    Dendrite-Free and Stable Lithium Metal BatteryAchieved by a Model of Stepwise Lithium Deposition and Stripping

    2021-10-21 03:30:54TiancunLiuJinlongWangYiXuYifanZhangYongWang
    Nano-Micro Letters 2021年11期

    Tiancun Liu ,Jinlong Wang ,Yi Xu ,Yifan Zhang ,Yong Wang,2

    ABSTRACT The uncontrolled formation of lithium (Li)dendrites and the unnecessary consumption of electrolyte during the Li plating/stripping process have been major obstacles in developing safe and stable Li metal batteries.Herein,we report a cucumber-like lithiophilic composite skeleton (CLCS) fabricated through a facile oxidationimmersion-reduction method.The stepwise Li deposition and stripping,determined using in situ Raman spectra during the galvanostatic Li charging/discharging process,promote the formation of a dendrite-free Li metal anode.Furthermore,numerous pyridinic N,pyrrolic N,and CuxN sites with excellent lithiophilicity work synergistically to distribute Li ions and suppress the formation of Li dendrites.Owing to these advantages,cells based on CLCS exhibit a high Coulombic efficiency of 97.3% for 700 cycles and an improved lifespan of 2000 h for symmetric cells. The full cells assembled with LiFePO4 (LFP),SeS2 cathodes and CLCS@Li anodes demonstrate high capacities of 110.1 mAh g-1 after 600 cycles at 0.2 A g-1 in CLCS@Li|LFP and 491.8 mAh g-1 after 500 cycles at 1 A g-1 in CLCS@Li|SeS2.The unique design of CLCS may accelerate the application of Li metal anodes in commercial Li metal batteries.

    KEYWORDS Lithiophilic skeleton;Stepwise Li deposition and stripping;Dendrite suppression;Lithium metal battery;Electrochemical properties

    1 Introduction

    Lithium (Li) metal anodes exhibit a high theoretical capacity(3860 mAh g-1) and the lowest reduction potential (-3.04 V vs.SHE) among next-generation high-energy systems to enhance the Li-ion battery [1-3].However,issues such as the fatal growth of dendritic Li,inhomogeneous Li deposition,and additional electrolyte consumption during the Li plating/stripping process result in low Coulombic efficiency (CE),quick capacity decay,and the internal short circuit of the cell.These critical challenges need to be overcome effectively for the practical utilization of Li metal anodes [4-6].The primary concern is restraining the production and growth of Li dendrites.Recent literature has yielded several effective methods such as constructing an artificial solid electrolyte interface(SEI) with high stiffness [7-10],designing functional separators [11-13],and modifying the electrolyte by adding additives [14-16] to suppress the growth of Li dendrites.Consequently,these solutions have improved the cycling stability and prolonged the lifespan of the Li metal anode.

    Constructing functional current collectors is another effective approach to achieve dendrite-free Li metal anodes.The Chazalviel diffusion model suggests that decreasing the effective electrode current density extends the Sand’s time,i.e.,initial time for the growth of Li dendrites [17-19].Consequently,the increase in the specific surface area reduces the local current density of the electrode while further suppressing the generation of Li dendrites.Several substrates with high specific surface areas have been designed as containers for the deposited metallic Li to produce dendrite-free Li metal anodes [20-24].Additionally,lithiophilic sites in the substrate effectively disperse Li ions,thereby reducing the Li nucleation barrier and guiding uniform Li deposition.Some inorganic components such as heteroatom-doped carbon [25-27],metals and their derivatives [28-35] along with unique organic materials [36-39] possess excellent lithiophilicity to promote homogeneous Li deposition and growth.Therefore,an ideal current collector must possess abundant lithiophilic groups to impart substantial lithiophilicity.

    Herein,we propose a distinct cucumber-like lithiophilic composite skeleton (CLCS) as a loader of deposited Li metal to enhance the electrochemical performance and improve the lifespan of Li metal batteries.Specifically,numerous lithiophilic groups (pyridinic N,pyrrolic N,and CuxN sites)in the CLCS exhibit strong binding to Li atoms,resulting in improved homogeneous dispersion of Li ions and subsequent dendrite-free Li deposition.Furthermore,stepwise Li deposition and stripping can be conducted during the galvanostatic Li charging/discharging process,suppressing concentrated Li nucleation while avoiding aggressive Li growth.Consequently,both asymmetric and symmetric cells based on CLCS exhibit a prolonged cycling lifetime and a decreased voltage polarization.Furthermore,full cells composed of CLCS@Li anodes deliver a stable cycling plot and high capacity retention when coupled with common cathode materials (LiFePO4and SeS2).

    2 Experimental Section

    2.1 Materials

    Commercial copper foam (CF) substrate with the thickness of 0.5 mm was provided by KunShan GuangJiaYuan new materials Co.,Ltd.N,N-dimethylformamide (DMF) solvent and poly(acrylonitrile) (Mw=150,000) were obtained from J&K Scientific and Sinopharm Chemical Reagent Co.,Ltd..

    2.2 Material Synthesis

    Commercial CF substrates were cleaned and placed in a muffle furnace and annealed at 600 °C for 2 h in the presence of air.Subsequently,the black oxidized CF substrates were immersed in a pre-prepared poly(acrylonitrile) solution (8 wt%) for 10 min and then transferred to an oven for drying.The CLCS was prepared by annealing the dried mixture at 600 °C for 2 h in a H2/Ar (5/95,v/v) atmosphere.The heating rate was set at 2 °C min-1.

    2.3 Material Characterization

    The morphologies of various samples were observed and analyzed using a scanning electron microscopy (Hitachi SU1510) and transmission electron microscopy (JEM-2010F).The components of the CLCS were characterized using X-ray diffraction (XRD,Rigaku D/max-2550 V).Raman spectra and in situ Raman spectra were obtained using a Raman spectrometer (Renishaw inVia plus).Related in situ optical images were conducted by Smartroom 5(Zeiss).The XPS measurements were conducted on a Thermo Scientific K-Alpha instrument.

    2.4 Electrochemical Measurements

    Each coin cell (CR 2032) based on CF or CLCS electrodes was assembled in an argon-filled glove box with H2O and O2content lower than 0.1 ppm.The Coulombic efficiency was determined using a specific amount of Li metal plated on the bare CF and CLCS,which was then stripped away through the voltage of 1 V.For galvanostatic charge/discharge testing,CF@Li or CLCS@Li electrodes loaded with a Li deposition of 3 mAh cm-2were assembled into symmetrical cells.Specially,the specific capacity of the CLCS@Li composite anode in symmetry and full cells is~ 1600 mAh g-1.Celgard 2400 and 1 M LiTFSI in DOL/DME (1:1,v/v) with 2% LiNO3additive were chosen as the separator and electrolyte,respectively,in asymmetrical and symmetrical cells.The amount of selected electrolyte was controlled at 40 uL per coin cell.The full cells assembled using commercial LiFePO4(LFP) and selenium sulfide(SeS2) cathodes.The SeS2cathodes were fabricated by preparing a mixture of weighed cathode powder,conductive carbon black,and polyvinylidene fluoride (PVDF) binder in a mass ratio of 8:1:1 dispersed in N-methyl-2-pyrrolidone (NMP) solvent and casting it on Al foil.Subsequently,the Al foil with slurry was dried in a vacuum oven at 120 °C for 10 h.The dried foil loaded with an LFP (areal mass:~ 6 mg cm-2) or SeS2(areal mass:~ 1.5 mg cm-2)cathode was assembled into a full cell with a specific Li metal anode.1 M LiPF6in EC/DEC (1:1,v/v) and 1 M LiTFSI in DOL/DME (1:1,v/v) with 2% LiNO3additive were used as the electrolytes of the full cells composed of LFP and SeS2,respectively.Furthermore,the amount of electrolyte used was fixed at 40 μL per coin cell.The voltage window of 2.5-4.2 V was applied to the Li|LFP cell.Similarly,the Li|SeS2full cell was controlled between 1.7 and 2.8 V.The electrochemical performance was measured in a LAND-CT2001 test system.

    2.5 Theoretical Calculation

    The constructed model of CLCS composite was optimized by the DMol3module of Materials Studio (MS) software,in which the functional was chosen as Perdew-Wang (PWC) in local density approximation (LDA).

    3 Results and Discussion

    3.1 Preparation and Characterizations of CLCS

    A facile oxidization-immersion-reduction method was explored to produce a novel functional current collector.Figure 1a illustrates the preparation of the CLCS in detail.Initially,metallic copper foam (CF) was oxidized in air and transformed into the fragile and black copper oxide (CuO)skeleton.Subsequently,the free-standing CuO skeleton was immersed in an as-prepared commercial-grade polyacrylonitrile (PAN) solution for organic coating.Finally,CLCS was obtained through a reduction process at 600 °C in a H2and Ar (5%/95%,v/v) atmosphere from a CuO composite skeleton coated with PAN with the color of the products changing from black to brown.As illustrated in Fig.1b,the different morphology observed following Li deposition on bare CF and CLCS highlights the difference in the lithiophilicity between these two substrates.Furthermore,uniform Li nucleation and growth can be achieved in the CLCS where Li ions are attracted to lithiophilic N-containing groups(pyridinic N,pyrrolic N,and CuxN sites) during the Li plating process and then reduced on the CLCS.These excellent lithiophilic sites can suppress dendritic Li growth from the CLCS,and the resultant uniform Li deposition can enhance working safety,improve the electrochemical performance,and prolong the cycling life of cells.Conversely,an inhomogeneous distribution of metallic Li grains occurs in the CF substrate owing to its poor lithiophilicity at the initial Li nucleation stage.The continuous Li deposition would transform the plated Li metal into large bulks with various forms such as Li dendrites,resulting in unnecessary electrolyte consumption and the internal short circuit of the working battery.

    As displayed in Fig.S1,the bare CF exhibited a shiny color and a smooth surface.After calcination in air,the oxidized CF turned black owing to the formation of CuO(Fig.1a).Figure 2a-c displays the related scanning electron microscopy (SEM) images of the oxidized CF which anchors several vertical CuO nanoneedles with flat surfaces.However,these unique nanoneedles could not maintain their structure during the calcination process in a mixed gas atmosphere (H2/Ar:5%/95%,v/v).The reduced CF following the calcination process illustrated in Fig.S2 indicates the absence of the original nanoneedles and pores in the skeleton.Conversely,massive nanoneedles were retained in the CLCS with the perfect protection of the coated carbon layer.As shown in Fig.2d-f,several thin nanoneedles are decorated with Cu nanoparticles in the CLCS.The SEM image at higher magnification (Fig.S3) illustrates the surface of the CLCS being covered with massive N-doped carbon-coated Cu nanoparticles,which promotes uniform Li deposition.Figure 2g displays the transmission electron microscopy (TEM) image of a pristine CuO nanoneedle with a smooth surface and a solid structure,in agreement with Fig.2c.However,as shown in Fig.2h,a noticeable hollow space was observed in a nanoneedle of the CLCS,which could improve the electrolyte transport.Furthermore,there are some internal regular Cu nanoparticles formed from the decomposition and reduction of pristine CuO nanoneedles in addition to the external nanoparticles embedded in the nanoneedles.The elemental distributions of C,N,and Cu displayed in Fig.2i are detected accurately and observed in the vertical nanoneedles using energy-dispersive X-ray spectroscopy,illustrating the structural uniformity of the CLCS.Furthermore,the distinctive distributions of the aforementioned elements are in accordance with the selected detection area in the SEM image (Fig.S4).This result substantiates the uniform distribution of C,N,and Cu elements in the CLCS.Figure S5 illustrates the XRD patterns of the CLCS.The peak at 23° was assigned to the amorphous carbon,and three typical characteristic peaks belonging to Cu metal (JCPDS No.04-0836)were identified.As depicted in Fig.2j,the XPS results were used to validate the structural composition of the CLCS.The common graphic N (399.31 eV),pyrrolic N(399.31 eV),pyridinic N (398.75 eV),and notably the Cu-N site (398.21 eV) are observed in the N 1s spectrum of the CLCS [40-43].The isolated Raman spectrum of the CLCS displays a high degree of graphitization (Fig.S6).Additionally,the Raman spectra at different depths of the CLCS shown in Fig.2k illustrate the slow gradual increase and eventual stabilization of the intensity of the D-band (1320.71 cm-1) and G-band (1579.97 cm-1)indicating interactions between the N-doped carbon and the reduced Cu nanoparticles,which affect the structural uniformity.

    Fig.1 a Schematic diagrams for the synthetic process of CLCS.b Different Li deposition and growth behaviors in bare CF and CLCS

    Fig.2 SEM images of a-c oxidized CF and d-f CLCS.TEM images of g oxidized CF and h CLCS.i EDS mapping containing C,N and Cu element for CLCS.j XPS survey spectra (N 1s) and k Raman spectra at different depths of CLCS

    3.2 Li Deposition and Stripping in CLCS

    The remarkable lithiophilicity of the CLCS was explored using density functional theory (DFT) to calculate the binding energy and charge density of Li atoms adsorbed on preferential functional groups (Cu,graphite,pyridinic N,pyrrolic N,and CuxN sites).As shown in Figs.3a and S7,the binding energies of Li atoms and graphite and Li atoms and Cu were calculated to be 1.599 and 2.597 eV,respectively.This demonstrates the poor adsorption of Li atoms and the increased possibility of Li deposition and accumulation.However,the binding energy of the Li atom to pyridinic N (-2.976 eV),pyrrolic N (-1.795 eV),and Cu-N sites (-1.751 eV) indicates a strong Li adsorption and effective Li distribution.Furthermore,the difference in the charge densities of the adsorbed Li on these aforementioned groups helps in determining their different lithiophilicity.The electron accumulation and reduction are represented by the blue and yellow regions,respectively.A lower charge transfer was observed for Li adsorbed on Cu and graphite,demonstrating the weak bond between Li and Cu as well as Li and graphite.Conversely,a significant degree of charge transfer was observed for the Li adsorbed on pyridinic N,pyrrolic N,and Cu-N sites.This further corroborates the strong bond formed between Li and N-containing functional groups while highlighting the impressive lithiophilicity of the CLCS.SEM images of the CLCS and CF loaded with different areal capacities of metallic Li are presented to evaluate the effect of guiding uniform Li deposition and suppressing the generation of Li dendrites.The surface of the CLCS without any dendrites was found to be smoother in comparison with the original morphology as Li was plated on the CLCS (Fig.3b,c).These magnified images of the CLCS loaded with metallic Li indicate that the cucumberlike surface of the CLCS gradually disappears as the Li deposition capacity increases from 1 to 3 mAh cm-2,eventually flattening (Fig.S8a-c).In the process of Li stripping,the continuous stripping of Li metal from the CLCS causes the reappearance of a cucumber-like surface,indicating ordered,stepwise Li deposition and stripping (Fig.S8d-f).However,the Li deposition on CF exhibits a highly disordered distribution and an uncontrolled formation of dendritic Li due to the poor lithiophilicity of CF (Fig.3d,e).Notably,irregular Li bulks and pronounced Li dendrites were observed from magnified partial details in the SEM images (Fig.S9).Additionally,the morphology of cycled CLCS and CF after 50 cycles indicated residual Li on the CF skeleton as compared to the residual-free CLCS (Fig.S10).Figure 3f displays the XPS spectra of the cycled CLCS and CF to assess the surface components.As illustrated by the Li 1 s spectra,LiF(55.48 eV) was detected in the cycled CF and CLCS,which can be ascribed to the decomposition of the electrolyte on the surface of the electrodes [44].Furthermore,once the Li dendrites break the SEI,excess electrolyte consumption is inevitable for the formation of fresh SEI which culminates in the rapid failure of the cell.

    Fig.3 a Density functional theory calculations on the adsorption energy between Li atoms and graphite,pyridinic N,pyrrolic N and Cu-N site.Moreover,values of related adsorption energy for these groups are calculated.SEM images of CLCS loading with Li deposition of b 1 mAh cm-2 and c 2 mAh cm-2.SEM images of CF plating with metallic Li of d 1 mAh c m-2 and e 2 mAh cm-2.f XPS survey spectra of CLCS and CF electrode after 50 cycles.In situ optical observation of CLCS at the discharging time of g 0 min and h 30 min.In situ optical images of CF at the discharging time of i 0 min and j 30 min.In situ Raman spectra of CLCS at k Li plating and l Li stripping process

    An in situ optical micrograph test was carried out to observe the innate Li deposition behavior and further investigate the remarkable lithiophilicity of the CLCS.Figure 3g displays the initial state of the CLCS before the Li is plated on the skeleton.A homogeneous color change in the substrate was observed when metallic Li was plated on the CLCS for 30 min because of the favorable Li distribution and uniform Li deposition (Fig.3h).As shown in Fig.3i,bare CF exhibits a shiny color before the Li plating on the skeleton.However,the majority of the bare CF was not covered by metallic Li after continuous Li deposition for 30 min and was still exposed to the electrolyte (Fig.3j),further corroborating its poor lithiophilicity compared to CLCS.Although the superior lithiophilicity of CLCS has been confirmed,the priority of Li deposition in this carbon-based material needs further examination with defects in the carbon playing an important role in storing Li ions.Hence,in situ Raman spectra were investigated as an appropriate probing method to determine the priority of the Li deposition behavior.Figure S11 displays the discharging and charging profiles of the CLCS at a current density of 1 mA cm-2with an areal capacity of 3 mAh cm-2in an assembled battery.As highlighted in Fig.3k,the intensity of the D-band and G-band of the CLCS gradually decreased with the increase in Li plating time.Notably,the intensity of the D-band dropped faster than that of the G-band,indicating that metallic Li was preferentially deposited at the defects of CLCS [45].Additionally,the intensity of the G-band was found to be enhanced before the D-band during the inverse charging process (Fig.3l).The results of in situ Raman spectroscopy clearly demonstrate that metallic Li was first deposited on the defects,and gradually covered the surface of the CLCS.Hence,the stepwise Li deposition and stripping in the CLCS could avoid concentrated nucleation and the growth of metallic Li,effectively suppressing the generation of Li dendrites and the excess consumption of the electrolyte.

    3.3 Electrochemical Performances of CLCS-based Li Metal Batteries

    The excellent lithiophilicity should enhance the electrochemical performance of the asymmetric and symmetric cells based on the CLCS.The reversibility of the Li plating/stripping performance on the substrate is an essential factor for evaluating the formation of Li dendrites or dead Li in the current collector of Li metal anodes.Figure S12 shows the Nyquist plots of asymmetric cells based on bare CF and CLCS electrodes.The CLCS electrode delivers a higher transfer impedance of 54.7 Ω than that (37.3 Ω)of CF due to the existence of nitrogen-doped carbon coating,which is less conductive than Cu.Moreover,Nyquist plot of CLCS electrodes after 50 cycles can be observed in Fig.S13.Because of the interface stabilization,transfer impedance has been decreased to 21.2 Ω from the initial state (54.7 Ω).This reduced transfer impedance is beneficial to promoting the uniform Li deposition.As shown in Fig.4a,the asymmetric cells consisting of CLCS electrodes exhibit comparatively stable CE plots.Specifically,CLCS electrodes demonstrate a high CE value of 97.8% for 700 cycles at 1 mA cm-2,97.5% for 400 cycles at 3 mA cm-2,and 98.1% for 200 cycles at 5 mA cm-2,respectively.Conversely,the bare CF electrode maintains a shorter cycling lifespan with a quick CE decay because of the generation of Li dendrites.The CLCS displays a superior CE performance to that of CF even when cycled at a high areal capacity of 3 mAh cm-2(Fig.S14).Figure 4b displays the voltage profiles of the CLCS at different cycles at 1 mA cm-2with a plating capacity of 1 mAh cm-2,which demonstrate that the CLCS maintains a stable and high CE as the cycle number increases.Additionally,the voltage polarization was found to decrease from 29.8 mV at the 50th cycle to 23.9 mV at the 400th cycle,which may result from the gradual stabilization of the electrode interface.Apart from the continuous capacity loss of stripped Li metal,the voltage profiles at different cycles of the bare CF are displayed in Fig.4c and indicate a rapid voltage polarization drop from 44 mV at the 150th cycle to 22.4 mV at the 200th cycle,indicating an internal short circuit caused by dendritic Li.Symmetric cells based on CLCS@Li were assembled to determine the effect of improving the cycling stability and avoiding the generation of Li dendrites on the electrochemical performance.The CLCS@Li|CLCS@Li demonstrated an extremely stable voltage curve with an ultra-long cycling lifespan of 2000 h compared to the fluctuating voltage curves of Li|Li and CF@Li|CF@Li cells (Fig.4d).Furthermore,even after 1000 cycles,a relatively small voltage hysteresis of 20.3 mV was maintained (Fig.S15).The CLCS@Li|CLCS@Li cells exhibited a long-term cycling performance with enhanced stability when cycled at a high current density of 3 mA cm-2and 5 mA cm-2,similar to that at 1 mA cm-2(Fig.4e,f).However,the CF@Li|CF@Li cell experienced a rapid increase in voltage polarization after less than 200 h at 3 mA cm-2and at 60 h at 5 mA cm-2because of the uncontrolled growth of Li dendrites and excessive consumption of the electrolyte.The fragile SEI on the metallic Li foil was easily broken due to the large volume expansion of the plated Li metal,which diminishes the electrochemical performance of the Li|Li symmetric cell.Moreover,the CLCS@Li|CLCS@Li cell exhibits an impressive rate performance with slight fluctuations in voltage polarization.Notably,a symmetrical cell containing CLCS@Li exhibited a relatively low voltage hysteresis of approximately 115 mV at 10 mA cm-2(Fig.4g).These results indicate that CLCS with superior lithiophilicity can improve the electrochemical performance and extend the cycling life of working batteries.

    Fig.4 a Coulombic efficiency performance of bare CF and CLCS at 1,3,and 5 mA cm-2 with a fixed capacity of 1 mAh cm-2.Voltage-capacity plots at different cycles and corresponding voltage hysteresis of b CLCS and c CF.Voltage-time profiles in symmetric cells composing of Li,CF@Li and CLCS@Li electrodes at d 1 mA cm-2,e 3 mA cm-2 and f 5 mA cm-2.g Rate performance with a cycling capacity of 1 mAh cm-2

    A CLCS@Li anode was coupled to a commercial LiFePO4(LFP) cathode and assembled into a full cell to determine its potential in practical Li metal batteries.For the CLCS@Li anode,metallic Li of 3 mAh cm-2should be electroplated onto the skeleton.Additionally,the specific capacity of the CLCS@Li composite anode was measured to be around 1600 mAh g-1.The specific capacity of the unique anode is much superior to other types of anodes with Cu current collector.High density of Cu does have a negative effect on the specific capacity of composite anode.In order to better realize the practical application of high-energy Li metal batteries,it is essential to explore more light-weight current collectors.As displayed in Fig.5a,CLCS@Li|LFP demonstrates a comparatively stable capacity plot with a high CE value at a current density of 0.2 A g-1.A high specific capacity of 110.1 mAh g-1was obtained by the CLCS@Li|LFP full cell even after cycling 600 cycles.Additionally,a superior capacity retention ratio of 88.8% (compared to the initial specific capacity of 124 mAh g-1) indicates the suppressed formation of Li dendrites and dead Li,in contrast to the rapid capacity loss with sharp fluctuations for CF@Li|LFP and Li|LFP.Figure 5b displays the rate performance of full cells based on Li,CF@Li,and CLCS@Li anodes.The CLCS@Li|LFP cell displayed the highest specific capacity at various current densities compared to those of the Li|LFP and CF@Li|LFP full cells.The high capacity delivery and excellent capacity preservation exhibited by the CLCS@Li|LFP cell following the charge-discharge test at higher current density further demonstrate its improved electrochemical performance.Figure 5c displays the galvanostatic charge-discharge profiles at different current densities of CLCS@Li|LFP.The exceptional interfacial reaction kinetics increases the voltage polarization by approximately 30 mV from 0.05 to 1 A g-1.The CLCS@Li anode was also coupled with a selenium disulfide (SeS2)cathode to assemble a different full cell to gauge its applicability.As shown in Fig.5d,the electrochemical performances of Li|SeS2,CF@Li|SeS2,and CLCS@Li|SeS2cells were measured at a high current density of 1 A g-1.The CLCS@Li|SeS2cell exhibited the slowest capacity decay and the highest capacity retention (66.3%) after 500 cycles among these full cells,while the initial cell activation was at 0.2 A g-1for 3 cycles.A comparable Li|SeS2cell has similar capacity decay during the first 50 cycles,benefiting from the initially stable electrode interface formed on the Li foil.The interface is then broken down by the growing Li dendrites owing to the uneven Li deposition,unavoidably leading to additional electrolyte consumption.The specific capacity of the Li|SeS2cell decreases rapidly and continuously.This could be because the high amounts of dendritic Li originally on the anode,with the exception of the fragile CF@Li anode interface,are transferred onto the inactive dead Li during the continuous charge-discharge process,resulting in the extremely low capacity.Figure 5e exhibits the galvanostatic charge-discharge profiles at different cycles of the CLCS@Li|SeS2cell.This cell demonstrates a high specific capacity (491.8 mAh g-1) even after cycling for 500 cycles with minor voltage polarization fluctuations between the 100th and the 500th cycle,in sharp contrast to the significant changes in the voltage polarization of the Li|SeS2and CF@Li|SeS2cells (Figs.S16 and S17).The electrochemical performances and thorough discussion on the cells employing CLCS-based Li anodes have also been proved the excellent lithiophilicity and effectively suppressed formation of Li dendrites,highlighting their potential as efficient and realistic Li metal batteries.

    Fig.5 a Cycling performance of Li|LFP,CF@Li|LFP and CLCS@Li|LFP full cells at a current density of 0.2 A g-1.b Rate performance at various current densities from 0.05 to 1 A g-1 and c related galvanostatic charge-discharge profiles.d SeS2-based full cells coupled with Li,CF@Li and CLCS@Li anode at 1 A g-1.e Corresponding galvanostatic charge-discharge profiles at different cycles

    4 Conclusion

    In summary,we report the synthesis of a unique free-standing cucumber-like lithiophilic composite skeleton to function as a container for deposited Li metal through a facile fabrication method.The pyridinic N,pyrrolic N,and several CuxN sites provide excellent lithiophilicity to facilitate strong binding to the Li atoms,guide uniform Li deposition and suppress the generation of Li dendrites.Furthermore,stepwise Li deposition and stripping on the CLCS,as determined by in situ Raman spectra,alleviate the concentrated and uncontrolled Li nucleation and growth.The cells consisting of CLCS electrodes benefit from these advantages and display prolonged cycling life and improved electrochemical performance.Additionally,they demonstrate anextremely high CE performance of 97.3% after 700 cycles in an asymmetrical cell along with an ultra-long and stable lifespan of 2000 h for a symmetrical cell at 1 mA cm-2with a deposition capacity of 1 mAh cm-2.The full cells based on the CLCS@Li anodes assembled with LiFePO4and SeS2cathodes maintain a high reversible capacity of 110.1 mAh g-1after 600 cycles in the CLCS@Li|LFP cell and 491.8 mAh g-1after 500 cycles in the CLCS@Li|SeS2cell.The successful construction and application of CLCS provide a template for dendrite-free and high-capacity Li metal batteries.

    AcknowledgementsThis work is well supported by National Natural Science Foundation of China (52073170,21975154),Shanghai Municipal Education Commission (Innovation Program (2019-01-07-00-09-E00021) and Innovative Research Team of High-level Local Universities in Shanghai.The authors also acknowledge Lab for Microstructure,Instrumental Analysis &Research Center,Shanghai University,for their help on materials characterization.Moreover,the authors thank High Performance Computing Center of Shanghai University,and Shanghai Engineering Research Center of Intelligent Computing System (No.19DZ2252600) for the assistance of computing resources and technical support.

    Open AccessThis article is licensed under a Creative Commons Attribution 4.0 International License,which permits use,sharing,adaptation,distribution and reproduction in any medium or format,as long as you give appropriate credit to the original author(s) and the source,provide a link to the Creative Commons licence,and indicate if changes were made.The images or other third party material in this article are included in the article’s Creative Commons licence,unless indicated otherwise in a credit line to the material.If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use,you will need to obtain permission directly from the copyright holder.To view a copy of this licence,visit http:// creat iveco mmons.org/ licen ses/ by/4.0/.

    Supplementary InformationThe online version contains supplementary material available at https:// doi.org/ 10.1007/s40820-021-00687-3.

    亚洲专区中文字幕在线| 午夜福利18| 免费人成视频x8x8入口观看| 身体一侧抽搐| 欧洲精品卡2卡3卡4卡5卡区| 亚洲av日韩精品久久久久久密| 97碰自拍视频| 免费无遮挡裸体视频| 国产色爽女视频免费观看| 亚洲欧美一区二区三区黑人| 草草在线视频免费看| 又黄又粗又硬又大视频| 中出人妻视频一区二区| av在线天堂中文字幕| 国产三级在线视频| 国产伦在线观看视频一区| 狂野欧美激情性xxxx| 18禁美女被吸乳视频| 丰满人妻一区二区三区视频av | 一个人看视频在线观看www免费 | 欧美又色又爽又黄视频| 在线观看舔阴道视频| 色尼玛亚洲综合影院| 黄色片一级片一级黄色片| 一边摸一边抽搐一进一小说| 国产精品精品国产色婷婷| 亚洲无线在线观看| 18禁国产床啪视频网站| 欧美av亚洲av综合av国产av| 欧美绝顶高潮抽搐喷水| 亚洲天堂国产精品一区在线| 亚洲av电影不卡..在线观看| 国产一区二区三区在线臀色熟女| 国产一级毛片七仙女欲春2| 日韩欧美国产在线观看| 别揉我奶头~嗯~啊~动态视频| АⅤ资源中文在线天堂| 国产男靠女视频免费网站| 在线国产一区二区在线| 国产精品 国内视频| 国产国拍精品亚洲av在线观看 | 草草在线视频免费看| 日韩欧美精品v在线| 国产男靠女视频免费网站| 欧美bdsm另类| 午夜a级毛片| 18禁国产床啪视频网站| 亚洲激情在线av| 色噜噜av男人的天堂激情| 97碰自拍视频| 国产亚洲精品久久久久久毛片| 老司机福利观看| 亚洲内射少妇av| 亚洲真实伦在线观看| 3wmmmm亚洲av在线观看| 成人高潮视频无遮挡免费网站| 久久久久精品国产欧美久久久| 国产精品美女特级片免费视频播放器| 91在线精品国自产拍蜜月 | svipshipincom国产片| 久久性视频一级片| 在线观看免费视频日本深夜| 精品一区二区三区人妻视频| 免费av观看视频| 国产高清激情床上av| 欧美又色又爽又黄视频| 国产高清有码在线观看视频| 国产视频一区二区在线看| 国产麻豆成人av免费视频| 午夜久久久久精精品| a在线观看视频网站| 久久精品91无色码中文字幕| 国产一区二区三区视频了| 精品一区二区三区av网在线观看| 欧美丝袜亚洲另类 | 真人一进一出gif抽搐免费| 亚洲欧美日韩卡通动漫| 十八禁网站免费在线| 少妇丰满av| 午夜影院日韩av| 人妻夜夜爽99麻豆av| 网址你懂的国产日韩在线| 免费一级毛片在线播放高清视频| 精品久久久久久久久久久久久| 女生性感内裤真人,穿戴方法视频| 91麻豆精品激情在线观看国产| 久久99热这里只有精品18| 欧美一区二区国产精品久久精品| 精品久久久久久久毛片微露脸| 国产精品三级大全| 久久精品国产清高在天天线| 久久精品夜夜夜夜夜久久蜜豆| 国产野战对白在线观看| 国产高清视频在线播放一区| 国产毛片a区久久久久| 成年版毛片免费区| 久久久久久久久中文| 老司机在亚洲福利影院| 国产精品久久久久久人妻精品电影| 亚洲熟妇熟女久久| 久久精品国产自在天天线| 草草在线视频免费看| 哪里可以看免费的av片| 啪啪无遮挡十八禁网站| 精品免费久久久久久久清纯| 久久久久国内视频| 亚洲人成网站在线播放欧美日韩| 波多野结衣高清作品| 一进一出抽搐动态| 操出白浆在线播放| 国产黄a三级三级三级人| 岛国在线观看网站| 无限看片的www在线观看| 亚洲成人免费电影在线观看| 男女视频在线观看网站免费| 亚洲第一欧美日韩一区二区三区| 男女做爰动态图高潮gif福利片| 蜜桃亚洲精品一区二区三区| 一a级毛片在线观看| 久久精品国产99精品国产亚洲性色| 国产精品影院久久| 国产激情欧美一区二区| 在线观看av片永久免费下载| 久久精品影院6| 99riav亚洲国产免费| 免费看日本二区| av国产免费在线观看| 99在线人妻在线中文字幕| 亚洲第一电影网av| 日韩欧美在线乱码| 久久国产精品影院| 12—13女人毛片做爰片一| 噜噜噜噜噜久久久久久91| 亚洲国产精品成人综合色| 久99久视频精品免费| 国产一级毛片七仙女欲春2| tocl精华| 久久精品国产99精品国产亚洲性色| 一级a爱片免费观看的视频| 久久午夜亚洲精品久久| 午夜a级毛片| 国产av不卡久久| 国产 一区 欧美 日韩| 长腿黑丝高跟| 日韩国内少妇激情av| 国产淫片久久久久久久久 | 亚洲av美国av| 亚洲国产欧美人成| 99国产综合亚洲精品| 成人高潮视频无遮挡免费网站| 亚洲黑人精品在线| 欧美激情久久久久久爽电影| 动漫黄色视频在线观看| 欧美日韩福利视频一区二区| 欧美大码av| 极品教师在线免费播放| 久久这里只有精品中国| 91久久精品电影网| 国产精品亚洲av一区麻豆| 亚洲五月婷婷丁香| 中国美女看黄片| 亚洲av熟女| 男女床上黄色一级片免费看| 欧美精品啪啪一区二区三区| 久久久久九九精品影院| 成人午夜高清在线视频| 亚洲狠狠婷婷综合久久图片| ponron亚洲| 午夜免费男女啪啪视频观看 | 精品久久久久久久末码| 九色成人免费人妻av| 国产男靠女视频免费网站| 动漫黄色视频在线观看| 国产精品综合久久久久久久免费| 欧美日韩黄片免| 国产精品亚洲美女久久久| 欧美+日韩+精品| 最近在线观看免费完整版| 国产精品 国内视频| 国产黄色小视频在线观看| 中亚洲国语对白在线视频| 欧美zozozo另类| 女人十人毛片免费观看3o分钟| 少妇人妻一区二区三区视频| 午夜两性在线视频| 国产亚洲精品av在线| h日本视频在线播放| 在线十欧美十亚洲十日本专区| 亚洲最大成人中文| 中文资源天堂在线| 久久久久久久久中文| 欧美日韩国产亚洲二区| 内射极品少妇av片p| 成人一区二区视频在线观看| 午夜日韩欧美国产| 黑人欧美特级aaaaaa片| 麻豆国产av国片精品| 午夜福利在线观看吧| 亚洲精华国产精华精| 亚洲成av人片免费观看| 精品熟女少妇八av免费久了| 成人无遮挡网站| 精品99又大又爽又粗少妇毛片 | 亚洲精品影视一区二区三区av| 欧美不卡视频在线免费观看| 精品无人区乱码1区二区| 久久人妻av系列| 嫩草影院入口| 国产一区在线观看成人免费| 久久久久久久亚洲中文字幕 | 亚洲精品色激情综合| 90打野战视频偷拍视频| 法律面前人人平等表现在哪些方面| 网址你懂的国产日韩在线| 黄片大片在线免费观看| 午夜两性在线视频| 天美传媒精品一区二区| 老司机午夜十八禁免费视频| 尤物成人国产欧美一区二区三区| 亚洲无线观看免费| 精品熟女少妇八av免费久了| 国产精品久久视频播放| 国产欧美日韩精品亚洲av| 国产成人av教育| 国产精品一区二区免费欧美| 在线免费观看的www视频| 成人高潮视频无遮挡免费网站| 国产欧美日韩一区二区精品| 亚洲av美国av| 免费无遮挡裸体视频| 亚洲人成电影免费在线| 99国产精品一区二区蜜桃av| 俄罗斯特黄特色一大片| 中文字幕人妻丝袜一区二区| www.999成人在线观看| 亚洲,欧美精品.| 欧美性感艳星| 亚洲欧美一区二区三区黑人| 亚洲无线在线观看| 国产三级在线视频| 欧美三级亚洲精品| 国产精品久久视频播放| 亚洲精品亚洲一区二区| 亚洲国产高清在线一区二区三| 国产成+人综合+亚洲专区| 又爽又黄无遮挡网站| 蜜桃久久精品国产亚洲av| svipshipincom国产片| 国产欧美日韩精品一区二区| 亚洲av中文字字幕乱码综合| 成年女人毛片免费观看观看9| 熟女人妻精品中文字幕| 国产中年淑女户外野战色| 精品一区二区三区视频在线 | 中文字幕久久专区| 国产久久久一区二区三区| 久久性视频一级片| 草草在线视频免费看| h日本视频在线播放| 亚洲国产中文字幕在线视频| h日本视频在线播放| 精品国内亚洲2022精品成人| 日本在线视频免费播放| 国产精品影院久久| 日本一二三区视频观看| av片东京热男人的天堂| 搡老妇女老女人老熟妇| 美女cb高潮喷水在线观看| 国产亚洲精品久久久com| 一个人观看的视频www高清免费观看| 丰满人妻熟妇乱又伦精品不卡| 香蕉av资源在线| 精品人妻一区二区三区麻豆 | 国产亚洲欧美98| 午夜福利成人在线免费观看| 波野结衣二区三区在线 | av天堂中文字幕网| 国产一区二区亚洲精品在线观看| 成人av一区二区三区在线看| 国语自产精品视频在线第100页| 变态另类丝袜制服| 久久精品国产自在天天线| 欧美av亚洲av综合av国产av| 国产一区二区在线观看日韩 | 国产久久久一区二区三区| 国语自产精品视频在线第100页| 国产精品久久久久久人妻精品电影| 国产精品亚洲一级av第二区| 99热精品在线国产| 国产探花极品一区二区| 午夜福利在线在线| 99精品欧美一区二区三区四区| 亚洲欧美日韩卡通动漫| 精品人妻一区二区三区麻豆 | 看免费av毛片| 在线观看av片永久免费下载| 18禁黄网站禁片免费观看直播| 19禁男女啪啪无遮挡网站| 毛片女人毛片| 级片在线观看| 精品国产亚洲在线| 国产成人系列免费观看| 少妇裸体淫交视频免费看高清| 欧美日韩福利视频一区二区| 少妇的逼水好多| 亚洲va日本ⅴa欧美va伊人久久| 老熟妇乱子伦视频在线观看| 日韩精品青青久久久久久| 国产精品一区二区三区四区久久| 中亚洲国语对白在线视频| 少妇的丰满在线观看| 国产精品电影一区二区三区| 亚洲人成网站在线播放欧美日韩| 国产不卡一卡二| 亚洲av一区综合| www国产在线视频色| 在线观看舔阴道视频| 波多野结衣高清无吗| 一二三四社区在线视频社区8| 亚洲国产色片| 99久久精品一区二区三区| 日本黄色视频三级网站网址| 一区福利在线观看| 国产精品久久视频播放| 亚洲avbb在线观看| 成人高潮视频无遮挡免费网站| 亚洲乱码一区二区免费版| 色综合站精品国产| 国产成人aa在线观看| 国产 一区 欧美 日韩| 小说图片视频综合网站| 国产91精品成人一区二区三区| 久久久久久久精品吃奶| 成熟少妇高潮喷水视频| 在线观看舔阴道视频| 欧美av亚洲av综合av国产av| 69人妻影院| svipshipincom国产片| 国产一区二区三区视频了| 中文字幕人成人乱码亚洲影| 午夜老司机福利剧场| 成人一区二区视频在线观看| 熟女电影av网| 男人舔女人下体高潮全视频| a在线观看视频网站| 精品国内亚洲2022精品成人| 搞女人的毛片| 最好的美女福利视频网| av在线天堂中文字幕| av片东京热男人的天堂| 免费在线观看日本一区| 日韩欧美 国产精品| 麻豆国产97在线/欧美| 精品一区二区三区视频在线 | 免费电影在线观看免费观看| 性色avwww在线观看| 天堂网av新在线| 麻豆成人av在线观看| 欧美午夜高清在线| 精品欧美国产一区二区三| 国产精品一区二区免费欧美| 中文字幕av成人在线电影| 偷拍熟女少妇极品色| 国产精品久久电影中文字幕| 久久精品91蜜桃| 九九久久精品国产亚洲av麻豆| 一夜夜www| 女警被强在线播放| 成人一区二区视频在线观看| 成人国产一区最新在线观看| 在线观看美女被高潮喷水网站 | 国产99白浆流出| 综合色av麻豆| 无人区码免费观看不卡| 欧美乱码精品一区二区三区| 精华霜和精华液先用哪个| 黄片小视频在线播放| 欧美色欧美亚洲另类二区| 久久精品国产综合久久久| 亚洲精品日韩av片在线观看 | 男人的好看免费观看在线视频| 欧美国产日韩亚洲一区| av天堂中文字幕网| 亚洲,欧美精品.| 色视频www国产| 两性午夜刺激爽爽歪歪视频在线观看| 国产男靠女视频免费网站| 69av精品久久久久久| 啦啦啦韩国在线观看视频| 亚洲专区中文字幕在线| 九色成人免费人妻av| 无人区码免费观看不卡| av福利片在线观看| 欧美日韩中文字幕国产精品一区二区三区| 熟女人妻精品中文字幕| 夜夜躁狠狠躁天天躁| 丁香欧美五月| 真人一进一出gif抽搐免费| 国产精品野战在线观看| 搡老岳熟女国产| 最近最新免费中文字幕在线| 精品久久久久久久人妻蜜臀av| 3wmmmm亚洲av在线观看| 午夜福利在线观看吧| 三级男女做爰猛烈吃奶摸视频| 久久久久久久精品吃奶| 国产综合懂色| 国产真实伦视频高清在线观看 | 人人妻人人看人人澡| avwww免费| 可以在线观看的亚洲视频| 激情在线观看视频在线高清| 国产高清激情床上av| 熟女人妻精品中文字幕| 国产乱人伦免费视频| 男女下面进入的视频免费午夜| 欧美色视频一区免费| 久久精品国产亚洲av涩爱 | 国产亚洲精品久久久com| 黑人欧美特级aaaaaa片| 一进一出抽搐gif免费好疼| 亚洲狠狠婷婷综合久久图片| 少妇人妻精品综合一区二区 | 亚洲va日本ⅴa欧美va伊人久久| 在线看三级毛片| 99久久九九国产精品国产免费| 亚洲内射少妇av| 人妻久久中文字幕网| 人妻夜夜爽99麻豆av| 99国产综合亚洲精品| 精品日产1卡2卡| 亚洲专区国产一区二区| 亚洲无线在线观看| 99热这里只有精品一区| 欧美日韩综合久久久久久 | 三级毛片av免费| 成人国产综合亚洲| 18禁黄网站禁片免费观看直播| 女人十人毛片免费观看3o分钟| 欧美乱码精品一区二区三区| 他把我摸到了高潮在线观看| 国产精华一区二区三区| 国产激情偷乱视频一区二区| 精品国产三级普通话版| 99riav亚洲国产免费| 少妇的逼水好多| 午夜福利在线在线| 国产一区二区三区在线臀色熟女| 尤物成人国产欧美一区二区三区| 欧美乱色亚洲激情| av国产免费在线观看| 无人区码免费观看不卡| 女同久久另类99精品国产91| 久久久成人免费电影| www.www免费av| 国产欧美日韩精品一区二区| 最新中文字幕久久久久| 久久久久国内视频| 香蕉久久夜色| 久久精品夜夜夜夜夜久久蜜豆| 18美女黄网站色大片免费观看| 波多野结衣巨乳人妻| 久久精品影院6| 尤物成人国产欧美一区二区三区| 中文字幕人成人乱码亚洲影| 最近在线观看免费完整版| 国产精品国产高清国产av| 综合色av麻豆| 最新美女视频免费是黄的| 搡老岳熟女国产| 亚洲人与动物交配视频| 午夜两性在线视频| 最近视频中文字幕2019在线8| 黑人欧美特级aaaaaa片| 啦啦啦免费观看视频1| 日韩高清综合在线| 啦啦啦观看免费观看视频高清| 精华霜和精华液先用哪个| 夜夜爽天天搞| 国产熟女xx| 亚洲av成人av| 一本精品99久久精品77| avwww免费| 成人亚洲精品av一区二区| 精品人妻1区二区| 免费看十八禁软件| 99久久精品一区二区三区| 欧美黑人欧美精品刺激| 精品人妻一区二区三区麻豆 | 久久精品国产综合久久久| 午夜免费观看网址| 免费看日本二区| 久久国产乱子伦精品免费另类| 久久久久性生活片| 嫩草影视91久久| 麻豆国产av国片精品| 亚洲一区二区三区色噜噜| 免费观看的影片在线观看| 九九在线视频观看精品| 午夜福利在线观看吧| 99久久九九国产精品国产免费| 偷拍熟女少妇极品色| 欧美日本视频| 亚洲18禁久久av| 99久久成人亚洲精品观看| 国产不卡一卡二| 美女 人体艺术 gogo| 日本黄色视频三级网站网址| 久久天躁狠狠躁夜夜2o2o| 精品福利观看| 国产一级毛片七仙女欲春2| 久久久精品欧美日韩精品| 国产伦精品一区二区三区四那| 在线观看一区二区三区| aaaaa片日本免费| 日韩中文字幕欧美一区二区| 精品免费久久久久久久清纯| 成人永久免费在线观看视频| 99精品欧美一区二区三区四区| 精品人妻一区二区三区麻豆 | 1000部很黄的大片| 18禁裸乳无遮挡免费网站照片| 免费人成在线观看视频色| 亚洲成人精品中文字幕电影| 国产精品美女特级片免费视频播放器| 免费人成在线观看视频色| 国产伦精品一区二区三区视频9 | 亚洲一区高清亚洲精品| 亚洲av电影不卡..在线观看| bbb黄色大片| 欧美高清成人免费视频www| 国内揄拍国产精品人妻在线| 中出人妻视频一区二区| 午夜福利高清视频| 嫁个100分男人电影在线观看| 免费av观看视频| 最近视频中文字幕2019在线8| 真人做人爱边吃奶动态| 国产三级黄色录像| 99热这里只有是精品50| 一进一出好大好爽视频| 欧美日韩亚洲国产一区二区在线观看| 亚洲成人中文字幕在线播放| 欧美黄色淫秽网站| 国产av在哪里看| 欧美色欧美亚洲另类二区| 国产一级毛片七仙女欲春2| 午夜福利视频1000在线观看| 成人国产综合亚洲| 亚洲欧美日韩卡通动漫| 国产精品一区二区三区四区免费观看 | 国产单亲对白刺激| 午夜福利18| 国产单亲对白刺激| 18禁黄网站禁片免费观看直播| 国产单亲对白刺激| 久久精品国产自在天天线| 国产v大片淫在线免费观看| 少妇丰满av| 日本三级黄在线观看| 色哟哟哟哟哟哟| 久99久视频精品免费| 国产精品影院久久| 97超级碰碰碰精品色视频在线观看| 日韩人妻高清精品专区| 在线观看日韩欧美| 色哟哟哟哟哟哟| 日本一二三区视频观看| 亚洲中文字幕日韩| 桃红色精品国产亚洲av| 悠悠久久av| 中文字幕精品亚洲无线码一区| 老司机深夜福利视频在线观看| 欧美一区二区国产精品久久精品| 少妇的逼水好多| 黄色视频,在线免费观看| 熟妇人妻久久中文字幕3abv| 欧美午夜高清在线| 成人亚洲精品av一区二区| 国内揄拍国产精品人妻在线| 高清在线国产一区| 精品国产美女av久久久久小说| 丰满人妻熟妇乱又伦精品不卡| 成人国产一区最新在线观看| 亚洲一区高清亚洲精品| 久久这里只有精品中国| 国产精品一区二区免费欧美| 国产主播在线观看一区二区| 国产又黄又爽又无遮挡在线| 色吧在线观看| 一本精品99久久精品77| 波多野结衣高清作品| 高潮久久久久久久久久久不卡| 亚洲av美国av| 免费一级毛片在线播放高清视频| 久久久精品欧美日韩精品| 搡老熟女国产l中国老女人| а√天堂www在线а√下载| 久久久久国产精品人妻aⅴ院| www.www免费av| 91久久精品电影网| 国内精品久久久久久久电影| 日韩成人在线观看一区二区三区| 老司机福利观看| 高清日韩中文字幕在线| 脱女人内裤的视频| 国产精品爽爽va在线观看网站| 国产亚洲精品一区二区www| 中文字幕人成人乱码亚洲影| av黄色大香蕉| 长腿黑丝高跟| 啦啦啦韩国在线观看视频| 欧美日韩中文字幕国产精品一区二区三区| 国产精品99久久久久久久久| 久久精品91无色码中文字幕|