reader is referred to the web version of this article.)

    4.Conclusion

    In the present work,a new method was introduced for quantitative investigation of galvanic corrosion attack on AZ31B by other materials (i.e.,steel rivets and TS-CFRP)in F-SPR joints.The corrosion current densities of AZ31B under galvanic impact was determined by measuring the corrosion volume,which was at least 48 times greater than the corrosion current density with no galvanic coupling.X-ray tomography and SEM characterizations for post-corroded FSPR joints revealed that the inter-joint area was not signifi cantly corroded because the solution had limited access into the tight gap between the TS-CFRP and AZ31B in the joint.Mechanical joint integration was retained at almost 90% of that of the original F-SPR joint for testing up to 200 h.However,the strength of the F-SPR joint started to decrease after 350 h of exposure because of the large volume loss of AZ31B in the joint.The failure mode of corroded F-SPR joints was pullout of AZ31B until after 200 h of exposure,which was the same failure mode as for uncorroded F-SPR joints.Subsequently,the failure mode of corroded F-SPR joints changed to base AZ31B failure as a result of massive loss of AZ31B volume in the joint.

    Author contribution

    Conceptualization,Y.C.Lim,J.Jun;Methodology,Y.C.Lim,J.Jun;Investigation,Y.C.Lim,J.Jun,D.Leonard,Y.Li,J.Chen;Data curation,Y.C.Lim,J.Jun,M.P.Brady;Roles/writing—original draft,Y.C.Lim,J.Jun,D.Leonard,Y.Li;Writing—review and editing,Y.C.L,J.Jun,M.P.Brady,Z.Feng;Supervision,M.P.Brady,Z.Feng.

    Acknowledgments

    This research was financially sponsored by the US Department Energy Vehicle Technologies Office as part of the Joining Core Program.Oak Ridge National Laboratory (ORNL)is managed by UT-Battelle LLC for the US Department of Energy under Contract DE-AC05-00OR22725.The authors would like to thank Donald Erdman III and Rick R.Lowden for their help in the mechanical testing laboratory.

    Appendix

    The nominal surface area of AZ31B during corrosion was estimated using the corrosion depths described in Fig.A1.The surface area at the end of the corrosion exposure was estimated as 2.3 mm×(d1+10 mm) for one side and 2.3 mm×(d2+10 mm) for the other side,making the total area 2.3 mm×(d1+d2+20 mm).The initial and final areas,46 mm2and 2.3 mm×(d1+d2+20 mm),respectively,were averaged to define the nominal surface area as 1.15 mm×(d1+d2+40 mm).Note that the AZ31B area in the mating surface was not considered for the nominal surface area because the rate of Mg dissolution on the mating surface was considered to be much lower than the dissolution rate on the side surfaces.

    Fig.A1.A schematic description of corroded Mg in an F-SPR joint with the measured depths,d1 and d2,used to calculate the nominal surface area for anodic current density calculation..

    欧美日本视频| 国产精品美女特级片免费视频播放器| 一级作爱视频免费观看| 亚洲男人的天堂狠狠| 久久久精品大字幕| 精品国内亚洲2022精品成人| 99久久99久久久精品蜜桃| 九九在线视频观看精品| 久久精品人妻少妇| 男女下面进入的视频免费午夜| 国产精品三级大全| 亚洲av成人av| АⅤ资源中文在线天堂| 我要搜黄色片| 色精品久久人妻99蜜桃| 成人av在线播放网站| 午夜福利视频1000在线观看| 午夜福利视频1000在线观看| 国产成人a区在线观看| 亚洲av二区三区四区| 成人三级黄色视频| 亚洲欧美日韩卡通动漫| 国产v大片淫在线免费观看| 亚洲无线观看免费| 国产精品影院久久| 国产黄色小视频在线观看| xxxwww97欧美| 成人高潮视频无遮挡免费网站| 日本与韩国留学比较| or卡值多少钱| 免费看日本二区| 亚洲无线观看免费| 最新中文字幕久久久久| 中国美女看黄片| 亚洲精品乱码久久久v下载方式 | 久久久久久国产a免费观看| 久久午夜亚洲精品久久| 国产激情偷乱视频一区二区| 男人舔奶头视频| 色综合站精品国产| 夜夜夜夜夜久久久久| 午夜日韩欧美国产| 免费看日本二区| 国产精品1区2区在线观看.| 少妇高潮的动态图| 国产探花极品一区二区| 亚洲人成伊人成综合网2020| 亚洲成a人片在线一区二区| 99热这里只有精品一区| 日日夜夜操网爽| 熟妇人妻久久中文字幕3abv| 国产老妇女一区| 成人国产一区最新在线观看| av欧美777| 国产精品日韩av在线免费观看| 日本a在线网址| 成人性生交大片免费视频hd| 精品日产1卡2卡| 99久久精品一区二区三区| 12—13女人毛片做爰片一| 老汉色av国产亚洲站长工具| 午夜激情福利司机影院| 老司机深夜福利视频在线观看| 久久人人精品亚洲av| 欧美性感艳星| 国产日本99.免费观看| 一个人免费在线观看的高清视频| 久久精品影院6| 国产欧美日韩精品亚洲av| 日本a在线网址| 国产真实乱freesex| 蜜桃亚洲精品一区二区三区| 国产成人av激情在线播放| 内射极品少妇av片p| 国产一级毛片七仙女欲春2| 精品久久久久久,| 亚洲18禁久久av| 亚洲国产精品成人综合色| 在线观看日韩欧美| 国产精品永久免费网站| 三级男女做爰猛烈吃奶摸视频| www.色视频.com| 一边摸一边抽搐一进一小说| 午夜精品一区二区三区免费看| 三级国产精品欧美在线观看| 久久久国产精品麻豆| 国内精品久久久久久久电影| 欧美精品啪啪一区二区三区| 国产精品久久久久久精品电影| 久久久久国内视频| 精品一区二区三区av网在线观看| 此物有八面人人有两片| 亚洲aⅴ乱码一区二区在线播放| 国产久久久一区二区三区| 亚洲精品一卡2卡三卡4卡5卡| 国产免费av片在线观看野外av| 亚洲精品久久国产高清桃花| 怎么达到女性高潮| 亚洲美女黄片视频| www.www免费av| 精品久久久久久久久久免费视频| 日韩欧美国产一区二区入口| 69av精品久久久久久| 国产精品 欧美亚洲| 99视频精品全部免费 在线| 久久中文看片网| 欧美成狂野欧美在线观看| 国产精品电影一区二区三区| 久久人人精品亚洲av| av视频在线观看入口| 色尼玛亚洲综合影院| 99视频精品全部免费 在线| 中文字幕人妻丝袜一区二区| 99久久精品国产亚洲精品| 熟妇人妻久久中文字幕3abv| 91麻豆精品激情在线观看国产| 国产精品嫩草影院av在线观看 | 欧美性感艳星| 国产在视频线在精品| 午夜福利在线观看免费完整高清在 | 国产三级在线视频| 欧美xxxx黑人xx丫x性爽| 久久久久久久亚洲中文字幕 | 亚洲精品国产精品久久久不卡| 99热6这里只有精品| 一本综合久久免费| 国产精品久久久久久精品电影| 一本一本综合久久| 看黄色毛片网站| 亚洲美女黄片视频| 一本久久中文字幕| 欧美日本视频| 色吧在线观看| 国产精品亚洲av一区麻豆| 网址你懂的国产日韩在线| 色吧在线观看| 欧美中文日本在线观看视频| 国产精品久久久久久久电影 | 国产精品国产高清国产av| 免费av毛片视频| 别揉我奶头~嗯~啊~动态视频| 9191精品国产免费久久| 国产欧美日韩一区二区三| 久久午夜亚洲精品久久| 国产精品乱码一区二三区的特点| 国产成年人精品一区二区| 狂野欧美白嫩少妇大欣赏| 两性午夜刺激爽爽歪歪视频在线观看| 深夜精品福利| 亚洲欧美精品综合久久99| 亚洲人成网站在线播放欧美日韩| 国产一区二区三区在线臀色熟女| 丰满人妻熟妇乱又伦精品不卡| av在线蜜桃| 偷拍熟女少妇极品色| 亚洲avbb在线观看| 国产三级中文精品| 欧美成人a在线观看| 天堂网av新在线| 中文字幕av成人在线电影| 日日干狠狠操夜夜爽| 国内久久婷婷六月综合欲色啪| 精品一区二区三区人妻视频| 日本免费a在线| 欧美国产日韩亚洲一区| 日韩免费av在线播放| 欧美日韩乱码在线| 19禁男女啪啪无遮挡网站| 两人在一起打扑克的视频| 欧美激情久久久久久爽电影| 97超视频在线观看视频| 久久久久性生活片| 一区二区三区激情视频| 国产一区二区三区在线臀色熟女| 亚洲avbb在线观看| 男人舔奶头视频| 欧美成人a在线观看| 啦啦啦韩国在线观看视频| 村上凉子中文字幕在线| 一本一本综合久久| 网址你懂的国产日韩在线| 少妇的逼好多水| 首页视频小说图片口味搜索| 久久精品91蜜桃| 天天添夜夜摸| 国产成人a区在线观看| 亚洲真实伦在线观看| 亚洲精华国产精华精| 99久久精品一区二区三区| 色噜噜av男人的天堂激情| 免费观看的影片在线观看| 久久精品国产综合久久久| 草草在线视频免费看| 别揉我奶头~嗯~啊~动态视频| 两性午夜刺激爽爽歪歪视频在线观看| 国产精品三级大全| 国产综合懂色| 久久精品国产自在天天线| 精品欧美国产一区二区三| 国产探花极品一区二区| 成人特级av手机在线观看| 蜜桃久久精品国产亚洲av| 老熟妇仑乱视频hdxx| av视频在线观看入口| 啦啦啦韩国在线观看视频| 啦啦啦免费观看视频1| 日韩亚洲欧美综合| 网址你懂的国产日韩在线| 国产亚洲欧美在线一区二区| 国产aⅴ精品一区二区三区波| 国产男靠女视频免费网站| 日韩欧美精品免费久久 | 亚洲精品在线观看二区| 国产亚洲精品久久久com| 内射极品少妇av片p| 国产精品一区二区三区四区久久| 蜜桃久久精品国产亚洲av| 亚洲专区中文字幕在线| 久久久久九九精品影院| 搞女人的毛片| 久久久精品欧美日韩精品| 级片在线观看| 97人妻精品一区二区三区麻豆| 欧美成狂野欧美在线观看| 欧美精品啪啪一区二区三区| 亚洲av电影在线进入| 午夜久久久久精精品| 人人妻人人澡欧美一区二区| 欧美日韩一级在线毛片| 在线观看免费视频日本深夜| 狠狠狠狠99中文字幕| 国产色婷婷99| 高清日韩中文字幕在线| 蜜桃亚洲精品一区二区三区| 午夜福利在线在线| 亚洲国产色片| 亚洲国产高清在线一区二区三| 日韩欧美免费精品| 怎么达到女性高潮| 美女黄网站色视频| 精品久久久久久成人av| 日韩成人在线观看一区二区三区| 在线免费观看不下载黄p国产 | 成人国产综合亚洲| 国内毛片毛片毛片毛片毛片| 免费一级毛片在线播放高清视频| 婷婷六月久久综合丁香| 成年女人毛片免费观看观看9| 每晚都被弄得嗷嗷叫到高潮| 桃红色精品国产亚洲av| 亚洲精品一卡2卡三卡4卡5卡| 国产精品精品国产色婷婷| 男女那种视频在线观看| 热99在线观看视频| 国产精品久久久久久久久免 | 欧美bdsm另类| 性欧美人与动物交配| 1000部很黄的大片| 免费观看的影片在线观看| 757午夜福利合集在线观看| 色综合站精品国产| 国产精品电影一区二区三区| 国产高清视频在线观看网站| 国产在视频线在精品| 亚洲国产精品sss在线观看| 欧美日韩一级在线毛片| 我的老师免费观看完整版| 日本 欧美在线| 亚洲无线观看免费| 天天添夜夜摸| 午夜日韩欧美国产| 免费高清视频大片| 黑人欧美特级aaaaaa片| 日韩欧美一区二区三区在线观看| 色综合欧美亚洲国产小说| 久久精品人妻少妇| 国产精品美女特级片免费视频播放器| 麻豆久久精品国产亚洲av| 天天躁日日操中文字幕| 成人高潮视频无遮挡免费网站| 九九热线精品视视频播放| 观看免费一级毛片| 久久这里只有精品中国| 特大巨黑吊av在线直播| 91av网一区二区| 中文字幕精品亚洲无线码一区| 国产精品久久久久久久电影 | 老熟妇仑乱视频hdxx| a在线观看视频网站| 免费看光身美女| 亚洲av电影在线进入| 看免费av毛片| 天堂√8在线中文| 黄色丝袜av网址大全| 亚洲欧美日韩无卡精品| 欧美丝袜亚洲另类 | 变态另类成人亚洲欧美熟女| 免费人成视频x8x8入口观看| 欧美精品啪啪一区二区三区| а√天堂www在线а√下载| 看片在线看免费视频| 免费电影在线观看免费观看| 精品人妻一区二区三区麻豆 | 国产97色在线日韩免费| 人人妻,人人澡人人爽秒播| 麻豆国产av国片精品| 中文亚洲av片在线观看爽| 丝袜美腿在线中文| 色老头精品视频在线观看| av在线天堂中文字幕| 欧美一级a爱片免费观看看| 婷婷六月久久综合丁香| 欧美国产日韩亚洲一区| 国产蜜桃级精品一区二区三区| 国产v大片淫在线免费观看| 国产av在哪里看| 18禁黄网站禁片午夜丰满| 不卡一级毛片| 精品一区二区三区视频在线 | 免费在线观看成人毛片| av天堂中文字幕网| 亚洲狠狠婷婷综合久久图片| 成人午夜高清在线视频| 母亲3免费完整高清在线观看| 法律面前人人平等表现在哪些方面| 国产精品久久久久久久电影 | 一卡2卡三卡四卡精品乱码亚洲| 最近最新免费中文字幕在线| 99热这里只有精品一区| 免费在线观看影片大全网站| 啪啪无遮挡十八禁网站| 窝窝影院91人妻| 五月伊人婷婷丁香| 亚洲最大成人手机在线| 欧美高清成人免费视频www| 久久精品夜夜夜夜夜久久蜜豆| 日日干狠狠操夜夜爽| e午夜精品久久久久久久| 天堂av国产一区二区熟女人妻| 精品国产超薄肉色丝袜足j| 精华霜和精华液先用哪个| 叶爱在线成人免费视频播放| av女优亚洲男人天堂| 在线播放国产精品三级| 久久精品国产综合久久久| 亚洲专区中文字幕在线| 国产精品一及| 久久天躁狠狠躁夜夜2o2o| 亚洲国产中文字幕在线视频| 99国产精品一区二区三区| 午夜免费成人在线视频| 午夜福利免费观看在线| 亚洲人成电影免费在线| 免费人成在线观看视频色| 老汉色∧v一级毛片| 国产高清视频在线观看网站| 午夜福利视频1000在线观看| 亚洲天堂国产精品一区在线| 精品不卡国产一区二区三区| 国产伦精品一区二区三区视频9 | 国产视频内射| 国产亚洲精品综合一区在线观看| 91字幕亚洲| 露出奶头的视频| 很黄的视频免费| 午夜免费男女啪啪视频观看 | 久久人人精品亚洲av| 香蕉丝袜av| 国产成人欧美在线观看| 国产免费男女视频| 97人妻精品一区二区三区麻豆| 国产黄色小视频在线观看| 久久草成人影院| 婷婷亚洲欧美| 久久这里只有精品中国| 亚洲五月天丁香| 黄色丝袜av网址大全| 精品国产三级普通话版| 中文字幕熟女人妻在线| 97超级碰碰碰精品色视频在线观看| 99久久99久久久精品蜜桃| 国产三级在线视频| 男女之事视频高清在线观看| 国产69精品久久久久777片| 中文资源天堂在线| 午夜免费观看网址| 中国美女看黄片| 亚洲人成网站高清观看| 每晚都被弄得嗷嗷叫到高潮| 国产三级黄色录像| 无人区码免费观看不卡| 搡老熟女国产l中国老女人| 久久国产乱子伦精品免费另类| 日日干狠狠操夜夜爽| 欧洲精品卡2卡3卡4卡5卡区| 小说图片视频综合网站| 一进一出好大好爽视频| 欧美成狂野欧美在线观看| 色老头精品视频在线观看| 俄罗斯特黄特色一大片| 九色国产91popny在线| 国产一区在线观看成人免费| 久久精品91无色码中文字幕| 国产熟女xx| 哪里可以看免费的av片| 精品熟女少妇八av免费久了| 在线观看66精品国产| 亚洲性夜色夜夜综合| 国产aⅴ精品一区二区三区波| 日韩 欧美 亚洲 中文字幕| 午夜激情欧美在线| 日本黄色视频三级网站网址| 18禁美女被吸乳视频| 国产精品野战在线观看| 99精品欧美一区二区三区四区| 99热这里只有精品一区| 村上凉子中文字幕在线| 三级毛片av免费| 人妻夜夜爽99麻豆av| 成人无遮挡网站| 欧美乱色亚洲激情| 亚洲精品粉嫩美女一区| 欧美大码av| 在线观看一区二区三区| 国产成人av教育| 三级国产精品欧美在线观看| 午夜老司机福利剧场| 老司机深夜福利视频在线观看| 丰满乱子伦码专区| 国产色爽女视频免费观看| 国产真人三级小视频在线观看| 桃色一区二区三区在线观看| 日韩人妻高清精品专区| 午夜精品久久久久久毛片777| 日韩中文字幕欧美一区二区| 久久天躁狠狠躁夜夜2o2o| 欧美不卡视频在线免费观看| 18禁美女被吸乳视频| 无限看片的www在线观看| 综合色av麻豆| 国产激情欧美一区二区| 国产精品三级大全| 国产精品野战在线观看| 国产一区二区在线av高清观看| 制服人妻中文乱码| 久久99热这里只有精品18| 国产成人啪精品午夜网站| 国产真人三级小视频在线观看| 国产成人欧美在线观看| 免费av不卡在线播放| 18禁国产床啪视频网站| 中文在线观看免费www的网站| www.色视频.com| 亚洲不卡免费看| 国产高清激情床上av| 99久久综合精品五月天人人| 丁香欧美五月| 欧美性猛交╳xxx乱大交人| 亚洲av中文字字幕乱码综合| 亚洲精品色激情综合| 国产精品久久电影中文字幕| 日本与韩国留学比较| 首页视频小说图片口味搜索| 麻豆久久精品国产亚洲av| 最近最新中文字幕大全免费视频| 在线十欧美十亚洲十日本专区| 超碰av人人做人人爽久久 | 精品人妻偷拍中文字幕| 日韩亚洲欧美综合| 老熟妇仑乱视频hdxx| 在线观看日韩欧美| 91字幕亚洲| 国产日本99.免费观看| av天堂在线播放| 一级黄片播放器| 欧美日本亚洲视频在线播放| 首页视频小说图片口味搜索| 亚洲欧美日韩无卡精品| 久久草成人影院| 五月伊人婷婷丁香| 少妇的丰满在线观看| 国产高清视频在线播放一区| 久久久久久人人人人人| 男人和女人高潮做爰伦理| 日韩欧美 国产精品| 日韩有码中文字幕| 大型黄色视频在线免费观看| 国产欧美日韩一区二区精品| 日韩中文字幕欧美一区二区| 亚洲欧美日韩高清专用| 久久久久久人人人人人| 精品无人区乱码1区二区| 日本与韩国留学比较| 国产视频内射| 精品电影一区二区在线| 一进一出抽搐动态| ponron亚洲| 麻豆成人午夜福利视频| 人妻夜夜爽99麻豆av| 成人av在线播放网站| 午夜福利在线在线| 国产69精品久久久久777片| 美女免费视频网站| 精品久久久久久成人av| 久久这里只有精品中国| 国产成人啪精品午夜网站| 国产高清激情床上av| 中文在线观看免费www的网站| 97超视频在线观看视频| 日本一本二区三区精品| 亚洲精品粉嫩美女一区| 午夜视频国产福利| 黄色视频,在线免费观看| 色综合婷婷激情| 欧美黄色片欧美黄色片| 精品久久久久久久久久免费视频| 波多野结衣高清作品| 一本精品99久久精品77| 在线免费观看的www视频| 99热精品在线国产| 欧美一区二区国产精品久久精品| 一本综合久久免费| 岛国在线免费视频观看| 网址你懂的国产日韩在线| 久久久久九九精品影院| 久久久久久人人人人人| 国产美女午夜福利| 国产高潮美女av| av片东京热男人的天堂| 一级a爱片免费观看的视频| 性欧美人与动物交配| 无遮挡黄片免费观看| bbb黄色大片| 神马国产精品三级电影在线观看| 免费观看的影片在线观看| 亚洲电影在线观看av| 久久性视频一级片| 午夜福利在线观看免费完整高清在 | 757午夜福利合集在线观看| 欧美激情在线99| 白带黄色成豆腐渣| 亚洲五月天丁香| 久久香蕉精品热| 久久性视频一级片| 每晚都被弄得嗷嗷叫到高潮| 精品熟女少妇八av免费久了| 伊人久久大香线蕉亚洲五| 亚洲欧美激情综合另类| 色在线成人网| 国产单亲对白刺激| 亚洲成人中文字幕在线播放| 熟女少妇亚洲综合色aaa.| 久久婷婷人人爽人人干人人爱| 精品人妻一区二区三区麻豆 | 日韩有码中文字幕| 国产伦精品一区二区三区视频9 | 国产一区二区在线av高清观看| 欧美不卡视频在线免费观看| 国产成人av教育| 精品国产美女av久久久久小说| 亚洲欧美日韩高清在线视频| 亚洲av日韩精品久久久久久密| 欧美+日韩+精品| 久久99热这里只有精品18| 欧美日本亚洲视频在线播放| 国内精品久久久久久久电影| 国产不卡一卡二| 淫妇啪啪啪对白视频| 听说在线观看完整版免费高清| 国产精品1区2区在线观看.| 亚洲国产色片| 丁香欧美五月| 国产精品一区二区免费欧美| 亚洲无线在线观看| 手机成人av网站| 真人一进一出gif抽搐免费| 国产三级中文精品| www国产在线视频色| www日本黄色视频网| 蜜桃久久精品国产亚洲av| 国产免费av片在线观看野外av| 久久伊人香网站| 天堂动漫精品| 中文字幕av在线有码专区| 天美传媒精品一区二区| 亚洲av五月六月丁香网| 免费看十八禁软件| 日本黄大片高清| 一级黄片播放器| 亚洲国产精品999在线| 国产成人啪精品午夜网站| 18禁国产床啪视频网站| 国产探花在线观看一区二区| or卡值多少钱| 久久久久国产精品人妻aⅴ院| 十八禁人妻一区二区| 国产高清视频在线播放一区| 欧美黄色淫秽网站| 色综合亚洲欧美另类图片| 啦啦啦韩国在线观看视频| 免费大片18禁| 国产老妇女一区| 国产成人aa在线观看| 亚洲成人精品中文字幕电影| 亚洲avbb在线观看| 国产国拍精品亚洲av在线观看 | 黄片小视频在线播放| 日韩精品中文字幕看吧| aaaaa片日本免费| 国产av不卡久久| 欧美区成人在线视频| 亚洲欧美精品综合久久99| or卡值多少钱| 免费在线观看影片大全网站| av黄色大香蕉|