    Porous Bioactive Ceramic Derived from Polyurethane Foams

    2020-09-15 11:46:22ZHANGYuanyuanLUOMinhuaXIAOZhuohaoZHUQingxiaLIUSaliCHENHuilingGUORulian
    陶瓷學(xué)報(bào) 2020年4期

    ZHANG Yuanyuan , LUO Minhua , XIAO Zhuohao , ZHU Qingxia , LIU Sali ,CHEN Huiling , GUO Rulian

    (1. Jingdezhen Ceramic Institute, Jingdezhen 333403, Jiangxi, China; 2.Tiangong University, Tianjin 300380, Tianjin, China)

    Abstract: Bioceramic matrix powders were synthesized by using a sol-gel method, while water based slurries were prepared by adding lab-made flux, polyvinyl alcohol (PVA), carboxyethyl cellulose and n-butanol. Polyurethane foams after hydrolysis and surface modification were impregnated in the slurries and the excess slurries were removed. The samples were then dried and sintered at high temperatures to obtain bioactive ceramics. The effects of PVA content, self-prepared flux content and sintering temperature on porosity and flexural strength of the samples were systematically studied. The pore samples were analyzed by using scanning electron microscope (SEM), their biological activity was examined by using simulated body fluid (SBF), and the phase changes before and after mineralization were characterized by using X-ray diffraction (XRD). It was found that porous bioactive ceramics with promising comprehensive properties can be obtained by adding 30 wt.% flux and 0.76 wt.% PVA, with a sintering temperature of 1000 °C. The porosity of the optimized sample is 81.35% and the flexural strength is 2.75 MPa.

    Key words: porous bioceramic; organic foam impregnation method; porosity; biological activity; flexural strength

    1 Introduction

    Bioactive ceramics prepared by using sol-gel methods are of special compositions, high bioactivity and biocompatibility, thus having wide applications in bone tissue reconstruction[1]. Since biological scaffolds made of bioactive ceramics have large porosities with interconnected pores, the smaller pores are responsible for transport of nutrition and discharge of wastes, while the larger pores provide channels and space for the growth of osteoblasts,when they are implanted into human bodies, thus ensuring the rapid growth of blood vessels and tissue cells and promote the development of bone tissues[2]. There are various ways to fabricate bioactive scaffolds. The use of pore agents is a simple method to obtain bioactive scaffolds, but the pore sizes are not uniform, so that it is difficult to form 3D interconnected channels and they have relatively low mechanical strengths[3,4]. Foaming methods have disadvantages of uncontrollable pore structures, poor pore size distribution and low pore connectivity[5-7].Freeze drying methods result in directionally controllable pores, but the pore connectivity and strength are relatively low, while the pore sizes are small[8,9]. 3D printing technologies require slurries with high contents of liquid phases, which cause deformation of green bodies due to the effect of gravitation. Meanwhile, the samples are prone to crack and deform during binder burning and sintering[10,11]. In comparison, foam conversion process is of various advantages, such as simple operation, cost-effectiveness, high porosity and high pore connectivity, thus attracting strong attentions all around the world[2,12-14]. However, there are still rooms for further improvement. For instance, as the porosity is higher than 80%, compressive strengths of the scaffolds will be only in the range of 0.3-0.4 MPa[15-17]. Baino et al.[18]introduced organic components to increase the strength of scaffolds, but the highest compressive strength as still only 1.0 MPa, below the requirement of bone regeneration.Although the mechanical strength could be increased by increasing the sintering temperature,this process would also reduce the bioactivity of the scaffolds. Therefore, it is still a challenge to fabricate bioactive ceramic scaffolds with sufficiently high mechanical strengths, while not compromising their porosity and bioactivity[19].

    In this study, a sol-gel process was employed to prepare bioactive ceramic scaffold through foam conversion, which exhibited sufficiently high porosity, strong mechanical properties and relatively high bioactivity, by adjusting the contents of PVA and lab-made flux.

    2 Experimental

    2.1 Materials

    In the sol-gel process, chemicals and reagents include anhydrous ethanol (C2H6O, AR), tetraethyl oxysilicate (C8H20O4Si, AR), triethyl phosphate(C6H15O4P, CP), citric acid (C6H15O4P, CP), calcium nitrate tetrahydrate (Ca(NO3)·4H2O, AR) and polyethylene glycol 400 (H(OCH2CH2)nOH, CP).Chemicals for bioactive ceramics include polyvinyl alcohol ([-CH2CHOH-]n/(C2H4O)n, AR), carboxyethyl cellulose (C2H6O2·X, CP) and n-butanol (C4H10O,AR). Properties of the polyurethane foams used in the experiment are listed in Tab. 1. Sodium hydroxide (NaOH, AR), tween 80 (C24H44O6, CP)were used to pretreat the polyurethane foams.

    The chemical reagents used to prepare SBF include sodium chloride (NaCl, AR), sodium bicarbonate (NaHCO3, AR), potassium chloride(KCl, AR), dipotassium hydrogen phosphate (K2HPO4·3H2O, AR), magnesium chloride hexahydrate(MgCl2·6H2O, AR), hydrogen chloride (HCl, AR),calcium chloride (CaCl2, AR), sodium sulfate(Na2SO4, AR), and trihydroxymethylaminomethane((CH2OH)3CNH2, AR).

    2.2 Sol-gel process to prepare bioactive ceramics

    320 mL deionized water and 50 mL anhydrous ethanol were mixed at 30 °C, while 1.5 g citric acid was dissolved into the mixture with the aid of stirring. 40 mL TEOS and 3.5 mL triethyl phosphate were mixed, according to the composition of the bioceramics, i.e., 60% SiO2, 4% P2O5and 36% CaO. In the mixture, 31 g calcium nitrate tetrahydrate was slowly added. Then, 2 mL polyethylene glycol 400 was dropped to foam sol.The sol was sealed and kept in a water bath then aged 24 h into gel, dried at 48 h for 70 °C. The dried gel was calcined at 600 °C for 2 h with a heating rate of 5 °C /min in a muffle furnace, and thenbioactive ceramics were obtained.

    2.3 Selection and pretreatment of polyurethane foams

    Organic precursor is critical to the fabrication of porous scaffolds. The selected polyurethane foam is of 2D interconnected porous structure, strong resilience, wide volatilization temperature range(200-600 °C), high temperature volatilization temperature (380 °C) and low softening temperature(250 °C)[20]. As a result, it is softened gradually during the thermal decomposition process, thus preventing the samples from deformation during the volatilization of the organic components. In order to avoid the occurrence of plugging in the porous scaffolds due to excessive inter-membranesin the polyurethane foam, also owing to reduced slurry adhesion on the smooth surface of the polyurethane foam, it should be pretreated with alkaline solutions[21]. In this study, water was used as the solvent; the wettability of the polyurethane foam by the slurry after the alkaline treatment was still insufficient, thus leading to too thin and too thick coatings of slurry at the cross section and corner line,respectively[22]. This occurrence would result in serious cracking of the scaffolds, thus deteriorating their mechanical strengths. Surfactant is a hydrophilic substance, which can be used to improve the hydrophilicity of polyurethane foam and hence reduce the surface/interface tension[23]. As a consequence,water-based slurries can be firmly adsorbed onto the polyurethane foam, so as to improve the wettability between polyurethane foam and slurry.

    To measure flexural strengths, the polyurethane foam was cut into strips with sizes of 40 mm × 15 mm × 15 mm. The strip samples were immersed in 0.6 mol/L NaOH solution for 2 h and then washed with distilled water to neutral pH, followed by drying. The dried samples were kept in tween 80 solution for 2 h and dried again.

    2.4 Preparation of porous bioactive ceramics

    52.5 g bioactive ceramic powder and lab-made flux were ball milled separately and sieved through 250 mesh. The milled samples were mixed with 100 ml distilled water, followed by adding 0.5 g carboxyethyl cellulose and stirring for 30 min. Then,PVA solution (PVA was dissolved in 100 mL distilled water at 90 °C with constant stirring) and stirred for 1 h, followed by dropping 1 mL n-butanol and stirring for 24 h to foam slurry. Pretreated polyurethane foam strips were entirely soaked in the slurry. The soaked samples were taken out and squeezed to remove the excessive slurry, followed by drying at 30 °C for 12 h and 60 °C for 12 h at a heating rate of 0.5 °C /min. The dried samples were sintered at 1000 °C, 1100 °C and 1200 °C for 2 h, at heating rate 2 °C /min. The contents of lab-made flux and PVA are listed in Tab. 2.

    Tab.1 Properties of the polyurethane foam

    2.5 Preparation of SBF and bioactivity characterization

    Bioactive materials are defined as those that have chemical bonding with living bone tissues and soft tissues[24,25]. The chemical bonding is formed through the deposition of hydroxycarbonate apatite(HCA) at interfaces between the biomaterials and HCA, because HCA is similar to the basic mineral hydroxyapatite (HA) in structure and properties. In addition, HCA has relatively high solubility in body flow and hence degradable in human body, thus have high bioactivity[26]. Moreover, biological proteins can be adsorbed onto HCA to form bone cells, thus facilitating bone guidance and ensuring the chemical bonding between the bioactive materials and the bones[25]. The binding capability of biomaterials to host bones is closely related to the presence of the HCA layer formed on surface of the biomaterials. Therefore, the biological activity of biomaterials can be preliminarily evaluated by monitoring the growth of HCA on the surface of biomaterials by immersing them in SBF solution[27].

    Tab.2 Slurry formula in terms of the contents of lab-made flux and PVA

    Lab-use SBF contained no cell and protein, with a pH value of 7.4. The contents of ions are listed in Tab. 3, which are similar to those of human blood plasma. To prepare the SBF[28], 8.035 g NaCl, 0.355 g NaHCO3, 0.255 g KCl, 0.231 g K2HPO4·3H2O,0.311 g MgCl2·6H2O, 0.292 g CaCl2and 0.072 g Na2SO4were successively put in 900 mL distilled water, with constant stirring at 37 °C. The solution was adjusted to pH value of 2.0 ± 1.0 with 1 mol/L HCl solution, followed by adding 6.118 g(CH2OH)3CNH2with stirring. Finally, pH value was adjusted to 7.4 and the solution was transferred to a 1000 mL flask.

    Tab.3 Ion concentration in human plasma and the SBF solution (mmol /L)

    The porous samples were immersed in SBF solution in polyethylene bottles, according to the ratio of sample mass to SBF solution volume of 1 mg/mL. The bottles were then sealed and statically kept at 37 °C, while the SBF solution was replaced every two days. After reaction for different times (2,5, 10 days), the samples were taken out and washed with acetone for one time and deionized water for 3-4 times, followed by drying at 40 °C and sterilization at 120 °C.

    2.6 Characterization

    Porosity of the samples was measured by using a volume-mas tester. Phase composition was examined by using XRD (D8 Advance, Bruker AXS,Germany), at voltage of 40 kV and current of 40 mA,with scanning step of 0.2 °. Pore structure and mineralized morphology were characterized by using field emission scanning electron microscopy(JSM-6700F, JEOL). Flexural strength was tested by using a pressure tester (FC056R), with a loading rate of 0.5 mm/min. Viscosity of the slurry was measured by using a digital rotational viscometer(LVDV-1), over 10-600 Pa·s. Crystal size was estimated by using the Scherrer formula[29]:

    whereDis crystal size,k= 0.89,λis the wavelength of X-ray,βis full width at half maximum(FWHM) of diffraction peaks andθis the diffraction angle.

    3 Results and Discussion

    3.1 Slurry viscosity

    Fig. 1 shows viscosities of the samples with different contents of PVA (0 wt.%, 0.57 wt.%, 0.76 wt.%, 0.95 wt.%) and flux agent (0 wt.%, 10 wt.%,20 wt.%, 30 wt.%). Obviously, the effect of flux agent on viscosity of the slurries was relatively weak. The viscosity was gradually increased with increasing content of PVA, with the maximum value to be 5.3 Pa·s (with flux of 30 wt.%). The viscosities were increased by 32-37% and 22-25%, as the contents of PVA were increased from 0.57 wt.% to 0.95 wt.% and 0.76 wt.% to 0.95 wt.%, respectively.This is because PVA promoted the connection of the ceramic particles through either chemical or molecular bonding, thus reducing the flowability and hence increasing the viscosity of the slurries.

    Fig.1 Viscosities of the slurries with different contents of flux as a function of the content of PVA

    3.2 Porosity

    Fig. 2 shows porosities of the porous samples.For the samples with same content of flus after sintering at same temperature, the viscosity followed the same variation trend, which was increased first and then decreased. As the PVA content was 0.76 wt.%, porosity of the samples was maximized.Initially, with increasing content of PVA, the viscosity of the slurries was increased, so that cohesion of the slurry onto the polyurethane foam was enhanced. As a result, the slurries would not flow into the pores, thus leading to samples with high porosity. However, if the viscosity was too high,the excessive slurries could not be completely removed from the foam, so that the porosity was decreased. With same contents of flux and PVA, the porosity was significantly reduced with increasing sintering temperature, simply because sintering resulted in shrink of the samples.

    With fixed content of PVA and sintering temperature, the effect of flux on porosity was not very significant. As the content of PVA was 0.57 wt.% and the sintering temperature was 1200 °C, the highest porosity was 74.19% and the lowest one was 72.24%, with a difference to be only 2.6%. This is simply because the flux had almost no effect on the viscosity of the slurries. Also, the ceramic bodies had been nearly fully densified after sintering at temperatures of ≥1000 °C. At the sintering temperatures, the molten flux would fill the pores.Therefore, porosity of the samples was mainly determined by the porosity of the polyurethane foams.

    Fig.2 Porosities of the samples with different contents of PVA and flux after sintering at different temperatures

    3.3 Flexural strengths

    Fig. 3 shows flexural strengths of the porous samples. With given content of flux and sintering temperature, the variation trends in flexural strength were similar over the PVA content range of 0-0.95 wt.%. The increase in flexural strength was quite fast initially and the slowed down. However, without the use of PVA (0 wt.%), the sample had obviously very low strength. This is because the PVA absent slurry had too low viscosity, so that the content adsorbed by the foam was very low. As a consequence, the ceramic layers were too thin and hence the flexural strength was low. With the addition of PVA, the quantity of the slurry adsorbed by the foam was increased, so that the thickness of the ceramic layer was increased. Accordingly, the flexural strength was increased. However, the magnitude of increase in flexural strength as a function of PVA content was almost neglectable. For instance, as the content of PVA was increased from 0.57 wt.% to 0.95 wt.%, the flexural strength was increased by only ≤ 5%. With fixed contents of flux and PVA, the flexural strength was greatly increased with increasing sintering temperature, simply because of the increased density of the samples.

    For the samples with same content of PVA after sintering at same temperature, their flexural strength was rapidly increased first and slowly went up later,as the content of flux was increased from 0 wt.% to 30 wt.%. Without the addition of flux, the sample had a very low flexural strength. This is because the ceramic powder could not be fully densified during the sintering process, without the presence of liquid phase (flux). The maximum strength was only 0.73 MPa. The liquid phase was filled in the pores in between the ceramic particles, promoting the densification of the samples. The magnitude of the increase in flexural strength was about 10%.

    It is accepted that the minimum compressive strength required for cancellous bone is 2 MPa[30],because flexural strength of ceramics is usually lower than their compressive strength. As seen in Fig. 3, except the ones without the addition of PVA and flux, all the samples meet the minimum strength requirement. Close inspection of Fig. 2 revealed that the four samples with 0.76 wt.% PVA after sintering at 1000 °C exhibited higher porosities (data in the dotted line box) than other ones. Taking into account the porosity and flexural strength, the sample with the highest porosity of 82.34% had a flexural strength of 2.34 MPa, while the sample with highest flexural strength of 2.75 MPa possessed a porosity of 81.35%. In other words, the flexural strength was increased by 17.5%, while the porosity was only reduced by 1.2%. In this case, the content of flux was 30 wt.%. Because low sintering temperature is beneficial to bioactivity[31], the sample with 0.76 wt.% PVA and 30 wt.% flux after sintering at 1000 °C (12# in Tab. 2) was used for the characterization of pore structure and mineralization.

    Fig.3 Flexural strengths of the samples with different contents of PVA and flux after sintering at different temperatures

    3.4 Pore structure and size distribution

    Fig. 4 shows SEM images of the sample 12#. As illustrated in Fig. 4(a), the sample contained a large number of pores with sizes at millimeter scale, which were attributed to the porous structure of the polyurethane foam. The pores were entirely interconnected, with pore sized to be in the range of 100-700 μm at the connecting paths. The sizes of pores suitable for the growth of non-mineral bone tissues, bone tissues, new bone and blood vessels are 40-100 μm, 150 μm, 200-400 μm and ≥500 μm,respectively[32,33]. Meanwhile, connectivity of the scaffold structure is also of crucial effect on the growth of tissues. A high connectivity would ensure the space for tissue growth, boost microcirculation of tissue fluid, supply nutrition for the new bones inside the porous scaffold and promote the integration and growth of fibrous tissue and new bones[34].Ultimately, the porous scaffolds should allow the growth of bone tissues and blood vessels.

    As shown in Fig. 4(b), the inside walls of the pores are also highly porous. The large pores had sizes at micrometer scale, while the small ones were at nanometer scale, as observed in Fig. 4(c) and (d),respectively. Such porous structures would enlarge the specific surface area of the scaffolds, thus enhancing the absorption of osteogenic proteins,ion-exchange, dissolution-precipitation rate and hence formation of bone-like apatite. Consequently,fibrous tissues are formed, while nutrient transport and waste discharge are promoted[35]. In addition,the wall surface of the pore had a high roughness,leading to strong cell adhesion and enhanced growth of bone tissues[36]. The sample 12# had a porosity of 81.35%, with high connectivity. According to Fig. 4(a), pore size distributions were estimated, as listed in Tab. 4.

    Tab.4 Estimated pore size distributions of the sample 12#

    3.5 Mineralization

    Fig. 5 shows XRD patterns of the sample 12# before and after mineralization for 10 days.Before mineralization, the sample consisted mainly of HA, CaSiO3, SiO2and Ca2.86Mg0.14(PO4)2. After mineralization in SBF for 10 days, HCA was formed.CaSiO3has promising biocompatibility and is degradable in human body, while it is relatively weak in inducing the deposition of bone-like light apatite[37,38]. HA is a main component in human bones, which could promote the formation of collagen in bones and hence enhance the mineralization, thus having strong biocompatibility and bioactivity[30,40]. SiO2is highly biocompatible[41],while Ca2.86Mg0.14(PO4)2is able to promote the adhesion and increase the reproduction of bone cells, thus demonstrating high cell compatibility and bioactivity[42-44]. The HCA is high compatible with cells[45], further ensuring the growth of bone cells[25].Furthermore, HCA is highly biodegradable[26].

    Before mineralization, the average crystal size was 41.5 nm according to Eq. (1), while the maximum size was 65.3 nm. The nanocrystal phases precipitated during the sintering process could helped to increase the mechanical strength of the porous samples. The nanocrystals with different phases had different degradation rates, which was beneficial to the osteoinduction behavior of the scaffolds.

    Fig.4 SEM images of the sample 12#: (a, b) surface images, (c, d)zoom-in images of (b)

    Fig.5 XRD patterns of the samples 12# before and after mineralization

    Fig. 6 shows SEM images of the sample 12#after mineralization in the SBF solution for different time durations. As demonstrated in Fig. 6 (a), after mineralization for 2 days, surface of the sample became smooth, without the presence of any new phase. However, after mineralization for 5 days, the surface morphology was significantly changed.According to XRD patterns, HCA was generated on surface inside the pores of the scaffold. As revealed in the zoom-in image (Fig. 6 (c)) of selected area in Fig. 6(b), the HCA had a fluffy spherical morphology. After mineralization for 10 days, the spherical particles were transferred to leaf-shaped ones, covering the whole surface of the sample, as reflected in Fig. 6 (d). It is then suggested that the sample 12# was of pretty high bioactivity in SBF,thus make it suitable as plant for bone regeneration with strong binding[46,47].

    Fig.6 SEM images of the sample 12# after mineralization for different time durations:(a) 2 d, (b) 5 d, (c) partial enlarged picture of panel (b) and (d) 10 d

    4 Conclusions

    Bioactive porous ceramics, with porosity of 81.35% and flexural strength of 2.75 MPa, could be fabricated by using the foam conversion method from slurries, with the addition of 0.76 wt.% PVA and 30 wt.% lab-made flux, after sintering at 1000 °C. After mineralization for 10 days in SBF solution, a large number of plate-like HAC particles were formed, covering whole surface of the porous ceramic scaffold, showing promising bioactivity. The content of PVA had a significant effect on porosity of the bioactive ceramics, because an appropriate content of PVA resulted in slurries with suitable viscosity to ensure a strong adhesion onto the inside walls of the pores, while not compromising the connectivity of the samples. Due to the presence of millimeter sized interconnected pores in the polyurethane foams and the nanosized pores on the inner walls of the large pores, bone tissues and fibrous vessels could be well grown and the body fluid exchange could be promoted, thus enhancing bone growth.

    日日摸夜夜添夜夜爱| 亚洲熟女精品中文字幕| 在线看a的网站| 18+在线观看网站| 在线观看一区二区三区激情| 男人爽女人下面视频在线观看| 国产激情久久老熟女| 777米奇影视久久| 亚洲综合色惰| 亚洲伊人久久精品综合| 亚洲国产av新网站| 免费人妻精品一区二区三区视频| 一级毛片黄色毛片免费观看视频| 久久精品人人爽人人爽视色| 国产成人一区二区在线| 国产日韩欧美在线精品| 精品亚洲成a人片在线观看| 亚洲人成网站在线观看播放| 日本黄色日本黄色录像| 久久久国产精品麻豆| 国产欧美日韩一区二区三区在线| 亚洲精品国产色婷婷电影| 欧美日韩亚洲国产一区二区在线观看 | 欧美成人精品欧美一级黄| 韩国精品一区二区三区| 久久婷婷青草| 亚洲精品一二三| 国产高清不卡午夜福利| 国产成人精品久久二区二区91 | 免费在线观看完整版高清| 亚洲人成网站在线观看播放| 欧美变态另类bdsm刘玥| 亚洲久久久国产精品| 不卡视频在线观看欧美| 久久精品人人爽人人爽视色| 丝袜美腿诱惑在线| 天堂中文最新版在线下载| 一级片免费观看大全| av在线观看视频网站免费| 免费播放大片免费观看视频在线观看| 免费观看a级毛片全部| 日本wwww免费看| 波多野结衣一区麻豆| 午夜日本视频在线| 汤姆久久久久久久影院中文字幕| 免费观看在线日韩| 午夜精品国产一区二区电影| 最新中文字幕久久久久| 久久这里只有精品19| 午夜激情久久久久久久| 日韩三级伦理在线观看| av国产久精品久网站免费入址| 免费在线观看视频国产中文字幕亚洲 | 欧美日韩国产mv在线观看视频| 高清欧美精品videossex| 亚洲欧美清纯卡通| 又黄又粗又硬又大视频| 最近手机中文字幕大全| 在线亚洲精品国产二区图片欧美| 亚洲国产欧美日韩在线播放| 自线自在国产av| 亚洲少妇的诱惑av| 三上悠亚av全集在线观看| av线在线观看网站| 亚洲国产看品久久| 波野结衣二区三区在线| 中文字幕另类日韩欧美亚洲嫩草| 这个男人来自地球电影免费观看 | 肉色欧美久久久久久久蜜桃| 满18在线观看网站| 男女边摸边吃奶| 在线观看免费日韩欧美大片| av福利片在线| 美女国产视频在线观看| 日韩av免费高清视频| 国产精品一区二区在线不卡| 久久精品久久精品一区二区三区| 亚洲国产精品一区三区| 又黄又粗又硬又大视频| 欧美成人精品欧美一级黄| 一区二区日韩欧美中文字幕| 大陆偷拍与自拍| 交换朋友夫妻互换小说| 街头女战士在线观看网站| 在线 av 中文字幕| 晚上一个人看的免费电影| 韩国精品一区二区三区| 国产一级毛片在线| 精品亚洲乱码少妇综合久久| 一级爰片在线观看| 亚洲久久久国产精品| 久久精品人人爽人人爽视色| 久久久亚洲精品成人影院| 国产欧美日韩综合在线一区二区| 女人精品久久久久毛片| 久久久精品94久久精品| 亚洲av免费高清在线观看| 麻豆精品久久久久久蜜桃| 中文乱码字字幕精品一区二区三区| 久久精品久久久久久久性| 啦啦啦啦在线视频资源| 国产深夜福利视频在线观看| videos熟女内射| 久久久久久久久久人人人人人人| 国产精品成人在线| av福利片在线| 最近最新中文字幕免费大全7| 各种免费的搞黄视频| 成人18禁高潮啪啪吃奶动态图| 丝袜脚勾引网站| 丝袜在线中文字幕| 女人高潮潮喷娇喘18禁视频| 精品一区二区三卡| 在线天堂中文资源库| 中文字幕人妻丝袜制服| 欧美精品一区二区免费开放| 视频区图区小说| 秋霞伦理黄片| 国产伦理片在线播放av一区| 午夜福利在线观看免费完整高清在| 久久精品国产亚洲av高清一级| 国产精品偷伦视频观看了| 一边亲一边摸免费视频| 日韩欧美精品免费久久| 热re99久久精品国产66热6| 国产成人精品一,二区| 久久狼人影院| 久久这里有精品视频免费| 国产精品久久久av美女十八| 一区二区三区乱码不卡18| 亚洲情色 制服丝袜| 满18在线观看网站| 精品人妻偷拍中文字幕| 亚洲精品视频女| 日本色播在线视频| 黑人猛操日本美女一级片| 国产亚洲欧美精品永久| 老汉色av国产亚洲站长工具| 黄片播放在线免费| 精品少妇久久久久久888优播| xxx大片免费视频| 欧美亚洲 丝袜 人妻 在线| 只有这里有精品99| 高清av免费在线| 欧美日韩av久久| 午夜免费观看性视频| 亚洲欧美一区二区三区黑人 | 午夜久久久在线观看| videossex国产| 一级a爱视频在线免费观看| 男人舔女人的私密视频| 午夜福利,免费看| 哪个播放器可以免费观看大片| 久久 成人 亚洲| av在线app专区| 久久女婷五月综合色啪小说| 一级,二级,三级黄色视频| 国产一区亚洲一区在线观看| av在线播放精品| 久久久久国产精品人妻一区二区| 国产深夜福利视频在线观看| 国产精品.久久久| 久久99蜜桃精品久久| 激情五月婷婷亚洲| 免费在线观看视频国产中文字幕亚洲 | 亚洲欧美一区二区三区国产| 久久精品熟女亚洲av麻豆精品| 久久免费观看电影| 欧美另类一区| 亚洲av综合色区一区| 亚洲精品美女久久av网站| 国产麻豆69| 婷婷色综合www| 少妇精品久久久久久久| 久久久欧美国产精品| 婷婷色麻豆天堂久久| 精品第一国产精品| 建设人人有责人人尽责人人享有的| 人妻 亚洲 视频| 日韩av不卡免费在线播放| 欧美日韩一区二区视频在线观看视频在线| 欧美国产精品va在线观看不卡| 久久人人爽人人片av| videos熟女内射| 免费在线观看完整版高清| 男女下面插进去视频免费观看| 99热国产这里只有精品6| 亚洲国产欧美在线一区| 免费观看无遮挡的男女| 国产老妇伦熟女老妇高清| 另类精品久久| 久久久久久人妻| 波野结衣二区三区在线| 国产一区二区在线观看av| 91精品国产国语对白视频| 欧美日韩亚洲高清精品| 国产高清国产精品国产三级| 我要看黄色一级片免费的| 国产乱人偷精品视频| 老司机影院毛片| av片东京热男人的天堂| av国产久精品久网站免费入址| 国产精品99久久99久久久不卡 | 免费黄色在线免费观看| 亚洲人成网站在线观看播放| av.在线天堂| 久久久久国产网址| 国产又爽黄色视频| 亚洲国产精品一区二区三区在线| av天堂久久9| 韩国精品一区二区三区| 亚洲精品一区蜜桃| 成年美女黄网站色视频大全免费| 久久久久国产一级毛片高清牌| 超碰成人久久| 成年动漫av网址| 十八禁网站网址无遮挡| 久久精品国产亚洲av涩爱| 制服丝袜香蕉在线| www.熟女人妻精品国产| 另类精品久久| 免费观看av网站的网址| 97在线视频观看| 精品国产超薄肉色丝袜足j| av有码第一页| 日韩大片免费观看网站| 黄网站色视频无遮挡免费观看| 久久久久国产网址| 亚洲国产欧美在线一区| 亚洲精品中文字幕在线视频| 欧美变态另类bdsm刘玥| 波多野结衣一区麻豆| 午夜日韩欧美国产| h视频一区二区三区| 男的添女的下面高潮视频| 色视频在线一区二区三区| 在线观看人妻少妇| 美女大奶头黄色视频| 91在线精品国自产拍蜜月| 天天躁夜夜躁狠狠躁躁| 叶爱在线成人免费视频播放| 亚洲成国产人片在线观看| 国产黄色视频一区二区在线观看| 十八禁网站网址无遮挡| 亚洲伊人久久精品综合| 欧美日韩av久久| 在线天堂中文资源库| 色吧在线观看| 国产成人aa在线观看| 国产精品二区激情视频| 一本色道久久久久久精品综合| 啦啦啦中文免费视频观看日本| 国产乱人偷精品视频| 欧美精品一区二区大全| 黄片播放在线免费| 日韩制服丝袜自拍偷拍| 叶爱在线成人免费视频播放| 国产亚洲欧美精品永久| 久久久久久久大尺度免费视频| 捣出白浆h1v1| 男的添女的下面高潮视频| 2018国产大陆天天弄谢| 97精品久久久久久久久久精品| 国产精品国产av在线观看| 亚洲色图 男人天堂 中文字幕| 国产无遮挡羞羞视频在线观看| 看免费成人av毛片| 七月丁香在线播放| 日本欧美国产在线视频| 精品视频人人做人人爽| 久久精品亚洲av国产电影网| av国产精品久久久久影院| 国产又爽黄色视频| av在线观看视频网站免费| 亚洲国产欧美网| 美女中出高潮动态图| 亚洲欧美精品自产自拍| 免费av中文字幕在线| 国产成人欧美| 欧美日韩综合久久久久久| 国产成人精品婷婷| 一二三四在线观看免费中文在| 亚洲精品美女久久久久99蜜臀 | 巨乳人妻的诱惑在线观看| 亚洲精品日韩在线中文字幕| 黄色毛片三级朝国网站| av在线app专区| freevideosex欧美| 日日摸夜夜添夜夜爱| 免费黄频网站在线观看国产| 久久久亚洲精品成人影院| 亚洲,一卡二卡三卡| 久久久a久久爽久久v久久| 婷婷色麻豆天堂久久| 王馨瑶露胸无遮挡在线观看| 国产精品国产av在线观看| 日日撸夜夜添| 亚洲精品在线美女| 精品国产一区二区三区久久久樱花| 欧美另类一区| 国产在线一区二区三区精| av在线观看视频网站免费| 人妻人人澡人人爽人人| 高清视频免费观看一区二区| 99香蕉大伊视频| 午夜福利影视在线免费观看| 少妇的逼水好多| 亚洲第一区二区三区不卡| 久久ye,这里只有精品| 99久久人妻综合| 亚洲人成电影观看| 亚洲婷婷狠狠爱综合网| 国产不卡av网站在线观看| 少妇被粗大猛烈的视频| 少妇 在线观看| 亚洲成人av在线免费| 人人妻人人添人人爽欧美一区卜| 亚洲国产毛片av蜜桃av| 欧美bdsm另类| 亚洲欧美精品综合一区二区三区 | 亚洲一级一片aⅴ在线观看| 欧美 亚洲 国产 日韩一| 免费在线观看完整版高清| av免费在线看不卡| 在线观看www视频免费| 亚洲精品aⅴ在线观看| 青青草视频在线视频观看| 日韩电影二区| 在线观看免费日韩欧美大片| 免费在线观看视频国产中文字幕亚洲 | 精品视频人人做人人爽| 免费播放大片免费观看视频在线观看| 狂野欧美激情性bbbbbb| 亚洲成色77777| 国产亚洲午夜精品一区二区久久| 韩国精品一区二区三区| 亚洲一区二区三区欧美精品| 精品国产国语对白av| 18禁国产床啪视频网站| 亚洲伊人久久精品综合| 性色av一级| 黄频高清免费视频| 校园人妻丝袜中文字幕| 在线观看一区二区三区激情| 成人国产麻豆网| 国产亚洲一区二区精品| 女性生殖器流出的白浆| 国产精品女同一区二区软件| 男女无遮挡免费网站观看| 人人妻人人澡人人看| 国产黄色视频一区二区在线观看| 亚洲第一区二区三区不卡| 啦啦啦中文免费视频观看日本| 久久精品aⅴ一区二区三区四区 | 美女国产高潮福利片在线看| 精品人妻熟女毛片av久久网站| av又黄又爽大尺度在线免费看| 女人被躁到高潮嗷嗷叫费观| 亚洲精品视频女| 我要看黄色一级片免费的| 国产成人一区二区在线| 久久久久视频综合| 欧美 日韩 精品 国产| 午夜日本视频在线| 美国免费a级毛片| 看免费成人av毛片| 国产精品人妻久久久影院| 亚洲国产欧美日韩在线播放| 国产女主播在线喷水免费视频网站| 啦啦啦在线免费观看视频4| 欧美变态另类bdsm刘玥| 一本—道久久a久久精品蜜桃钙片| 亚洲国产欧美日韩在线播放| 亚洲精品自拍成人| 亚洲欧美清纯卡通| www.av在线官网国产| 精品一区在线观看国产| 丁香六月天网| 日本av免费视频播放| 欧美日韩精品网址| 老司机影院毛片| 日韩成人av中文字幕在线观看| 亚洲国产看品久久| 亚洲天堂av无毛| 亚洲欧美中文字幕日韩二区| 国产伦理片在线播放av一区| 亚洲欧洲日产国产| av在线app专区| 男人操女人黄网站| 九色亚洲精品在线播放| 亚洲成色77777| 国产高清国产精品国产三级| av在线老鸭窝| 一区二区三区精品91| av电影中文网址| 亚洲,欧美,日韩| 少妇的丰满在线观看| 韩国高清视频一区二区三区| 交换朋友夫妻互换小说| 大片免费播放器 马上看| 亚洲,欧美,日韩| 日韩一卡2卡3卡4卡2021年| 在线观看www视频免费| 香蕉丝袜av| 亚洲精品av麻豆狂野| 久久久久久久国产电影| 天天躁夜夜躁狠狠久久av| 亚洲国产精品一区三区| 18禁观看日本| 国产成人精品无人区| 啦啦啦在线观看免费高清www| 激情视频va一区二区三区| 最近中文字幕2019免费版| 日本av手机在线免费观看| 少妇的逼水好多| 亚洲精品乱久久久久久| 香蕉精品网在线| 少妇被粗大猛烈的视频| 99久国产av精品国产电影| 亚洲人成网站在线观看播放| av免费在线看不卡| 成人二区视频| 亚洲,欧美精品.| 亚洲国产精品999| 在线观看三级黄色| www日本在线高清视频| 免费高清在线观看日韩| 在线观看美女被高潮喷水网站| 欧美97在线视频| 亚洲国产av新网站| 欧美日韩亚洲高清精品| 男女啪啪激烈高潮av片| 美国免费a级毛片| 人人妻人人澡人人爽人人夜夜| 91精品国产国语对白视频| 伦精品一区二区三区| 一级片'在线观看视频| 老熟女久久久| 一区在线观看完整版| 亚洲国产精品一区三区| 日日摸夜夜添夜夜爱| 国产成人午夜福利电影在线观看| 秋霞在线观看毛片| av.在线天堂| 婷婷色综合www| 亚洲成人av在线免费| 在线观看免费高清a一片| 国产一区二区三区综合在线观看| 成人18禁高潮啪啪吃奶动态图| 秋霞伦理黄片| 熟女少妇亚洲综合色aaa.| 一个人免费看片子| 亚洲欧美成人综合另类久久久| 国产精品久久久久久久久免| 五月伊人婷婷丁香| 丝袜在线中文字幕| 黄片无遮挡物在线观看| 一二三四在线观看免费中文在| 亚洲一码二码三码区别大吗| 超碰成人久久| 久久人妻熟女aⅴ| 婷婷色综合www| 国产精品av久久久久免费| 久久午夜福利片| 久久女婷五月综合色啪小说| 在线观看免费高清a一片| 九草在线视频观看| av国产精品久久久久影院| 十八禁网站网址无遮挡| 色视频在线一区二区三区| 亚洲男人天堂网一区| 黑人欧美特级aaaaaa片| 亚洲精华国产精华液的使用体验| 丰满乱子伦码专区| h视频一区二区三区| 国产男女内射视频| 久久婷婷青草| 国产激情久久老熟女| 国产又爽黄色视频| 中文精品一卡2卡3卡4更新| 免费少妇av软件| 久久久久视频综合| 欧美精品高潮呻吟av久久| 色吧在线观看| 国产精品麻豆人妻色哟哟久久| 国产一区亚洲一区在线观看| 女人高潮潮喷娇喘18禁视频| 少妇人妻久久综合中文| 久久精品国产鲁丝片午夜精品| 日韩制服骚丝袜av| 女人高潮潮喷娇喘18禁视频| av免费在线看不卡| 国产成人精品一,二区| 中文字幕色久视频| 男人添女人高潮全过程视频| 男女边吃奶边做爰视频| 成年女人在线观看亚洲视频| 一级片'在线观看视频| 美女中出高潮动态图| 亚洲欧美成人综合另类久久久| 欧美 日韩 精品 国产| 久久精品国产自在天天线| 在线观看www视频免费| 一级片免费观看大全| 国产精品99久久99久久久不卡 | 十八禁网站网址无遮挡| 久久99热这里只频精品6学生| 欧美黄色片欧美黄色片| 男女高潮啪啪啪动态图| 男女无遮挡免费网站观看| 成人国语在线视频| 老熟女久久久| 又大又黄又爽视频免费| 纯流量卡能插随身wifi吗| 国产免费福利视频在线观看| 性色avwww在线观看| 免费在线观看完整版高清| 亚洲精品国产一区二区精华液| 午夜影院在线不卡| 国产一区亚洲一区在线观看| tube8黄色片| 日韩大片免费观看网站| 亚洲国产毛片av蜜桃av| 18禁裸乳无遮挡动漫免费视频| 97在线人人人人妻| 亚洲av成人精品一二三区| 香蕉精品网在线| 91国产中文字幕| 久久人人爽人人片av| 一级,二级,三级黄色视频| 国产黄色视频一区二区在线观看| 成人毛片a级毛片在线播放| 欧美日韩av久久| 男的添女的下面高潮视频| 国产片特级美女逼逼视频| 亚洲欧美精品自产自拍| 日本欧美国产在线视频| 成年美女黄网站色视频大全免费| 夜夜骑夜夜射夜夜干| 欧美激情高清一区二区三区 | 国产1区2区3区精品| 精品人妻熟女毛片av久久网站| 久久综合国产亚洲精品| 国产不卡av网站在线观看| 国产精品一区二区在线不卡| 欧美激情 高清一区二区三区| 搡老乐熟女国产| 热99久久久久精品小说推荐| 欧美日韩亚洲国产一区二区在线观看 | 国产乱人偷精品视频| 亚洲国产欧美在线一区| av视频免费观看在线观看| 色视频在线一区二区三区| 看十八女毛片水多多多| 日韩欧美精品免费久久| 免费观看av网站的网址| 夜夜骑夜夜射夜夜干| 日本-黄色视频高清免费观看| 最近手机中文字幕大全| 欧美xxⅹ黑人| 777久久人妻少妇嫩草av网站| 2022亚洲国产成人精品| 妹子高潮喷水视频| 中文字幕人妻熟女乱码| 亚洲伊人色综图| 国产一区亚洲一区在线观看| 欧美97在线视频| 久久久精品94久久精品| 免费在线观看完整版高清| 观看美女的网站| 免费在线观看完整版高清| av一本久久久久| 18禁国产床啪视频网站| 中国国产av一级| 99re6热这里在线精品视频| 国产一区二区在线观看av| 久久久久久人人人人人| 美女主播在线视频| 精品亚洲乱码少妇综合久久| 国产熟女午夜一区二区三区| 久久精品久久久久久久性| av福利片在线| 波多野结衣av一区二区av| 99热网站在线观看| 国产淫语在线视频| 在线观看美女被高潮喷水网站| 色94色欧美一区二区| 五月天丁香电影| 大香蕉久久成人网| 亚洲精品中文字幕在线视频| 亚洲精品日本国产第一区| 亚洲人成电影观看| 18禁观看日本| 久久久久国产一级毛片高清牌| 国产精品不卡视频一区二区| 久久韩国三级中文字幕| 大话2 男鬼变身卡| 一级a爱视频在线免费观看| 亚洲色图 男人天堂 中文字幕| 国产爽快片一区二区三区| 精品福利永久在线观看| 久久人人爽人人片av| 在线观看免费日韩欧美大片| 丝袜在线中文字幕| 少妇人妻 视频| 巨乳人妻的诱惑在线观看| 久久ye,这里只有精品| 免费大片黄手机在线观看| 婷婷色综合www| 日韩人妻精品一区2区三区| 三级国产精品片| 婷婷色综合大香蕉| 亚洲美女搞黄在线观看| 亚洲精品乱久久久久久| 久久精品aⅴ一区二区三区四区 |