    Grinding force and surface quality in creep feed profile grinding of turbine blade root of nickel-based superalloy with microcrystalline alumina abrasive wheels

    2021-04-06 10:25:28QingMIAOWenfengDINGWeijieKUANGChangyongYANG
    CHINESE JOURNAL OF AERONAUTICS 2021年2期

    Qing MIAO, Wenfeng DING, Weijie KUANG, Changyong YANG

    National Key Laboratory of Science and Technology on Helicopter Transmission, Nanjing University of Aeronautics and Astronautics, Nanjing 210016, China

    KEYWORDS Creep feed profile grinding;Fir-tree blade root;Grinding force;Single crystal nickel-based superalloy;Surface quality

    Abstract Creep feed profile grinding of the fir-tree blade root forms of single crystal nickel-based superalloy was conducted using microcrystalline alumina abrasive wheels in the present study.The grinding force and the surface quality in terms of surface topography, subsurface microstructure,microhardness and residual stress obtained under different grinding conditions were evaluated comparatively.Experimental results indicated that the grinding force was influenced significantly by the competing predominance between the grinding parameters and the cross-sectional root workpiece profile.In addition,the root workpiece surface,including the root peak and valley regions,was produced with the large difference in surface quality due to the nonuniform grinding loads along the root workpiece profile in normal section. Detailed results showed that the surface roughness, subsurface plastic deformation and work hardening level of the root valley region were higher by up to 25%,20%and 7%in average than those obtained in the root peak region,respectively,in the current investigation. Finally, the superior parameters were recommended in the creep feed profile grinding of the fir-tree blade root forms.This study is helpful to provide industry guidance to optimize the machining process for the high-valued parts with complicated profiles.

    1. Introduction

    The detachable rotating turbine blades are employed by the majority of advanced aero-engines, and they are usually mounted onto a series of rotor disks by using the fir-tree blade root forms (Fig. 1).1,2Due to the strict environment of application,the turbine blade roots are generally fabricated by various nickel-based superalloys and titanium alloys because of their high strength, high wear and corrosion resistance at elevated temperatures.3–5These excellent properties, however,throw great challenges for the efficient and cost-effective machining. In addition, such materials are usually difficult to cut as demonstrated by the large cutting forces, high tooling wear,low machining quality and relatively long manufacturing times,like in the broaching and milling processes for the blade root manufacture.6–13To overcome these problems,creep feed grinding(CFG)is introduced,involving the use of large grinding depth, slow workpiece speed, flexible machining centers equipped with highly porous conventional abrasive wheels,high pressure fluid delivery system, and semicontinuous dressing.2The large grinding depth of CFG is also well preferred due to the large stock allowances of the turbine blade root workpiece.

    Therefore, CFG associated with conventional abrasive wheels becomes the traditional grinding strategy for machining the fir-tree blade root forms.However,a practical result found in previous tests is that the rapid rate of wheel wear and low ability to maintain the dimensional accuracy are always the bottleneck for conventional abrasive wheels to reach a desired grinding efficiency.14Increasing the dressing frequency tends to solve these practical problems, while the tool service life has to be greatly shortened. For this reason, the superhard abrasive wheels, e.g. CBN wheels, are proposed to use for machining the fir-tree blade root. Nevertheless, the high cost and the low potential with regard to the dressing capability are the generally major problems for superhard abrasive wheels to profile grinding,15,16even though it is demonstrated that the active surfaces of superhard abrasive wheel can be specially-designed and textured,17,18and are capable of creep feed grinding deep fir-tree slots and fir-tree root forms on the difficult-to-cut nickel-based superalloys with free workpiece burning.2,19–21On the contrary, due to the low hardness and cost-effective price compared to the superhard abrasive wheels,conventional abrasive wheels are evidenced with an excellent profiling ability and become widely applied in the turbine blade root manufacture. For instance, Poklad22used different alumina abrasive wheels for creep feed grinding the fir-tree blade root forms. High surface quality, e.g.the surface roughness of 0.65 μm and the compressive stress of up to 490 MPa,was achieved. Guo et al.23,24developed the process to realize the continuous dressing creep feed profile grinding of the firtree blade root forms using conventional abrasive wheels.Control of the blade root grinding process was further optimized by monitoring the power signature and adjusting the dress infeed rate and workpiece speed to improve the grinding efficiency. The consequences in above tests indicate that the relatively short service life of conventional abrasive wheels can be offset by the high profiling ability and acceptable surface quality.

    In addition, the newly developed microcrystalline alumina abrasive wheels have the higher potential for profile grinding as evidenced by the large grinding ratios, high MRRs, low grinding forces, low geometrical wear, and good ground surface integrity, compared to the conventional abrasive wheels.25-29This type of grinding wheel is therefore very suitable for creep feed profile grinding blade root forms though further investigations have to be done to optimize the process results.

    To this end, an experimental study for developing the process to creep feed profile grinding the fir-tree blade root forms of single crystal nickel-based superalloy using microcrystalline alumina abrasive wheels was carried out. In particular, only single sided root form was ground and considered throughout the present work for simplicity.The grinding force and surface quality (including the surface topography, subsurface microstructure, microhardness and residual stress) generated under different combinations of grinding parameters were evaluated comparatively. The present investigation can provide a deep understanding and useful guidance for creep feed grinding the high-valued parts with fir-tree forms in production.

    2. Experimental procedure

    Fig. 2 shows the experimental setup for creep feed profile grinding.All the grinding tests were conducted on the Profimat MT-408 grinding center (Blohm, Germany) with a maximum spindle speed of 8000 r/min and power rating of 45 kW. High pressure pumping system(up to 1.5 MPa with the flow rate of 45 L/min) was utilized to cool the grinding zone via the laminar flow nozzle using 5% water based emulsion. Rectangular blocks of single crystal nickel-based superalloy with the dimensions of 32 mm×15 mm×12 mm were employed as the workpiece materials.Detail properties on this workpiece material are shown in Table 1.28,30The workpiece was clamped by the jig which was mounted on the machine worktable (Fig. 2(c)). The microcrystalline alumina abrasive wheels(400 mm×20 mm×127 mm, 5SG80F45V, Sisha Co., Ltd.China) which had the vitrified bond, open structure and mesh size of 80# were used as the grinding tools.

    The full experimental process consisted of 2 grinding cases involving variations in wheel speed vs, workpiece speed vw,grinding depth apand accumulated grinding depth h. The accumulated grinding depth h was the distance that the wheel moved in the vertical direction, as schematically shown in Fig. 3. The total stock allowance of the blade root workpiece was designed as 2.63 mm in the current study. All tests were performed in an up grinding creep feed model without spark-out. The experimental arrangements are displayed in Table 2. Each grinding case involved 6 grinding passes on the workpiece.After each grinding pass,dressing of the wheels was performed by using the diamond roller dresser with the diameter of 152.1 mm and the mesh size of 45#, as shown in Fig. 2(b), under the following conditions: dressing speed 20 m/s, dressing speed ratio -0.7, dressing infeed rate 1.3 mm/min, and total dressing amount 0.2 mm.

    Fig. 2 Experimental setups.

    Table 1 Chemical compositions, heat treatments and mechanical properties of single crystal nickel-based superalloy used in study.28,30

    Fig. 3 Schematic diagram of the profile grinding process in the vertical direction.

    In the creep feed profile grinding process,the grinding force components were measured by the three-component dynamometer modeled HR-FP3407 (H&T Horizon). After grinding, the residual stresses of selected regions on the blade root specimen were firstly measured using the X-ray method by means of a MG2000L goniometer with Mn Kα radiation(LXRD micro-area, Proto, Canada). Two measurements were recorded in one selected region and the results were averaged.Secondly, the surface topography of the specimen was examined by the scanning electron microscope (SEM) (Hitachi S3400, Japan) and then cut perpendicular to the grinding direction.Thirdly,the specimen was polished to achieve a surface roughness of below 0.1 μm,followed by etching for about 30 s using a special reagent (25 mL HNO3+25 mL H2O+50 mL HCl). Finally, the subsurface microstructural examination was conducted with an optical microscope(OM)(Leica DM3000, Germany) and the above-mentioned SEM. In addition, the microhardness evaluation was undertaken with an HXS-1000AK hardness tester using the Vickers indenter at a load of 25 g applied for 15 s.

    3. Results and discussion

    3.1. Grinding forces

    Fig. 4 shows the changes of the grinding force components,including the tangential grinding force Ftand the normal grinding force Fn, as the accumulated grinding depth h increased in the creep feed profile grinding process. It can be observed that, based on the results of grinding case I, as h increased from 1.5 (grinding pass No.1) to 4.13 mm (grinding pass No.4), the grinding force components, i.e., Ftand Fn,increased remarkably from 118.8 to 238.4 N and from 287.5 to 572.9 N, respectively. But the grinding forces changed slightly if h further increased to 5.26 mm (grinding pass No.6) compared to those results obtained when h was 2.63 mm(grinding pass No.3).It was also found in Fig.4 that,Ftand Fnincreased from 118.8 to 144.1 N and from 287.5 to 424.5 N respectively,when h increased from 1.5(grinding pass No.1) to 2.5 mm (grinding pass No.2), while they tended to decrease from 238.4 to 145.2 N and from 572.9 to 361.5 N respectively, when h increased from 4.13 (grinding pass No.4) to 5.13 mm (grinding pass No.5). The common characteristic between the grinding passes No.1 and No.4, No.2 and No.5, No.3 and No.6, respectively, was the same grinding parameters that used in the root forms grinding process(Table 2). However, the changes of corresponding grinding forces were different.Similar trends were found in the grindingcase II.The grinding forces measured based on grinding case II were inevitably larger than those obtained in the grinding case I due to the bigger workpiece speeds used in grinding. These facts indicate that the forces were highly dependent on not only the grinding parameters, but also the accumulated grinding depth in the profile grinding process.

    Table 2 Experimental arrangement.

    Fig. 4 Effect of accumulated grinding depth on changes of grinding force components.

    Workpiece material removal and surface integrity are produced within the wheel-workpiece contact zone during grinding. The wheel-workpiece contact area is therefore an important determinant in the grinding process. In addition,the grinding forces are strongly influenced by the undeformed chip thickness which dominants the workpiece material removal process in the contact zone.31–33To further understand the relationship between the grinding forces, root profiles and the grinding parameters, the changes of grinding force with increasing wheel-workpiece contact area are shown in Fig. 5. Particularly, the contact area S was calculated according to the profile changes of root workpiece (Fig. 3)and can be expressed as follows34:

    where l is the profile length of root workpiece in grinding and dsis wheel diameter.It can be found in Fig.5 that regardless of which case of grinding parameters was used, the wheelworkpiece contact area had generally the positive effects on the increasing grinding force due to the increased numbers of active abrasive grains involved in cutting. In addition,the factors that resulted in the changes of contact area and further affected the grinding force can be analyzed as follows:

    (i) Assuming that the wheel diameter remained constant,Eq.(1)shows that if the root profile length l or the grinding depth apwas decreased,the wheel-workpiece contact area S could be reduced. Apparently, when h=2.63 mm or h=5.26 mm, the profile of root workpiece was very close to the target one and would be great similar (Table 2). At this moment, the small value of approduced the small contact area S (around 120 mm2)and then led to the small grinding force F due to the reduced undeformed chip thickness.34Therefore, in this period, it can be stated that the parameters used in the grinding process were the key factor that dominated the grinding force change.

    (ii) When S was further increased from 155 to 274 mm2,the increased grinding force could be observed in Fig.5,and the values of h varied in the range of 1.5–2.5 mm.At this time,the target profile of root workpiece was unfinished according to Table 2. But both the contact area S and the grinding force F were increasing though apwas decreased.Under this condition,the root profile length l was expended and became the predominant factor that influenced the grinding force.

    Fig. 5 Effect of wheel-workpiece contact area on changes of grinding force components.

    (iii) The grinding force reached the maximum value when the contact area S was increased to 377 mm2.The corresponding h was 4.13 mm.It can be found in Table 2 that apwas increased resulting in large undeformed chip thickness while there was almost no change in the root profile. Under such conditions, the increasing of grinding forces was again mainly caused by the large grinding parameters.

    It results from above analysis that the alternating process between the profile of root workpiece and the grinding parameters affected the grinding forces significantly. This means, if the profile of root workpiece(i.e.,accumulated grinding depth h) was kept the same, the aggressive parameters (i.e., large grinding depth ap) could cause the increased grinding forces due to the large undeformed chip thickness. If the grinding parameters were kept constant,the short profile of root workpiece(i.e.,small wheel-workpiece contact area S)could lead to the reduced grinding forces due to the decreased active grains numbers.This probably gives the rough feel for the control of the grinding force by adjusting the parameters and the root workpiece profile in the creep feed grinding process.

    3.2. Ground surface topography and surface roughness

    Fig. 6 shows the typical surface topography in both the peak region and valley region of the root workpiece ground based on grinding case I. Here, the surface examination positions were marked by the small yellow triangles. As shown in Fig. 6, the surface textures generated were clear and the abrasive grain tracks were uniform.In Fig.7 which shows the typical surface topography of the root workpiece in the grinding case II, these features were also visible but on a less smooth surface.And some slightly black colors were found in the root peak regions as demonstrated in Fig. 7(a), which was possibly the oxidation of workpiece material due to the high grinding temperature.

    The surface roughness Sa was measured by the optical microscope and the results are shown in Fig. 8. For grinding case I, the average surface roughness Sa measured in the root peak region and valley region was 0.37 and 0.48 μm, respectively. Grinding case II produced a larger surface roughness(0.8 μm in the root peak region and 1.0 μm in the root valley region) than grinding case I due to the increased smearing and side flow of the workpiece material (Fig. 7). It was also found in both grinding cases that the surface roughness in the root valley region was higher by around 25% than that in the root peak region. The difference in surface quality of root workpiece could be due to the working state variation of wheel surface during profile grinding.

    Fig. 6 Typical surface topography in different root regions for grinding case I.

    Fig. 7 Typical surface topography in different root regions for grinding case II.

    Fig. 8 Ground surface roughness of root workpiece.

    In the creep feed profile grinding process, the wheel peak regions are firstly in contact with the workpiece, large impact force and force moment can be caused due to the increasing contact area and active grain numbers in the grinding zone.The wear in the wheel peak regions can be induced in the form of grain wear flat, workpiece material adhesion, and the fractures of grains and bond bridges.28Among these wear patterns the fracture wear plays the predominate role, especially in the creep feed grinding of difficult-to-cut materials,such as nickelbased superalloys.This could result in that the peak regions on the wheel surface are worn more easily and quickly than the valley regions in the profile grinding process,14and therefore tend to cause the dimensional errors and the degraded surface quality of root workpiece. For instance, the fractured grains become the hard particles involving in the grinding process and produce various ground surface defects in the workpiece valley regions.34,35This is the reason why the root peak regions had much smoother surface than the root valley regions. It is also worthwhile mentioning that due to the small parameters used in the grinding pass No.6, few surface defects can be observed in Figs. 6(b) and 7(b). However, the large forces induced by grinding passes No.4 and No.5 could lead to great plastic deformation into the subsurface layer though it might be removed partially by grinding pass No.6. This is the main concern in Section 3.3.In addition,the difference of machining quality on the ground surface was also found in the creep feed profile grinding of the gear forms.36,37The root reason can be attributed to the nonuniform distribution of grinding loads along the profile of workpiece in the normal section during grinding.Continuous dressing of the grinding wheel to recover the profile geometry of the worn tool is thus necessary to guarantee the consistence of surface quality of workpiece.

    3.3. Subsurface microstructure

    In Figs.9 and 10,along the profile of root workpiece in normal section, the odd numbers of 1, 3 and 5, and the even numbers of 2,4 and 6 were used to represent the root peak regions and valley regions, respectively. Furthermore, Fig. 9 presents the subsurface microstructures of the root peak region No.3, the root valley region No.4 and the middle region between them,which were produced by grinding case I. Because there was no grain boundary inside the single crystal nickel-based superalloy workpiece, the microstructural alternation was difficult to be observed in the ground surface layer from the optical microscope (Fig. 9(a)–(c)). The high resolution micrographs taken by SEM were displayed in Fig. 9(d)–(f) in the same regions,and showed that the strengthening phases of cuboidal γ′-particles were almost absent due to the etching while the matrix phases of γ-channels were apparent.Moreover,bending γ-phases were clearly visible in Fig. 9(d) and (f). The microstructural deformation to a depth of around 3 μm,2 μm and 4 μm in the peak region No.3 (Fig. 9(d)), middle region (Fig. 9(e)) and valley region No.4 (Fig. 9(f)), respectively, was observed in the ground surface layer.

    Fig. 9 Microstructure variation on cross section of the root workpiece in grinding case I.

    Fig. 10 Microstructure variation on cross section of the root workpiece in grinding case II.

    Using the similar characterization method, the subsurface microstructure of cross section of the root workpiece produced by grinding case II was examined,as shown in Fig.10.Similar to the results of Fig. 9(a)–(c), few visible changes of microstructure were found in the surface layer in Fig. 10(a)–(c) through optical microscope. While severe plastic deformation having the depth of about 4 μm, 3 μm and 8 μm was detected by SEM in the peak region No.3 (Fig. 10(d)), middle region (Fig. 10(e)) and valley region No.4 (Fig. 10(f)), respectively. In particular, in the peak region No.3 (Fig. 10(d)), the defects of several micro cavities were generated in the topmost surface,and the continuous white layer to a depth of about 1–2 μm was found.Similar defects were also observed in the root valley region No.4 (Fig. 10(f)).

    Fig.11 shows the results of the thickness of the microstructural deformation layer estimated by SEM under different grinding conditions. No doubt that grinding case II had a larger value in the deformation layer thickness than grinding case I. Furthermore, the root valley region was of the deformation layer thickness 4.5 μm for grinding case I and 5.8 μm for grinding case II in average. And the corresponding values in the root peak regions became 3.4 and 4.6 μm. This indicates that the deformation layer thickness of the root valley region was typically higher by up to 23% for grinding case I and 21%for grinding case II, respectively, compared to the root peak region.

    During creep feed grinding nickel-based superalloy, the highest plastic deformation is generally formed at the position where the largest grinding forces are generated due to the material removal and wheel wear. This means that, the root valley regions endured greater grinding loads than the root peak regions during profile grinding.In other words, the peak regions on the wheel surface produced larger grinding forces than the valley regions and thus the former can wear more easily.All these led to that the microstructure of the subsurface exhibited great plastic deformation and bending of the γ and γ′phases in the root valley regions,as shown in Figs.9(f)and 10(f). While in the root peak regions, relatively slight plastic deformation was observed. As such, the difference of the subsurface microstructure along the root workpiece profile in the normal section could be created.

    Fig. 11 Variation of the thickness of plastic deformation layer along root workpiece profile in normal section.

    3.4. Mechanical properties of ground surface

    3.4.1. Microhardness

    It is known that the large grinding forces often tend to cause the work hardening of the subsurface as a result of the plastic deformation.38,39While the large amount of heat generated in the grinding zone often raises the thermal softening of the subsurface.40–42The competing process between the work hardening and the thermal softening determines the final state of the subsurface. Usually, for the blade root grinding, the final grinding pass is to removal the grinding burr and obtain the enhanced mechanical properties of the subsurface by using the conservative grinding parameters (i.e., the small grinding depth in grinding pass No.6). Therefore, the work hardening or thermal softening of the subsurface induced by the previous grinding passes might be reduced to some extents. The proper work hardening of the subsurface is always preferred due to the induced compressive residual stress and high wear resistance.

    Microhardness variation beneath the ground surface measured for grinding cases I and II are detailed in Figs. 12 and 13,respectively.In the grinding case I,the near surface microhardness of the root workpiece in different regions varied from 444 to 478 HV0.025, which indicated the occurrence of work hardening. The limited surface hardening level of around 3.2–11.1% was produced to a depth of below 10 μm, which corresponded well with the microstructure detection results shown in Fig. 9. In contrast, changes in microhardness (from 469 to 516 HV0.025) subject to grinding case II were more significant as shown in Fig.13.The surface hardening level of different measured regions was generally in the range of 9.1%-20% to a depth of around 30 μm. The microhardness results of the present study indicate the pronounced working hardening of the subsurface, rather than the thermal softening.

    Fig. 12 Microhardness variation on cross section of root workpiece in grinding case I.

    Fig. 13 Microhardness variation on cross section of the root workpiece in grinding case II.

    Additionally, the microhardness variation in different root regions was measured. In the grinding case I, the average microhardness in the root peak region was 455 HV0.025, with a work hardening level of 5.8%,while the larger work hardening level(up to 10%)was observed in the root valley region.In the grinding case II, the average microhardness for the root peak and valley region, increased up to 466 and 507 HV0.025,respectively, equivalent to the work hardening level of 8.4%and 17.9%. These results indicate that the work hardening level of the root valley region was approximately twice higher compared to that of the root peak region irrespective of the grinding conditions. The reason for this would be the greater than expected plastic deformation produced by the grinding forces in the root valley regions, as descripted in Section 3.3.

    3.4.2. Residual stresses

    Compressive residual stress contributes to improving the fatigue life of stress sensitive parts, i.e., the turbine blade root.Due to the small size of root workpiece and testing method of residual stress of single crystal nickel-based superalloy, the stress in the root valley region was difficult to measure by the stress analyzer.Therefore,Fig.14 only displays the results of the residual stresses measured in the root peak regions under two different grinding conditions. As can be seen from Fig. 14, two principle stresses, i.e., σ11and σ22, for grinding case I, were obtained as -86 and -138 MPa, respectively,while they reached -185 and -440 MPa for grinding case II.The compressive residual stresses were generated in both grinding cases I and II.

    Fig. 14 Residual stresses of ground surface of root workpiece.

    The generation of residual stresses in the ground surface is mainly ascribed to the thermal expansion and phase transformation due to the grinding temperature,and the plastic deformation due to the grinding forces.43The above analysis on the microstructure alternation and work hardening of the subsurface suggests that the grinding forces had the more pronounced effect than the grinding temperature for both grinding cases. Thus, the residual stresses were mainly produced by the mechanical interactions between the grinding wheel and the workpiece. The variation of the mechanical properties of the subsurface can be due to the plastic deformation resulted from the grinding forces. In addition, as can be seen from Fig.14,the aggressive parameters(i.e.,grinding case II) can removal large volume of materials while leading to the high grinding forces and the workpiece appearance changing as well. By comprehensively taking into consideration of the surface topography, subsurface plastic deformation and work hardening, the parameters in the grinding case I might be the superior choice for achieving the better quality of machined surface in the creep feed profile grinding of blade root workpiece,though grinding case II produced the higher compressive stresses on the ground surface.

    4. Conclusions

    In the present study, the profiled microcrystalline alumina abrasive wheels were employed to creep feed grind single crystal nickel-based superalloy for achieving the fir-tree blade root forms.Grinding force and surface quality were evaluated comparatively by using two different groups of parameters. The main results are concluded as follows:

    (1) During creep feed profile grinding of the blade root forms, the combined effects from the grinding parameters and the cross-sectional profile of root workpiece on the grinding forces were found.That is,the root profile had more effects on the grinding forces compared to the grinding parameters when the target root profile wasn’t completely finished, while the grinding parameters dominated the grinding forces when the target root profile was achieved.

    (2) Regardless of the grinding parameters, the surface roughness, the subsurface plastic deformation layer,and the work hardening level in the root valley regions were found to be higher by 25%,22%and 7%on average than those obtained in the root peak region, respectively, in the current investigation.

    (3) In the present study, both grinding cases I and II could produce the ground surfaces with favorable compressive residual stresses (σ11=-86 MPa and σ22=-138 MPa for grinding case I, σ11=-185 MPa and σ22=-440 MPa for grinding case II.).However,grinding case I might produce the better surface quality (i.e., on average,the defect-free surface with Sa 0.43 μm, the subsurface plastic deformation of 4 μm, and the work hardening level of 7.9% to a depth of below 10 μm) in the creep feed profile grinding of the blade root forms in general.

    Acknowledgements

    The authors gratefully acknowledge the financial support for this work by the National Natural Science Foundation of China (No. 51775275), the Funding of Jiangsu Innovation Program for Graduate Education of China (KYCX17_0245),the Funding for Outstanding Doctoral Dissertation in NUAA of China (BCXJ17-04), the Fundamental Research Funds for the Central University of China (No. NP2018110), the National Science and Technology Major Project and the Six Talents Summit Project in Jiangsu Province of China (No.JXQC-002).

    精品久久蜜臀av无| 亚洲av成人av| 淫秽高清视频在线观看| 日韩高清综合在线| 日韩欧美在线二视频| 91九色精品人成在线观看| 国产精品亚洲美女久久久| 亚洲一区二区三区色噜噜| 国产精品久久久久久精品电影 | 欧美日韩亚洲国产一区二区在线观看| 搞女人的毛片| 亚洲自拍偷在线| 亚洲精品美女久久av网站| 国产精品久久视频播放| 高清在线国产一区| 熟女电影av网| 亚洲精品美女久久久久99蜜臀| 色播亚洲综合网| 老司机午夜福利在线观看视频| 日日爽夜夜爽网站| 日韩欧美 国产精品| 国产免费av片在线观看野外av| 嫩草影院精品99| 三级毛片av免费| 成人欧美大片| av天堂在线播放| 国产精品日韩av在线免费观看| 丝袜人妻中文字幕| 中文在线观看免费www的网站 | 啦啦啦免费观看视频1| 国产精品av久久久久免费| 别揉我奶头~嗯~啊~动态视频| 国产高清videossex| 美女国产高潮福利片在线看| 国产在线观看jvid| 国产精品爽爽va在线观看网站 | 国产精品99久久99久久久不卡| 午夜影院日韩av| a级毛片a级免费在线| 国产麻豆成人av免费视频| 免费在线观看日本一区| 97碰自拍视频| 搡老妇女老女人老熟妇| 欧洲精品卡2卡3卡4卡5卡区| av免费在线观看网站| 草草在线视频免费看| cao死你这个sao货| 国产又黄又爽又无遮挡在线| 一进一出抽搐gif免费好疼| 亚洲熟妇中文字幕五十中出| 非洲黑人性xxxx精品又粗又长| 久久青草综合色| 国产成人欧美| 亚洲熟妇中文字幕五十中出| 日本撒尿小便嘘嘘汇集6| 久久久久久久久中文| 国产精品影院久久| av视频在线观看入口| 亚洲第一欧美日韩一区二区三区| 欧美国产精品va在线观看不卡| 欧美日本亚洲视频在线播放| 99久久无色码亚洲精品果冻| 黄色丝袜av网址大全| 久热爱精品视频在线9| 黄色女人牲交| 日本 欧美在线| 亚洲国产精品久久男人天堂| 999久久久精品免费观看国产| 91麻豆精品激情在线观看国产| 99国产精品一区二区蜜桃av| 精品第一国产精品| 麻豆久久精品国产亚洲av| 国产精品二区激情视频| av在线天堂中文字幕| 久久久久久久精品吃奶| 成在线人永久免费视频| 搡老妇女老女人老熟妇| 国产成人精品无人区| 身体一侧抽搐| 国产不卡一卡二| 国产91精品成人一区二区三区| 国产主播在线观看一区二区| 国产一区二区在线av高清观看| 黄色视频,在线免费观看| 免费女性裸体啪啪无遮挡网站| a在线观看视频网站| 男人操女人黄网站| 日本成人三级电影网站| 亚洲自偷自拍图片 自拍| 亚洲一区二区三区不卡视频| 老熟妇乱子伦视频在线观看| 每晚都被弄得嗷嗷叫到高潮| 亚洲 国产 在线| 丰满的人妻完整版| 黑丝袜美女国产一区| e午夜精品久久久久久久| 香蕉久久夜色| 国产欧美日韩一区二区三| 国产精品久久视频播放| 欧美成人免费av一区二区三区| 国产视频内射| 99精品久久久久人妻精品| 十分钟在线观看高清视频www| 免费在线观看日本一区| 丁香欧美五月| 男女视频在线观看网站免费 | 高清在线国产一区| 大型黄色视频在线免费观看| 两个人视频免费观看高清| √禁漫天堂资源中文www| 国产乱人伦免费视频| 国产高清激情床上av| 日韩大码丰满熟妇| 久久 成人 亚洲| 亚洲真实伦在线观看| 成在线人永久免费视频| 一本精品99久久精品77| 国产精品影院久久| 69av精品久久久久久| 久久午夜综合久久蜜桃| 亚洲熟女毛片儿| 亚洲精品美女久久久久99蜜臀| 欧美人与性动交α欧美精品济南到| 精品一区二区三区av网在线观看| 久久精品人妻少妇| 51午夜福利影视在线观看| 99热这里只有精品一区 | 成年女人毛片免费观看观看9| 国产伦在线观看视频一区| 一a级毛片在线观看| 这个男人来自地球电影免费观看| 两个人看的免费小视频| 欧美又色又爽又黄视频| 欧美黑人巨大hd| 日本一本二区三区精品| 91成人精品电影| 欧美日韩乱码在线| 91大片在线观看| 午夜福利高清视频| 免费搜索国产男女视频| 欧美最黄视频在线播放免费| 中文字幕人成人乱码亚洲影| 给我免费播放毛片高清在线观看| 黄色a级毛片大全视频| 国内少妇人妻偷人精品xxx网站 | 变态另类丝袜制服| 国产一区二区激情短视频| 精品国产美女av久久久久小说| 日本三级黄在线观看| 日日夜夜操网爽| 亚洲欧美精品综合一区二区三区| 久久精品人妻少妇| 成人三级黄色视频| 99re在线观看精品视频| 一区二区日韩欧美中文字幕| 黄片小视频在线播放| 欧美日韩亚洲综合一区二区三区_| 国产成人影院久久av| 精品午夜福利视频在线观看一区| 最新美女视频免费是黄的| 又黄又爽又免费观看的视频| 99国产极品粉嫩在线观看| 亚洲熟妇中文字幕五十中出| 99riav亚洲国产免费| 国产亚洲欧美精品永久| 黑人操中国人逼视频| 色哟哟哟哟哟哟| 99热只有精品国产| 精品久久久久久久末码| 国产片内射在线| 在线观看66精品国产| 国产欧美日韩一区二区精品| 啦啦啦 在线观看视频| 亚洲,欧美精品.| 女人高潮潮喷娇喘18禁视频| 啦啦啦免费观看视频1| 久久久久久国产a免费观看| 亚洲五月婷婷丁香| 精品久久久久久成人av| 欧美精品亚洲一区二区| 国产成人系列免费观看| 听说在线观看完整版免费高清| 亚洲五月婷婷丁香| 精品久久久久久久久久久久久 | 亚洲三区欧美一区| 一级a爱片免费观看的视频| 天天添夜夜摸| 非洲黑人性xxxx精品又粗又长| 超碰成人久久| 99热只有精品国产| 午夜福利成人在线免费观看| 午夜福利高清视频| 午夜免费激情av| 国产熟女xx| 亚洲成人国产一区在线观看| 欧美一级毛片孕妇| 自线自在国产av| 真人做人爱边吃奶动态| 色综合亚洲欧美另类图片| 热99re8久久精品国产| 国产黄片美女视频| 日本免费a在线| 久久这里只有精品19| 中文字幕久久专区| 人人妻人人看人人澡| 亚洲国产日韩欧美精品在线观看 | 波多野结衣巨乳人妻| 国产午夜福利久久久久久| 久久天堂一区二区三区四区| 一个人观看的视频www高清免费观看 | 日韩视频一区二区在线观看| 一进一出抽搐动态| 人妻丰满熟妇av一区二区三区| 亚洲欧美精品综合一区二区三区| 搡老岳熟女国产| 欧美激情高清一区二区三区| 亚洲男人的天堂狠狠| 少妇粗大呻吟视频| 国产成人影院久久av| 欧美日本视频| 日韩三级视频一区二区三区| 国内久久婷婷六月综合欲色啪| 日韩欧美 国产精品| 日韩欧美免费精品| 国产v大片淫在线免费观看| 亚洲av片天天在线观看| 国产精品一区二区精品视频观看| 午夜视频精品福利| 国产91精品成人一区二区三区| 午夜福利免费观看在线| 欧美日韩一级在线毛片| 91麻豆av在线| 熟妇人妻久久中文字幕3abv| 亚洲成人精品中文字幕电影| 黄色视频,在线免费观看| 十分钟在线观看高清视频www| 久久精品国产亚洲av香蕉五月| 国产亚洲精品久久久久5区| 在线观看日韩欧美| 久久国产亚洲av麻豆专区| 亚洲精品中文字幕在线视频| 两个人免费观看高清视频| 中文字幕另类日韩欧美亚洲嫩草| 看免费av毛片| 国产蜜桃级精品一区二区三区| 亚洲人成电影免费在线| 妹子高潮喷水视频| 亚洲五月天丁香| 热re99久久国产66热| 国产主播在线观看一区二区| 久久久久国产一级毛片高清牌| 亚洲 欧美 日韩 在线 免费| cao死你这个sao货| 两性午夜刺激爽爽歪歪视频在线观看 | 国产高清视频在线播放一区| 午夜福利在线观看吧| 亚洲av片天天在线观看| 日韩三级视频一区二区三区| 国产成人av激情在线播放| 国产三级在线视频| 精品无人区乱码1区二区| 国产亚洲av高清不卡| 亚洲性夜色夜夜综合| 欧美一级a爱片免费观看看 | 人成视频在线观看免费观看| 欧美日本视频| 国产三级黄色录像| 日韩大尺度精品在线看网址| 精品乱码久久久久久99久播| 亚洲第一电影网av| 亚洲精品久久成人aⅴ小说| 国产欧美日韩一区二区精品| 亚洲人成网站在线播放欧美日韩| av在线天堂中文字幕| 久久青草综合色| 亚洲片人在线观看| 亚洲第一欧美日韩一区二区三区| 日韩欧美国产一区二区入口| 99精品久久久久人妻精品| 女同久久另类99精品国产91| 啪啪无遮挡十八禁网站| 亚洲va日本ⅴa欧美va伊人久久| 人人妻,人人澡人人爽秒播| 91国产中文字幕| 91在线观看av| 淫秽高清视频在线观看| 亚洲av中文字字幕乱码综合 | 亚洲在线自拍视频| 午夜免费观看网址| 色尼玛亚洲综合影院| 嫩草影视91久久| 日日干狠狠操夜夜爽| 国产精品久久久av美女十八| 久久婷婷成人综合色麻豆| www.999成人在线观看| 国产成人精品久久二区二区91| 亚洲五月婷婷丁香| 久久国产精品人妻蜜桃| 日韩欧美 国产精品| 变态另类丝袜制服| xxxwww97欧美| 女性被躁到高潮视频| 国产精品,欧美在线| 99在线视频只有这里精品首页| 久久午夜综合久久蜜桃| 丝袜在线中文字幕| 成人免费观看视频高清| 久久久久国产一级毛片高清牌| 亚洲色图av天堂| 美女高潮喷水抽搐中文字幕| 久久这里只有精品19| 韩国av一区二区三区四区| 99re在线观看精品视频| 俺也久久电影网| netflix在线观看网站| 免费在线观看完整版高清| 特大巨黑吊av在线直播 | 久久天躁狠狠躁夜夜2o2o| 亚洲专区字幕在线| 一夜夜www| 国产熟女xx| 十八禁网站免费在线| 久久国产精品人妻蜜桃| 他把我摸到了高潮在线观看| 级片在线观看| 日韩欧美一区视频在线观看| 99久久精品国产亚洲精品| 999精品在线视频| 国产黄色小视频在线观看| 黑人操中国人逼视频| 琪琪午夜伦伦电影理论片6080| 国产高清videossex| 草草在线视频免费看| 精品久久蜜臀av无| 亚洲自拍偷在线| 久久久精品国产亚洲av高清涩受| 亚洲 欧美 日韩 在线 免费| 成年人黄色毛片网站| 国产精品1区2区在线观看.| 狠狠狠狠99中文字幕| 又黄又粗又硬又大视频| 91成年电影在线观看| 啦啦啦韩国在线观看视频| 欧美黑人欧美精品刺激| 精品一区二区三区av网在线观看| 国产男靠女视频免费网站| 一进一出抽搐动态| www.自偷自拍.com| 在线观看日韩欧美| 97碰自拍视频| 桃色一区二区三区在线观看| 国产野战对白在线观看| 国产国语露脸激情在线看| 亚洲精品国产区一区二| 别揉我奶头~嗯~啊~动态视频| 国产黄片美女视频| 一边摸一边抽搐一进一小说| 日韩中文字幕欧美一区二区| 91国产中文字幕| 91在线观看av| 一个人免费在线观看的高清视频| 91大片在线观看| 少妇被粗大的猛进出69影院| 很黄的视频免费| 人人妻,人人澡人人爽秒播| x7x7x7水蜜桃| 亚洲欧美日韩无卡精品| 午夜福利成人在线免费观看| 国产av一区二区精品久久| 免费看日本二区| 18禁黄网站禁片免费观看直播| 99热6这里只有精品| 午夜福利在线在线| 首页视频小说图片口味搜索| 村上凉子中文字幕在线| 亚洲第一欧美日韩一区二区三区| 村上凉子中文字幕在线| 午夜福利成人在线免费观看| 少妇被粗大的猛进出69影院| 精品久久久久久久久久久久久 | 免费在线观看亚洲国产| 精品久久久久久,| 欧美黄色淫秽网站| av天堂在线播放| 国产亚洲欧美98| 国产爱豆传媒在线观看 | 午夜久久久久精精品| 久热这里只有精品99| av片东京热男人的天堂| 我的亚洲天堂| 欧美中文综合在线视频| 成人永久免费在线观看视频| 在线观看一区二区三区| 黄色片一级片一级黄色片| 亚洲自偷自拍图片 自拍| 1024香蕉在线观看| 国产色视频综合| 亚洲午夜精品一区,二区,三区| 久久久久久久久久黄片| 国产97色在线日韩免费| 一级黄色大片毛片| 91av网站免费观看| 99精品在免费线老司机午夜| 亚洲片人在线观看| 在线看三级毛片| 亚洲精品中文字幕在线视频| 精品国产乱码久久久久久男人| 91大片在线观看| 精品久久久久久,| 欧美人与性动交α欧美精品济南到| 欧美乱色亚洲激情| 精品国产美女av久久久久小说| 国产单亲对白刺激| 久久婷婷人人爽人人干人人爱| 亚洲精品国产一区二区精华液| 国产三级在线视频| 人妻久久中文字幕网| 男女下面进入的视频免费午夜 | 一级a爱视频在线免费观看| 色播亚洲综合网| 精品不卡国产一区二区三区| 午夜精品在线福利| 午夜视频精品福利| 桃色一区二区三区在线观看| 午夜a级毛片| 国产av一区在线观看免费| 亚洲男人天堂网一区| 观看免费一级毛片| 女生性感内裤真人,穿戴方法视频| 成年女人毛片免费观看观看9| 每晚都被弄得嗷嗷叫到高潮| 制服丝袜大香蕉在线| 级片在线观看| 亚洲美女黄片视频| 最近最新中文字幕大全免费视频| √禁漫天堂资源中文www| 成人av一区二区三区在线看| 日本 欧美在线| 国产精品亚洲美女久久久| 国产欧美日韩一区二区三| 亚洲人成伊人成综合网2020| 久久婷婷成人综合色麻豆| 欧美成人一区二区免费高清观看 | 亚洲片人在线观看| 亚洲成国产人片在线观看| 成人av一区二区三区在线看| a在线观看视频网站| 国产精品亚洲美女久久久| 亚洲精品美女久久av网站| 中出人妻视频一区二区| 久久国产精品男人的天堂亚洲| x7x7x7水蜜桃| 久久精品人妻少妇| www.自偷自拍.com| 精品久久久久久久毛片微露脸| 午夜久久久在线观看| 精品国内亚洲2022精品成人| 91成人精品电影| 99riav亚洲国产免费| 欧美激情久久久久久爽电影| 90打野战视频偷拍视频| 国产aⅴ精品一区二区三区波| 人人妻人人澡欧美一区二区| 久久久国产成人免费| 午夜两性在线视频| 欧美zozozo另类| 老司机深夜福利视频在线观看| 变态另类丝袜制服| 夜夜躁狠狠躁天天躁| 久久中文看片网| 精品日产1卡2卡| 亚洲欧美日韩无卡精品| av片东京热男人的天堂| 国产午夜福利久久久久久| 99riav亚洲国产免费| 亚洲欧美精品综合一区二区三区| 叶爱在线成人免费视频播放| 啦啦啦观看免费观看视频高清| 一区福利在线观看| 熟女少妇亚洲综合色aaa.| 男女做爰动态图高潮gif福利片| 国产aⅴ精品一区二区三区波| 久久精品影院6| 好看av亚洲va欧美ⅴa在| 亚洲国产欧美一区二区综合| 老熟妇仑乱视频hdxx| 狂野欧美激情性xxxx| 18禁国产床啪视频网站| 亚洲av中文字字幕乱码综合 | 国产亚洲精品综合一区在线观看 | 成熟少妇高潮喷水视频| 国产精品二区激情视频| 久久精品国产综合久久久| 国产精品 欧美亚洲| 免费av毛片视频| 脱女人内裤的视频| 午夜亚洲福利在线播放| 欧美三级亚洲精品| 国产亚洲欧美98| 一进一出好大好爽视频| 99久久99久久久精品蜜桃| 欧美黑人巨大hd| 老熟妇仑乱视频hdxx| 婷婷丁香在线五月| 免费高清视频大片| 免费在线观看视频国产中文字幕亚洲| 欧美成人一区二区免费高清观看 | 中文亚洲av片在线观看爽| 无人区码免费观看不卡| 久久亚洲精品不卡| 中文字幕av电影在线播放| 少妇裸体淫交视频免费看高清 | 精品国产超薄肉色丝袜足j| 黄色片一级片一级黄色片| 日韩精品免费视频一区二区三区| 亚洲人成网站高清观看| 免费女性裸体啪啪无遮挡网站| 一级a爱视频在线免费观看| 99在线视频只有这里精品首页| av中文乱码字幕在线| 正在播放国产对白刺激| 国产精品自产拍在线观看55亚洲| 国产精品99久久99久久久不卡| 欧美色视频一区免费| 波多野结衣av一区二区av| √禁漫天堂资源中文www| 国产欧美日韩精品亚洲av| 亚洲最大成人中文| 99在线视频只有这里精品首页| 村上凉子中文字幕在线| 91老司机精品| 亚洲七黄色美女视频| 精品国产亚洲在线| 老司机午夜福利在线观看视频| 1024香蕉在线观看| 亚洲国产欧美网| 母亲3免费完整高清在线观看| 身体一侧抽搐| 精品日产1卡2卡| 国产一区二区在线av高清观看| 香蕉久久夜色| 国产色视频综合| 丁香欧美五月| 亚洲精品av麻豆狂野| 日日干狠狠操夜夜爽| 每晚都被弄得嗷嗷叫到高潮| 亚洲精品国产一区二区精华液| 十八禁网站免费在线| 岛国在线观看网站| 中文字幕人妻熟女乱码| 97人妻精品一区二区三区麻豆 | 日韩欧美一区视频在线观看| 日日夜夜操网爽| 啪啪无遮挡十八禁网站| 国产精品久久久久久亚洲av鲁大| 欧美日韩亚洲国产一区二区在线观看| 长腿黑丝高跟| 午夜激情av网站| 一本一本综合久久| 日韩 欧美 亚洲 中文字幕| 久久青草综合色| 男女视频在线观看网站免费 | 变态另类丝袜制服| 国语自产精品视频在线第100页| 99精品久久久久人妻精品| 久久亚洲精品不卡| 国产亚洲精品av在线| 男人的好看免费观看在线视频 | 黄频高清免费视频| 日本黄色视频三级网站网址| 中出人妻视频一区二区| 美女高潮到喷水免费观看| 亚洲av五月六月丁香网| 免费在线观看成人毛片| 88av欧美| 婷婷亚洲欧美| 日韩一卡2卡3卡4卡2021年| 日韩欧美一区二区三区在线观看| 精品久久久久久久人妻蜜臀av| 亚洲精品中文字幕一二三四区| 亚洲一区二区三区色噜噜| 精品久久久久久成人av| 久久久精品欧美日韩精品| 精品国产亚洲在线| 色av中文字幕| 国产一区二区三区在线臀色熟女| 久久国产精品影院| 免费看日本二区| 亚洲中文av在线| 黑人巨大精品欧美一区二区mp4| 午夜老司机福利片| 久久中文看片网| 欧美日韩瑟瑟在线播放| 午夜激情福利司机影院| 18禁国产床啪视频网站| 亚洲专区字幕在线| 免费在线观看黄色视频的| 久久亚洲精品不卡| 国产伦在线观看视频一区| 中文字幕人妻熟女乱码| 日韩欧美一区视频在线观看| 午夜日韩欧美国产| 俺也久久电影网| 美女午夜性视频免费| 丁香六月欧美| 俺也久久电影网| 一a级毛片在线观看| 久久精品国产综合久久久| 一区二区三区精品91| av在线播放免费不卡| 中文资源天堂在线| 精品欧美国产一区二区三| 一区二区日韩欧美中文字幕| 国产亚洲精品综合一区在线观看 | 啦啦啦观看免费观看视频高清|