    Effects of admixture on properties of recycled aggregate mortar

    2020-10-15 02:56:26MiRenjiePanGanghuaLiYang

    Mi Renjie Pan Ganghua Li Yang

    (1 School of Materials Science and Engineering, Southeast University, Nanjing 211189, China)(2 Jiangsu Key Lab of Construction Materials, Nanjing 211189, China)(3 Jiangsu Collaborative Innovation Center, Nanjing 211189, China)(4 Department of Architecture and Civil Engineering, City University of Hong Kong, Hong Kong 999077, China)

    Abstract:Compared with strengthening the recycled fine aggregate (RFA) from construction and demolition waste, which is time-consuming and complex, adding admixture into the mixtures directly is more efficient and effective to expand the application of recycled aggregate mortar(RAM). The admixture (named as SSC), mixed with sodium hexametaphosphate, sodium ligninsulfonate and citric acid, was directly added into the RAM. First, the compositions and physical properties of the RFA and reference aggregate were studied, respectively. The properties of fresh and hardened mortars were then investigated. The results show that there is a clear difference between the RFA and reference aggregate, and the properties of RAM without SSC are not as good as those of normal mortar. However, the consistency value, water retention rate, compressive strength and setting time values of RAM increase by 5%,7%, 66% and 67%, and its consistency loss and density values decrease by 42% and 4% after the SSC is added into the RAM. Therefore, improving the properties of RAM through adding admixture is an effective and efficient approach to expanding its application.

    Key words:construction and demolition waste; recycled fine aggregate; recycled aggregate mortar; admixture

    Construction and demolition waste (CDW) has put a burden on the environment. Therefore, using the recycled fine aggregate (RFA) produced by the waste concrete in CDW to replace natural fine aggregate (NFA) can lower the pollution generated by CDW[1]. However, the RFA shows a high crush value, a high water absorption and a high powder content[23], so that the RFA cannot be widely used by mortar plants[46]due to its adverse impacts on the density[710]and consistency[7,1011]of fresh mortar, and on the setting time[9]and drying shrinkage[710,12]of hardened mortar. Therefore, many methods have been developed to enhance the properties of the mortar with RFA. For example, Pan et al.[23]increased the content of carbonated compounds in the RFA by calcium hydroxide pre-soaking. The results show that there is a significant improvement on the properties of aggregate, and on the flowability and compressive strength of the mortar. However, the processes of the above-mentioned strengthening method may require much time. Thus, these methods cannot be widely applied in actual projects.

    Fortunately, adding admixture directly into the cement-based materials with RFA makes it possible to shorten the procedure. Meanwhile, admixture can improve the properties of cement-based materials. For example, sodium ligninsulfonate (SL) and sodium hexametaphosphate (SH) benefit the cement hydration because they can induce the dispersion of the cement particle by favouring mutual repulsion and hindering flocculation[1315]. Additionally, SH and citric acid (CA) are responsible for prolonging the setting time of mixtures by forming an adsorption layer on the surface of the cement particle, which can isolate the contact of water from cement minerals and hinder the release of the ions into the solution[1314, 1617].

    However, it is still unclear whether admixture can improve the properties of recycled aggregate mortar (RAM). Therefore, in this study, SL, SH and CA were directly added into the RAM. The objective of this research is to investigate whether the used admixture can improve the properties of fresh and hardened RAMs. This study is significant because it can remind readers to add admixture directly to improve the properties of RAM rather than spending a lot of time to strengthen the properties of RFA for obtaining high-quality RAM. This can help mortar plants maximize the recycling of CDW and further mitigate the CDW pollution on the environment.

    1 Materials and Experiments

    1.1 Materials

    1.1.1 Aggregate

    River sand was used as the NFA, while the RFA was prepared by the CDW from housing in Zhenjiang in the 1980s. The CDW was offered by the Jiangsu Zhenjiang Research Institute of Building Science Group Co., Ltd. after be stored for 1 year. Afterwards, it was subjected to a primary crushing procedure for preparing the RFA and then put indoors for natural preservation. The fineness modulus of NFA and RFA are 2.7 and 2.8, respectively.

    1.1.2 Cementitious materials

    P·O 42.5 Portland cement which has properties that conform to the requirements of a Chinese specification[18]was provided by the Jiangsu Helin Cement Corporation. Its physical properties and chemical components were tested according to a Chinese specification[18]and the results are listed in Tabs.1 and 2, respectively. Additionally, the Zhenjiang Jianbi Power Plants provided the fly ash (FA) which is defined as level-2 based on the requirements of a Chinese specification[19]. The thickening powder, whose properties are given in Tab.3, was supplied by the Jiangsu Zhenjiang Research Institute of Building Science Group Co., Ltd.

    Tab.1 Properties of P·O 42.5 Portland cement

    Tab.2 Chemical composition of P·O 42.5 Portland cement %

    Tab.3 Properties of thickening powder

    1.1.3 Admixture

    The SL, SH and CA were offered by the Shanghai Yunzhe New Material Technology Company, Tianjin Hengxing Chemical Reagent Manufacturing Company and Sinopharm Chemical Reagent Company, respectively. In this study, the SL, SH and CA were mixed at a ratio of 2: 6: 1[20]and then the mixed admixture was labeled as SSC. The SSC was added into the mortar mixtures at 0.5% of the binding materials.

    1.2 Experiments

    1.2.1 Preparation

    According to the specific surface area method for mix proportion design[21], the specific surface area of aggregate should be decreased as much as possible to lower the consumption of cement. Thus, during the mix proportion design of RAMs, most researchers[2224]replaced NFA using the volume-replacement method since the density values of the RFAs in these studies were lower than those of the NFAs. However, in this study, the packing density of the NFA (1 520 kg/m3) is lower than that of the RFA (1 580 kg/m3). Thus, the authors decided to replace the NFA using the weight-replacement method to lower the specific surface area of the aggregate.

    Mortar mixtures with a compressive strength grade of 10 MPa were prepared, and the mix proportions were designed based on the specific surface area method[21]and the requirements in a Chinese specification[25], and the results are listed in Tab.4. Three kinds of mixtures were prepared: 1) The mixtures with the NFA were used as the reference (REF); 2) The mixtures with the RFA at a replacement rate of 100% were labeled as the RAM; and 3) The mixtures with the RFA at a replacement rate of 100% and with SSC were labeled as RAM+SSC. The mortar mixtures were cast in some plastic molds, compacted using a vibrating table, covered with a plastic sheet and then cured in a laboratory. The specimens were demolded after 24 h and further cured in a water curing tank at (27±1)℃ for 27 d. After that, all the specimens were removed from the curing tank for various tests.

    Tab.4 Mix proportions of mortars

    1.2.2 Testing

    The tests were divided into three groups and all the mean values of the properties for mortar specimens were obtained by three measurements. Firstly, two types of experiments were conducted to test the properties of fine aggregates: 1) The X-ray diffraction (XRD) patterns of the fine aggregates were collected using a D8 Advance instrument from Bruker AXS; and 2) The physical properties including crush value, water absorption rate, powder content, and packing density of the fine aggregates were obtained based on two Chinese standards[2627]. Secondly, four types of experiments were conducted to test the properties of the fresh mortars based on the Chinese specification[28]. The consistency and consistency loss after 2 h were obtained, while the water retention rate and apparent density were achieved based on the Chinese standard[29]. Thirdly, based on the Chinese standard[29], the experiments for the setting time and compressive strength at 28 d were conducted for the hardened mortars.

    2 Results and Discussion

    2.1 Aggregate

    2.1.1 Composition

    To investigate the composition of the fine aggregates, the XRD patterns are shown in Fig.1. As seen, quartz was detected in both the RFA and NFA, whereas CaCO3(CC) present in the form of calcite was only detected in the RFA. This is in agreement with Pan et al.’s work[2]. This is because the concrete members were subject to CO2attacks for approximately 30 years. Thus, most of Ca(OH)2in the cement paste has been transferred into CC due to the carbonation reaction[3031].

    Fig.1 XRD patterns for fine aggregates

    2.1.2 Physical properties

    Fig.2 displays the physical properties of the fine aggregates. It is clear that the powder content of the RFA (14.2%) is higher than that of the NFA (2.0%) because the powders are attached to the aggregate during the crushing of CDW. In addition, the water absorption rate of the RFA is 2.66% higher than that of the NFA because more cracks exist in the RFA[2]. Moreover, the RFA shows a higher crush value, which can also be ascribed to the fact that the RFA has more micro-cracks compared with the NFA[2]. As a result, the RFA shows a lower strength, which increases its crush value.

    2.2 Fresh mortar

    2.2.1 Consistency

    The consistency of fresh mortar is affected by three parameters: 1) The total amount of free water; 2) The rate between water and fine particle; and 3) The roughness of the aggregate surface[11]. Fig.3 displays the consistency values of the fresh mortars. It is evident that the consistency value of the RAM is lower than that of the REF by 3 mm, which is similar to the results obtained in a previous study[7]. This can be explained by two factors:1) The surface of the NFA is smoother than that of the RFA[2]; and 2) The micro powder content of the RFA is higher than that of the NFA (see Fig.2). Therefore, after all the NFAs are replaced by the RFAs, much free water is limited by the flocculate structures formed by micro powers because small particles can generate surface free energy[32].

    Fig.2 Physical properties of fine aggregates

    Fig.3 Consistency values of fresh mortars

    Additionally, the consistency value of the RAM+SSC is higher than that of the RAM by 4 mm and similar to the value of the REF, which means that the SSC has some positive effects on the consistency of the RAM. This is because the amount of free water in the RAM+SSC is higher than that in the RAM because the SH and SL in the SSC can disperse the flocculate structures generated by micro powders[1315]. Thus, much free water is present in the RAM+SSC mixtures.

    2.2.2 Water retention rate and consistency loss

    Fig.4 depicts the water retention rates and consistency loss values of the fresh mortars. It is evident that the value of consistency loss of the RAM (50.0 mm) is higher than that of the REF (28.9 mm). A possible reason is that the water absorption rate of the RFA is higher than that of the NAF (see Fig.2). Interestingly, the water retention rate of the RAM (89.8%) is also higher than that of the REF (84.5%). This can also be attributed to the results of the water absorption rate.

    Fig.4 Water retention rates and consistency loss values of fresh mortars

    In terms of the RAM + SSC, their consistency loss value is similar to that of the REF. Due to the fact that the products generated by the complexation between the ingredients of the chemical admixture, the SH and CA in the SSC, and the Ca2+in the cement are hydrophilic[13, 16], much water can remain in the mixtures instead of flowing out.

    2.2.3 Density

    Fig.5 presents the density values of the fresh mortars. It is evident that the density value of the RAM (1 890 kg/m3) is higher than that of the REF (1 830 kg/m3), which is in agreement with the result in Ref.[33]. This is because the water absorption rate of the RFA is higher than that of NFA (see Fig.2). As for the RAM+SSC, their density, which is similar to that of the REF, is lower than that of the RAM by 70 kg/m3as the water-binder ratio is reduced by 0.2 (see Tab.4).

    Fig.5 Density values of fresh mortars

    2.3 Hardened mortar

    2.3.1 Setting time

    The setting time results of the hardened mortars are shown in Fig.6. It is evident that the setting time of the RAM (336 min) is lower than that of the REF (506 min), which is in agreement with the result in Ref.[11]. This behavior might be related to the fact that the high water-retention capacity (see Fig.4) allows the material to hold a large amount of free water during the mortar preparation[2]. As expected, its setting time of RAM+SSC increases by 225 min because the SH and CA in the SSC can retard the hydration of the cement particle[1314, 1617].

    Fig.6 Setting time results of hardened mortars

    2.3.2 Compressive strength

    Fig.7 depicts the compressive strengths and effective water-binder rates (w/beff) of the hardened mortars.w/beffvalue can be calculated as

    (1)

    wherem1,m2, andm3are the weights of total water, aggregate and binding materials; andPis the water absorption rate of the aggregate after 24 h.

    Fig.7 Compressive strengths and effective water-binder rates of hardened mortars

    It is evident that the compressive strength of the RAM is higher than that of the REF, which is in agreement with the results of some previous studies[3435]. This phenomenon can be explained as follows: 1) The amount of water in the RFA is higher than that in the NFA because the RFA shows a higher water absorption rate compared with the NFA (see Fig.2), and the water provides an internal curing environment[2, 34]. This facilitates the dense combination with the set cement interface, so that the intensity between the RFA and set cement is significantly increased; and 2) More micro powders are present in the RFA, and these powders serve as filler materials, which decreases the porosity of the mortar[35].

    In terms of the RAM+SSC, its compressive strength value is higher than that of the RAM by 9.1 MPa.This phenomenon can be explained as follows:1) The water retention rate of the RAM+SSC is higher than that of the RAM; therefore, much more water is present in the RAM+SSC offering an internal curing environment. 2) The incorporation of SH and SL in the SSC can not only disperse the micro powders in the mixtures and then help the powders more effectively fill into the pores of the cement paste, but also decreases the amount of flocculate structures generated by micro powders and then loosens much free water for cement hydration.

    3 Conclusions

    1) The consistency value of fresh recycled aggregate mortar (RAM) is lower than that of the reference mortar by 3 mm, whereas the values of consistency loss, water retention rate and density of the RAM are higher than those of the reference mortar by 21.1 mm, 5.3% and 50 kg/m3, respectively. After the admixture is added into the RAM, the consistency value increased by 4 mm, and the consistency loss and density values decreased by 21.1 mm and 70 kg/m3, respectively.

    2) The setting time of hardened RAM is lower than that of the reference mortar by 170 min, but the compressive strength value of the RAM is higher than that of the reference mortar by 2.7 MPa. After the admixture is added into the RAM, the setting time and compressive strength increase by 225 min and 9.1 MPa, respectively.

    3) Therefore, adding SSC into RAM is an effective and efficient way to expand its application, and future research should pay more attention to the effect of the admixture on the durability of RAM.

    最黄视频免费看| 欧美日本中文国产一区发布| 9191精品国产免费久久| 国产一区亚洲一区在线观看| 亚洲av欧美aⅴ国产| 高清视频免费观看一区二区| 97在线人人人人妻| 亚洲精品成人av观看孕妇| 少妇猛男粗大的猛烈进出视频| 夫妻午夜视频| 哪个播放器可以免费观看大片| 欧美xxⅹ黑人| 久久鲁丝午夜福利片| 精品一区二区三卡| 免费黄网站久久成人精品| 男人爽女人下面视频在线观看| 亚洲 欧美一区二区三区| 国产一区亚洲一区在线观看| 亚洲熟女精品中文字幕| 最近中文字幕2019免费版| 熟女av电影| 极品少妇高潮喷水抽搐| 天堂俺去俺来也www色官网| 一本大道久久a久久精品| 成人18禁高潮啪啪吃奶动态图| 黑人高潮一二区| 最黄视频免费看| 男女啪啪激烈高潮av片| 少妇高潮的动态图| 精品一品国产午夜福利视频| 高清毛片免费看| 久久99热6这里只有精品| 热99国产精品久久久久久7| 免费观看性生交大片5| 国产国拍精品亚洲av在线观看| 少妇人妻 视频| 在线观看免费日韩欧美大片| 欧美日韩一区二区视频在线观看视频在线| 精品人妻熟女毛片av久久网站| 精品一品国产午夜福利视频| 精品亚洲成a人片在线观看| 在线观看www视频免费| 精品一区二区三区视频在线| 91精品伊人久久大香线蕉| 成人影院久久| 日韩三级伦理在线观看| 日韩中字成人| 蜜臀久久99精品久久宅男| 亚洲国产精品一区二区三区在线| 日韩,欧美,国产一区二区三区| 久久婷婷青草| 又黄又粗又硬又大视频| 精品久久国产蜜桃| 日韩一本色道免费dvd| 一级毛片黄色毛片免费观看视频| 久久久久久久久久成人| 久久婷婷青草| 又黄又爽又刺激的免费视频.| 精品99又大又爽又粗少妇毛片| 一级黄片播放器| 国产精品熟女久久久久浪| av卡一久久| 午夜免费鲁丝| 伦理电影免费视频| 亚洲av福利一区| 亚洲av男天堂| 最新中文字幕久久久久| 成人手机av| a级毛片在线看网站| av免费观看日本| 国产亚洲最大av| 男女边吃奶边做爰视频| 亚洲情色 制服丝袜| 国产高清国产精品国产三级| 搡老乐熟女国产| 美女xxoo啪啪120秒动态图| 两个人看的免费小视频| 亚洲成人手机| 美女国产高潮福利片在线看| 中文字幕免费在线视频6| 久久av网站| a级毛片在线看网站| 久久久久视频综合| 91在线精品国自产拍蜜月| 午夜福利视频精品| 亚洲精品国产色婷婷电影| 黄色毛片三级朝国网站| 好男人视频免费观看在线| 亚洲高清免费不卡视频| 啦啦啦在线观看免费高清www| 精品国产一区二区久久| 美女大奶头黄色视频| 欧美精品一区二区免费开放| 男的添女的下面高潮视频| 春色校园在线视频观看| 久久久国产一区二区| 久久99精品国语久久久| 新久久久久国产一级毛片| 免费观看无遮挡的男女| 国产亚洲欧美精品永久| 观看美女的网站| 又黄又粗又硬又大视频| 亚洲精品456在线播放app| 女的被弄到高潮叫床怎么办| 99热6这里只有精品| 五月天丁香电影| 国产亚洲精品久久久com| 嫩草影院入口| 一区二区三区四区激情视频| 成人18禁高潮啪啪吃奶动态图| 久久ye,这里只有精品| 午夜久久久在线观看| 亚洲av福利一区| 久久久国产一区二区| 久久久国产一区二区| 啦啦啦在线观看免费高清www| 中文精品一卡2卡3卡4更新| 我的女老师完整版在线观看| 久久这里只有精品19| 久久这里只有精品19| 视频区图区小说| 又大又黄又爽视频免费| 亚洲欧洲国产日韩| 久久精品久久久久久噜噜老黄| 99香蕉大伊视频| 国产精品一国产av| 亚洲熟女精品中文字幕| 哪个播放器可以免费观看大片| 国产欧美日韩综合在线一区二区| 欧美日韩精品成人综合77777| 两性夫妻黄色片 | 18禁裸乳无遮挡动漫免费视频| 免费久久久久久久精品成人欧美视频 | 精品午夜福利在线看| 看免费av毛片| 18禁在线无遮挡免费观看视频| 黄网站色视频无遮挡免费观看| 黑人巨大精品欧美一区二区蜜桃 | 91久久精品国产一区二区三区| 少妇的丰满在线观看| 成人国产av品久久久| 精品99又大又爽又粗少妇毛片| 婷婷色综合www| 精品少妇内射三级| 欧美3d第一页| av在线老鸭窝| av有码第一页| 亚洲av国产av综合av卡| 亚洲欧洲日产国产| 曰老女人黄片| 亚洲欧美色中文字幕在线| 精品国产露脸久久av麻豆| 精品国产乱码久久久久久小说| 久久ye,这里只有精品| 九色亚洲精品在线播放| 美女中出高潮动态图| 国产有黄有色有爽视频| 美女主播在线视频| 成人国产麻豆网| 国产亚洲最大av| 亚洲五月色婷婷综合| 赤兔流量卡办理| 永久网站在线| 久久久久久久久久久久大奶| 91午夜精品亚洲一区二区三区| 色94色欧美一区二区| 日韩熟女老妇一区二区性免费视频| 全区人妻精品视频| 永久网站在线| 18在线观看网站| av播播在线观看一区| 又大又黄又爽视频免费| 日韩大片免费观看网站| 国产激情久久老熟女| 在线观看国产h片| 人人妻人人添人人爽欧美一区卜| 亚洲,一卡二卡三卡| 国产在视频线精品| 国产成人aa在线观看| 久久99热6这里只有精品| 天天躁夜夜躁狠狠躁躁| 精品亚洲成a人片在线观看| 日韩精品免费视频一区二区三区 | 亚洲精品日韩在线中文字幕| 丝袜人妻中文字幕| 成人黄色视频免费在线看| 色婷婷av一区二区三区视频| 日韩大片免费观看网站| 男女国产视频网站| 亚洲精品久久午夜乱码| 国语对白做爰xxxⅹ性视频网站| 在现免费观看毛片| 黄网站色视频无遮挡免费观看| 久久人人爽av亚洲精品天堂| 91精品伊人久久大香线蕉| 中文乱码字字幕精品一区二区三区| 一边摸一边做爽爽视频免费| 久久久久久久国产电影| 国产又爽黄色视频| 国产成人午夜福利电影在线观看| 亚洲中文av在线| 国产成人精品无人区| 两性夫妻黄色片 | 精品少妇内射三级| 久久久久精品性色| 欧美丝袜亚洲另类| av在线app专区| 久热这里只有精品99| 国产探花极品一区二区| 你懂的网址亚洲精品在线观看| 美女大奶头黄色视频| 中文字幕人妻熟女乱码| 国产成人精品婷婷| 亚洲综合精品二区| 国内精品宾馆在线| 欧美xxxx性猛交bbbb| 成年av动漫网址| 国产xxxxx性猛交| 国产探花极品一区二区| 狠狠婷婷综合久久久久久88av| 丝袜人妻中文字幕| 国产国语露脸激情在线看| 99热网站在线观看| 国产视频首页在线观看| av天堂久久9| 久久精品国产综合久久久 | 插逼视频在线观看| 欧美精品人与动牲交sv欧美| 满18在线观看网站| 日韩中字成人| 国产激情久久老熟女| 亚洲精品av麻豆狂野| 亚洲综合精品二区| 欧美丝袜亚洲另类| 一级爰片在线观看| 久久av网站| 99国产综合亚洲精品| 国产精品偷伦视频观看了| 最近最新中文字幕免费大全7| 丰满迷人的少妇在线观看| 亚洲欧美清纯卡通| 韩国高清视频一区二区三区| 日本91视频免费播放| 欧美人与善性xxx| av.在线天堂| 五月伊人婷婷丁香| 久久久久视频综合| 久久97久久精品| 99热6这里只有精品| 午夜福利视频在线观看免费| 久久久久久久久久成人| 高清黄色对白视频在线免费看| 中文字幕人妻熟女乱码| 国产亚洲午夜精品一区二区久久| 毛片一级片免费看久久久久| 狂野欧美激情性bbbbbb| av线在线观看网站| 美女中出高潮动态图| 九草在线视频观看| 午夜福利网站1000一区二区三区| 永久网站在线| 亚洲精品久久久久久婷婷小说| 国产一区亚洲一区在线观看| 91在线精品国自产拍蜜月| 国产精品99久久99久久久不卡 | 亚洲美女黄色视频免费看| 777米奇影视久久| 日本av手机在线免费观看| 国产成人aa在线观看| 国产色爽女视频免费观看| 精品人妻熟女毛片av久久网站| 伊人亚洲综合成人网| 纵有疾风起免费观看全集完整版| 美女主播在线视频| 免费久久久久久久精品成人欧美视频 | 99久久中文字幕三级久久日本| 亚洲精品久久午夜乱码| 最近2019中文字幕mv第一页| 在线观看人妻少妇| 在线天堂中文资源库| 1024视频免费在线观看| 亚洲综合色网址| 午夜老司机福利剧场| 成人二区视频| 人妻 亚洲 视频| 亚洲成色77777| 欧美人与性动交α欧美精品济南到 | 国产在线一区二区三区精| 免费看光身美女| 日产精品乱码卡一卡2卡三| 亚洲伊人久久精品综合| 视频中文字幕在线观看| 免费黄色在线免费观看| 亚洲欧美色中文字幕在线| 国产精品一区二区在线观看99| 国产熟女午夜一区二区三区| 国产日韩一区二区三区精品不卡| 黄色视频在线播放观看不卡| 男女午夜视频在线观看 | 黄色怎么调成土黄色| a级毛片黄视频| 国产成人精品一,二区| 亚洲成人av在线免费| 婷婷色综合大香蕉| 搡老乐熟女国产| 狂野欧美激情性bbbbbb| 男女无遮挡免费网站观看| 人人妻人人澡人人爽人人夜夜| 如日韩欧美国产精品一区二区三区| 欧美精品一区二区免费开放| 国产 一区精品| 视频区图区小说| 我的女老师完整版在线观看| 黑人高潮一二区| 国产国拍精品亚洲av在线观看| 日本vs欧美在线观看视频| 成人国产av品久久久| 国产亚洲精品久久久com| 亚洲精品第二区| 国产成人a∨麻豆精品| 黄色毛片三级朝国网站| 国产1区2区3区精品| 亚洲精品久久午夜乱码| 国产精品女同一区二区软件| 丰满乱子伦码专区| 日本vs欧美在线观看视频| 人人妻人人添人人爽欧美一区卜| 亚洲色图综合在线观看| 在线观看国产h片| 国产亚洲最大av| 性色avwww在线观看| 纯流量卡能插随身wifi吗| 少妇的逼水好多| 人体艺术视频欧美日本| 精品人妻偷拍中文字幕| 97在线视频观看| 国产亚洲精品第一综合不卡 | 女性被躁到高潮视频| 国产成人精品一,二区| 99精国产麻豆久久婷婷| 亚洲综合色惰| 日日摸夜夜添夜夜爱| 日韩制服丝袜自拍偷拍| 精品酒店卫生间| 日韩中文字幕视频在线看片| 一本久久精品| 精品亚洲成a人片在线观看| 欧美最新免费一区二区三区| 免费播放大片免费观看视频在线观看| 国内精品宾馆在线| 国产一区二区三区综合在线观看 | 午夜激情av网站| 国产成人精品一,二区| 久久国产精品大桥未久av| 亚洲天堂av无毛| 免费大片18禁| 水蜜桃什么品种好| 又黄又爽又刺激的免费视频.| 亚洲av电影在线进入| 少妇被粗大猛烈的视频| 精品第一国产精品| 欧美成人午夜精品| 免费人成在线观看视频色| 天堂中文最新版在线下载| 亚洲av男天堂| 精品国产国语对白av| 中文字幕制服av| 亚洲国产日韩一区二区| 黄片无遮挡物在线观看| 久久影院123| 国产日韩欧美视频二区| 免费在线观看完整版高清| 国产亚洲欧美精品永久| 最近2019中文字幕mv第一页| 成人综合一区亚洲| 天堂中文最新版在线下载| 日韩大片免费观看网站| 99九九在线精品视频| 亚洲伊人色综图| 国产在线免费精品| 中文字幕人妻熟女乱码| 久久99热这里只频精品6学生| 啦啦啦啦在线视频资源| 一本一本久久a久久精品综合妖精 国产伦在线观看视频一区 | 日本免费在线观看一区| 亚洲美女视频黄频| 久久国产亚洲av麻豆专区| 女的被弄到高潮叫床怎么办| 午夜福利,免费看| 91国产中文字幕| 国产精品一区二区在线不卡| 少妇 在线观看| 欧美变态另类bdsm刘玥| 男女下面插进去视频免费观看 | 亚洲国产精品国产精品| 国产精品.久久久| 亚洲国产av新网站| 99九九在线精品视频| videos熟女内射| 插逼视频在线观看| 日韩中文字幕视频在线看片| 老司机亚洲免费影院| 久久精品熟女亚洲av麻豆精品| 国产成人精品无人区| 九色成人免费人妻av| 97人妻天天添夜夜摸| 免费人成在线观看视频色| 母亲3免费完整高清在线观看 | 日本-黄色视频高清免费观看| 国产欧美另类精品又又久久亚洲欧美| 亚洲,一卡二卡三卡| 欧美成人午夜免费资源| 亚洲av电影在线进入| 日韩大片免费观看网站| 老司机亚洲免费影院| 国产欧美亚洲国产| 国产亚洲午夜精品一区二区久久| 免费不卡的大黄色大毛片视频在线观看| 国产免费视频播放在线视频| 乱人伦中国视频| 成人亚洲欧美一区二区av| 一本—道久久a久久精品蜜桃钙片| 日韩成人av中文字幕在线观看| 18禁动态无遮挡网站| 人人妻人人澡人人爽人人夜夜| av免费在线看不卡| 在线 av 中文字幕| 午夜福利乱码中文字幕| 免费高清在线观看视频在线观看| 综合色丁香网| 黑人巨大精品欧美一区二区蜜桃 | 最近中文字幕高清免费大全6| 中文字幕免费在线视频6| 色网站视频免费| 久久人人爽人人爽人人片va| 最近2019中文字幕mv第一页| 亚洲人成网站在线观看播放| 国产精品国产三级专区第一集| 人人澡人人妻人| 亚洲国产成人一精品久久久| 欧美日韩综合久久久久久| 亚洲综合色网址| a级毛色黄片| 女人久久www免费人成看片| 99久久中文字幕三级久久日本| 在线 av 中文字幕| 久久亚洲国产成人精品v| 免费在线观看黄色视频的| 国产在视频线精品| 久热这里只有精品99| 国产极品天堂在线| 日日摸夜夜添夜夜爱| 91成人精品电影| 一级片免费观看大全| 搡老乐熟女国产| 成年av动漫网址| 高清黄色对白视频在线免费看| 亚洲国产精品一区三区| 久久久久久人妻| 天堂中文最新版在线下载| 久久ye,这里只有精品| 国产欧美日韩一区二区三区在线| 国产有黄有色有爽视频| 黑人猛操日本美女一级片| 啦啦啦啦在线视频资源| 女人久久www免费人成看片| 五月玫瑰六月丁香| 欧美日韩一区二区视频在线观看视频在线| 日韩中文字幕视频在线看片| 麻豆乱淫一区二区| 国产免费现黄频在线看| 亚洲av电影在线观看一区二区三区| 久久久欧美国产精品| 精品久久蜜臀av无| 精品亚洲成国产av| 国产黄色免费在线视频| 精品少妇内射三级| 久久精品aⅴ一区二区三区四区 | 日本欧美视频一区| 丝袜人妻中文字幕| 美女福利国产在线| 久热这里只有精品99| 国产欧美日韩综合在线一区二区| 在现免费观看毛片| 不卡视频在线观看欧美| 成人国产av品久久久| 日本爱情动作片www.在线观看| 久久人人97超碰香蕉20202| 99re6热这里在线精品视频| 日本午夜av视频| 热99国产精品久久久久久7| 精品少妇黑人巨大在线播放| 各种免费的搞黄视频| 国产乱来视频区| 在线天堂最新版资源| 国产一区亚洲一区在线观看| 妹子高潮喷水视频| 你懂的网址亚洲精品在线观看| 免费大片18禁| 欧美97在线视频| 国产极品粉嫩免费观看在线| 老司机影院成人| 国产精品.久久久| 一级毛片电影观看| av黄色大香蕉| 国产国语露脸激情在线看| 亚洲图色成人| 免费人妻精品一区二区三区视频| 最后的刺客免费高清国语| 免费在线观看完整版高清| 国产欧美另类精品又又久久亚洲欧美| 成人二区视频| 男的添女的下面高潮视频| 久久久久久久精品精品| 在线观看免费视频网站a站| 亚洲国产av新网站| 麻豆精品久久久久久蜜桃| 亚洲第一区二区三区不卡| 国产精品女同一区二区软件| 亚洲第一av免费看| 少妇人妻 视频| 激情视频va一区二区三区| 最近最新中文字幕大全免费视频 | 搡老乐熟女国产| 国产一区有黄有色的免费视频| 69精品国产乱码久久久| 国产 精品1| 精品国产露脸久久av麻豆| 看免费av毛片| 免费少妇av软件| 少妇人妻 视频| 妹子高潮喷水视频| 22中文网久久字幕| av国产久精品久网站免费入址| 免费看不卡的av| 又粗又硬又长又爽又黄的视频| 中文字幕亚洲精品专区| 国产黄色免费在线视频| 免费日韩欧美在线观看| av有码第一页| 视频中文字幕在线观看| 80岁老熟妇乱子伦牲交| 亚洲av.av天堂| 国产欧美日韩一区二区三区在线| 少妇被粗大猛烈的视频| 亚洲精品一区蜜桃| 美女主播在线视频| 在线观看美女被高潮喷水网站| 日韩一区二区视频免费看| 午夜免费鲁丝| 人妻 亚洲 视频| 精品午夜福利在线看| 久久精品国产鲁丝片午夜精品| 成人手机av| 51国产日韩欧美| 国产有黄有色有爽视频| 啦啦啦中文免费视频观看日本| 另类亚洲欧美激情| 中文字幕人妻熟女乱码| 欧美日韩国产mv在线观看视频| 亚洲国产毛片av蜜桃av| 男女啪啪激烈高潮av片| xxxhd国产人妻xxx| 99久久人妻综合| 交换朋友夫妻互换小说| 国产精品女同一区二区软件| 亚洲精品中文字幕在线视频| 国产精品一区二区在线观看99| 大码成人一级视频| 亚洲欧美中文字幕日韩二区| 精品一品国产午夜福利视频| 国产精品国产三级专区第一集| 国产av国产精品国产| 精品亚洲成国产av| 男女边摸边吃奶| 日韩 亚洲 欧美在线| 午夜福利网站1000一区二区三区| 国产免费视频播放在线视频| 一个人免费看片子| 亚洲精品日韩在线中文字幕| 一区二区三区四区激情视频| 免费黄频网站在线观看国产| 亚洲av中文av极速乱| 人人妻人人添人人爽欧美一区卜| 中文字幕免费在线视频6| 欧美xxⅹ黑人| 国产成人av激情在线播放| 亚洲精品一区蜜桃| 男女啪啪激烈高潮av片| 久久国产亚洲av麻豆专区| 欧美精品高潮呻吟av久久| 欧美日韩成人在线一区二区| 精品国产国语对白av| 午夜免费男女啪啪视频观看| 亚洲一级一片aⅴ在线观看| 伊人久久国产一区二区| 亚洲欧洲国产日韩| 亚洲国产欧美日韩在线播放| 成人国产av品久久久| 国产熟女午夜一区二区三区| 欧美精品高潮呻吟av久久| 亚洲精品国产色婷婷电影| 色94色欧美一区二区| 97人妻天天添夜夜摸| 五月伊人婷婷丁香| 少妇精品久久久久久久| 97在线视频观看| www.av在线官网国产| 国产精品熟女久久久久浪| 久久99蜜桃精品久久| 涩涩av久久男人的天堂| 国产精品欧美亚洲77777| 女人久久www免费人成看片| 人妻少妇偷人精品九色| 国产极品粉嫩免费观看在线|