    Friction surfacing of AISI 316 over mild steel:A characteriation study

    2018-08-25 03:15:26GeorgeSahayaNixonMohantySathish
    Defence Technology 2018年4期

    R.George Sahaya Nixon,B.S.Mohanty,R.Sathish

    aDepartment of Mechanical,Sathyabama University,Chennai 600119,Tamilnadu,India

    bDepartment of Mechanical Engineering,St.Joseph's College of Engineering,Chennai 600119,Tamilnadu,India

    cDepartment of Mechanical Engineering,SRM Easwari,Chennai 600089,Tamilnadu,India

    Keywords:Friction surfacing Rotational speed Traverse speed Axial load Salt spray test Microstructure XRD analysis Ram tensile test

    A B S T R A C T An attempt has been made with overlaying of stain-less steel on mild steel by the technique of friction surfacing.This investigation elaborates the excellence acquired by different combination of the process parameters used in friction surfacing specifically traverse speed of the cross slide,speed of rotation of the spindle and the uniaxial compressive load.Excellent overlaying has been obtained amongst the chosen materials.To which,the coating can be done with various set of process parameters.It has been observed that the bond strength of the coating was found to be at a maximum of 502 MPa by ram tensile test.Based upon this results the surface methodology was characterized with scanning electron microscope.For authenticating the results,the coated specimen was subjected to salt spray test.The bonding microstructure was characterized using optical microscopy and X-ray diffraction.Corrosion resistance of surfaced coatings was found to be more inferior to that of mechtrode material and greater with the substrate.

    1.Introduction

    Surface science and engineering truces with the exterior of the hardest material and it is sub restraint of materials science.The solid material includes a granular or lumpy mixture of material protected through an exterior surface and it is called outward phasing.The external surface of a solid interrelates with the adjacent atmosphere[1].Friction surfacing is a superior surface alteration process,this technique was comparatively very simple,with which overlaying of the materials will be empowered after reconstruction of friction welding processes(Fig.1).This process was much greater with related to resources of other surface modification processes and energy management[2].Wear can be curtailed by amending the surface possessions of solids by surface finishing or by use of lubricants.Approximately the entire kind of materials,polymers and composites were able to be bonded on materials which are alike or unlike[3].This phenomenon was obtained by creating the strengthened surface to the location in which it will be made to protect fromwear and corrosion to prolong its life and also develop artistic manifestation of the substrates.This means that proper maintenances and the standby of scratched components are not continuously essential,limited maintenances of faults will be permissible,and that was achieved by friction surfacing of nonferrous materials[4].In this process,tool steels which are contained with rigid stages cannot be easily formulated by deposition of materials.Here the melting process was not in bulk form and during the process of friction surfacing plasticization of materials due to dynamic re-crystallization has been highlighted[5].It is promising to weld the different materials that can be mismatched or challenging to overlay the consumable by non dilution processes[6].Related with these friction based processing techniques,by avoiding the deprivation on properties of material leads to lowering the heat input as well[7].Bedford et al.reported,that the non appearance of melting leads to lesser residual stages and disappearance of dilution meanwhile the solidification shrinkage does not occur in dissimilar steels[8].

    It consists of a rotating cylinder-shaped rod which is fed towards a plate with uniaxial compressive load performing at the same time.The difference in temperature is engendered amongst the plate and the rod.By the time of coating end of the rod is appropriately changed into the state of plasticization,the plate is intersected parallel with reference to the consumable rod[9].As the traverse speed was initiated at a definite amount,the metal undergone dilution consumed over it.A close view of friction surfacing process was shown in Fig.2.The axial force on the consumable,traverse speed on the substrate and rotational speeds on the rod is the primary process parameters for the aforementioned process[10].The effect of speed of the cross slide over the dimensional variables,bond uniqueness of the interface and mechanical characteristics of the bond has been reported by Khalid Ra fiH.et al.[11].

    2.Materials and experimental methods

    Mild steel plate of 10mm thickness as a substrate was machined to 75 mm width 150 mm length.AISI316 stainless steel bar of 20 mm in diameter and 100mm length was used as a coating rod.The chemical compositions of these base metals are shown in Tables 1 and 2,respectively.

    The geometry of the material used for friction surfacing process prior to coating was shown in Fig.3.Flatness of the consumable rod ends has been safeguarded by lathe machining.Surface grinding and milling was performed on the substrate to ensure flatness and the surface has to be restricted from oxides.Both consumable rod and the plate have to be washed with acetone earlier to surfacing towards reduction of the impurities during the process.Experimentations are piloted to define the operational assortment of the aspects,such as rotational speed of mechtrode,substrate traverse speed and axial force on mechtrode.The friction surfacing operation was done when the coating rod consumes about 30 mm from its length and the welding bead was at a distance of 50 mm to be overlaid.This process was done under the surfacing conditions of L9 orthogonal array as shown in Table 3.

    Table 1 Chemical composition of stainless steel AISI 316.

    Table 2 Chemical composition of mild steel.

    The interfacial strengths of the coating and the substrate were determined by a tailor made ram tensile strength method.The specimen is loaded in UTM and the tensile strength values in MPa were measured by using the ram tensile test setup as shown in Fig.4.Transverse segments were taken from the overlay were equipped for fractographic characterization for typical metallographic examination.X-ray diffraction(XRD)investigations were carried out by using A Philips X'pert PRO diffractometer at Cu Ka radiation for phase analysis.FS coated samples was carried out with XRD analysis.To evaluate the intensity over the bond,the d-ferrite quantity in FS coatings were found out by means of a Fischer-make polished specimens were electrolytically imprinted with 60%HNO3aqueous solution then the specimen were investigated by Leicamake optical microscope and an FEI-make SEM.AISI316 and mild steel were exposed to unfavorable chemical surroundings for the process of studying the durability and strength of AISI316-mild steel coatings under chemical resistance test.Salt spray tests of bonded specimen before and after acquaintance to 3.5%NaCl mist environment has been conducted.

    The tensile strength of the friction surfaced specimens was determined to find their effective coherence.The ram tensile fixture was specifically designed as per MIL-J-24445(SH)standard for estimating the tensile strength of the coating.The material coated and the substrate was made to lay upside down,coated surface facing the machining table and the substrate facing the tool.The Substrate was machined in the form of an inner circle or a hole to form an annular space between the substrate and the intact coating.Appropriate machining of the surfaces was made to facilitate effective clamping of the specimen on the designed fixture[12].The inner circular area in the annular space was meant only for loading.The Universal Testing Machine was utilized to test the specimens.The specimen is loaded in UTM and the tensile strength values in MPa were measured by using the ram tensile test setup as shown in Fig.4.The materials failed upon the action of regions where force is applied by push off tool.It is noticed that strong bonding between the materials has been obtained by applying tensile forces towards the materials.For the other samples the tensile testing were done to find the strength of the coating.It is observed that higher the axial load considerable rotational speed and traverse speed give more tensile strength and more ductility.Also when input process parameters are lowered it indicates lower tensile strength[13].Further studies have been made with the sample of greater bond strength i.e.the specimen with the highestvalue of bond strength was preceded for the characterization study.

    Table 3 Design matrix and measured bond strength.

    2.1.Ram tensile test

    There are various methods of mechanical testing were done with the friction surfaced samples like shear test,bend test and chisel test.Among these mechanical characterizations the bond strength can be evaluated by a tensile test method called as method called ram tensile test.These techniques make certain breakdown of the sample in the interface by a normal tensile force which signifies the bond strength.The bond strength of overlay is shown in Table 3.From Table 3 it can be concluded that the highest tensile strength of 502 MPa and the lowest bond strength of 259 MPa were acquired on the AISI 316 bonding created in the present investigation[14]All ram tensile test samples were noticed that it will deform at the substrate interface.Representing sketch and image of ram tensile test sample are shown in Fig.4.

    3.Results and discussion

    3.1.Quality of deposition

    Initially the bond quality has been predicted by visual inspection.Deposit appearance and the images are given in Fig.5.Deposits are classified into narrow deposit,deposit due to shear,greater width,variable width,decreasing width,continuous,uniform and non-uniform are attained by several combinations of the process parameters[14].The dependency on the coating conditions might be the purpose for quantity of the deposit since surfacing was maintained in accordance with the length of the mechtrode.The exterior of the bonding varies upon the parameter levels.The schematic diagram after the process is shown in Fig.3.It was evidently shown that the circularity patterns become visible on the plate by the rotation of the spindle i.e.,the rod which has been consumed,apart from of the speed of the cross slide.The exterior of bond was alike other nonferrous materials[15].Sample S3 gets thinner deposit and it was uniform throughout the bead.Similarly sample S6 and S9 deposits are also in the same case since the deposit geometry are found to be excellent in ripple formation.In the overlaid samples S2 and S8 it is observed that the bonding was discontinuous with constant rotational speed.The coating interpretation for the entire specimen was shown in Table 4.The roughness of the deposits has been measured and that is in the range of 1.5 μm-3.5 μm.The bonding with length was between 100.5 and 110.8±0.05mm,coating width of 23.5-24.5±0.05mm and coating thickness of 2.21±0.05mm,were formed by the known process parameters[16].

    3.2.Chemical resistance test

    Chemical resistance test for mechtrode(AISI316)and mild steel substrate.For the chemical resistance test,AISI316 and mild steel were exposed to unfavorable chemical atmosphere viz.H2O,acid and alkali for the process of studying the durability and strength of AISI316-mild steel coatings[17].The data obtained for mechtrode(AISI316)and mild steel substrate have been listed in Table 5.

    The MILD STEEL substrate experienced extreme weight loss in aquatic medium while AISI316-MILD STEEL coatings showed no effect in aqueous medium on behalf of that these bonded specimen of(AISI316-MILD STEEL)representing an impervious prevention to the plate of mild steel which would not consent entry for water and other corrosive species,there by authorizing the success in guarding the substrate from rust[18].In addition,the immersion of these test specimens in 5wt%Sulfuric acid and 5wt%Sodium Hydroxide for 24h had their exteriors continue undamaged with a minor weight loss.The enhanced performance exposed by AISI316,AISI316-MILD STEEL coatings may be due to passive film,causing greater reliability of such coatings.However,AISI316-MILD STEEL bonded specimen were said to be temporarily resistant to alkali atmosphere.Significant corrosion attacks did not exhibited in the consumable rod in the friction surfaced bonding and was free from intergranular corrosion[19].

    3.3.Microstructure analysis

    For the sample,the fractography indicates fusion between the two parent metals,the fractography illustrate ferrite-pearlite grains perceived all over the matrix and next to the heat affected zone presenting fine grains of ferrite-pearlite and somewhat malformed martensite.Higher hardness was denoted due to incomplete martensitic pattern[20].Fig.6(a)and(b)shows the microstructures in the parent metals of substrate and the mechtrode.During friction surfacing,as the parent metals experiences a thermomechanical phenomena, fine grained microstructure is generated by dynamic recrystallization.The microstructure was then found using metallurgical microscope called metascope The etchant used for AISI 316 is 10ml of nitric acid(HNO3)+10 ml of acetic acid+15 ml of hydrochloric acid(HCl)and two drops of glycerol.By this the microstructure revealed that austenite,delta ferrite and small percentage of chromium-n precipitate having a pearlite in a ferrite matrix.After the process microstructure is in the type of eutectic ferrite and pearlite.Grains in Fig.6(c)shows the fusion between the two interfaces.It was observed that the intermingling of both these materials in the fusion zone was bonded with greater coherence[21].This confirms that more amount of heat was generated in friction surfacing of 316 when compared to other grades of steel.Also the diffusion pattern between AISI 316 and mild steel was denser than other grades of steel.The grain size in the HAZ is small which causes the increase in hardness of the material at the joint of two materials.Plastic deformation and heat generation in combination reports full austenization and dynamic recrystallization[22].It has been noticed that bonding geometry may rely on the parametric stages and in addition the grains were dynamically recrystallized due to the speed of the cross-slide on both the progressing and withdrawing sides[23].

    Table 4 Process parameters for specimens and the interpretations on the consumable rod and overlay.

    Table 5 Results of chemical resistance tests.

    3.4.SEM analysis(scanning electron microscope)

    The SEM images of MS laid on SS316 for the sample subjected to maximum bond strength has been done with Leica-make optical microscope and an FEI-make SEM.The images displayed are a)500X magnification and b)1000X magnification respectively.It has been observed that the base metal was highly corroded when compared with the consumable material.The interface of the overlaid materials of SS316 metal exhibits very fine martensitic features as that of the coated metal MS.In advancing and retreating side very fine martensitic features was visible to which it is displayed in Fig 7.1(a)and(b).The cross sectional view show more homogeneous surface compared to the top and bottom surface of metal however some pores are observed in the advancing side[24].The retreating side was the end where the direction of spindle rotation and the direction of the overlaying.The end where path of consumable rod rotation and way to coating development are opposite is referred to as retreating side[25].Owing to the movement of material from one end to the other end there was some microstructural differences are probably will be there in-between the advancing and retreating sides as shown in Fig 7.2(a)and(b)which was free from any pores and considered as more effective bonding between the substrate and mechtrode.The huge force exerted on the base metal SS316 might have disturbed its austenitic matrix further the temperature generated might have been less than 1200°C to form austenitic phase at the interface[26].The Fig 7.3(a)and(b)shows the SEM images parent metal.The high magnification image reveals fine intra-granular lath martensitic features in austenitic matrix[27].

    3.5.XRD analysis(X-ray diffraction)

    XRD studies were done to assess the presence ofα-ferrite in the deposited austenitic matrix.XRD studies of friction surfaced coating confirmed the absence ofα-ferrite and the presence of strain-induced martensite(Fig.8).The findings were well matched with the observation of microstructural inspection.Throughout the process,the consumable rod becomes austenitized,upon with speedy cooling,changes into martensite,resulting in a solid tool steel bonding[28].The nonexistence ofα-ferrite in the bonding clearly established that the temperature(1000°C)generated during friction surfacing has not exceeded the limit(1200°C)required for the formation ofα-ferrite,and suggest that the mechtrode was made with raise in temperature into theα-ferrite zone field towards the process.Similar results were observed in earlier studies for different metal coating.The absence ofα-ferrite in the bonding is beneficial in improving the corrosion resistance compared to fusion based cladding process[29].The table gives the peak position,intensity,full width half maximum value(FWHM)and dspacing values of MS laid over SS316 Table 6.The XRD analysis confirms the presence of martensitic phase as observed in SEM image[30].Friction-surfaced SS316-coated mild steel specimen seems to be appropriate for usage in coated state.Additional development in fractography and characterization were possible with appropriate post-surfacing heat treatment,which will make stronger martensite and make things easier with carbide precipitation[31].

    Table 6 XRD results.

    3.6.Salt spray test(corrosion)

    Salt spray test was done with samples of 10 mm×10 mm×10 mm with cubic bonded pieces.It is used to create the oceanic atmosphere where the specimen was interpreted according to ASTM B 117-3.Fig.9 provides details of the salt spray results of bonded pieces prior and after acquaintance to 3.5%NaCl mist environment.There was no observable corrosion products on the exterior of the mechtrode at the conclusion of the salt spray test region of sections coated with mild steel.The results of the interpretations made for the coatings AISI316,AISI316-and MILD STEEL after 50 h and 250 h of salt-spray test are seen in Table 7.There was neither corrosion nor bonding imperfections on the parent metal sections shown by the intact flaws.The processes used for cleaning the samples prior to loading and subsequently complete the testing as given as:a)Samples are cleaned mildly before loading:b)Surfaces dried immediately from clean running water slightly to remove salt deposits.The pieces were sensibly noticed for the finding of corroded area on their exterior area and images were taken by digital camera.The period for the development of brown rust and blisters was noticed.The specimen before and after test was displayed in Fig.9 However,rusting without spread was seen at AISI316-MILD STEEL.This indicates an impressive enactment of the originations against salt surroundings[32].Hence AISI316-MILD STEEL formulations produced satisfactory good outcomes without any maximum loss of coating,blazing and eroding of the cross-cut still after 250h of salt-spray testing in the filing cabinet.On the other hand,the substrate mild steel shows pitiable salt-spray resistance[33].The results of the salt spray test was displayed in Table 7.

    3.7.Research gap

    The corresponding literature show the investigations by several researchers in number of combinations on dissimilar materials in friction surfacing.Also,numerous researchers were conductedexperiments to analyze the mechanical and metallurgical behavior of selected materials.The analysis of the deposit geometry and corrosion analysis over the friction surfaced specimen has been carried out over the deposited material.However,the efforts so for made indicates an insufficiency of attempts towards replacing the substrate material by Mild steel over AISI316 which exhibits poor corrosion resistance,improved mechanical properties and also high machinability having wide commercial applications.The uses for Mild steel are defined by the requirement for a high tensile strength and ductility that,despite its brittleness when compared to other forms of steel,make it the preferred choice.The present work deals with these important concerns[34].

    Table 7 Results of salt spray(fog)test.

    4.Conclusion

    The friction-surfacing development was found prime to substantial particle enhancement.The creative grains were first rigorously cropped and dispersed due to the geometrical consequence of strain.The widespread sub operational enlargement segmented them into minor,irregular-shaped grains,thus evidencing the occurrence of continuous recrystallization.The huge force exerted on the base metal AISI 316 might have disturbed its austenitic matrix further the temperature generated might have been less than 1200°C to form austenitic phase at the interface.The ultimate tensile strength varies from 259 MPa to 504MPa by ram tensile test.The high magnification FESEM image reveals fine intragranular martensitic features in austenitic matrix.The absence ofαferrite in friction the coating is beneficial in improving the corrosion resistance compared to fusion based cladding process.The XRD analysis confirms the presence of martensitic phase as observed in SEM image.There was no observable corrosion products on the exterior of the mechtrode at the conclusion of the salt spray test region of sections coated with mild steel.

    色婷婷av一区二区三区视频| 久久av网站| 久久久久精品人妻al黑| 国产精品99久久99久久久不卡| 日日爽夜夜爽网站| 极品人妻少妇av视频| 精品人妻1区二区| 不卡一级毛片| 精品一区二区三区av网在线观看 | 午夜日韩欧美国产| 午夜福利影视在线免费观看| 美国免费a级毛片| 美国免费a级毛片| 在线十欧美十亚洲十日本专区| 免费在线观看日本一区| 一本久久精品| 真人做人爱边吃奶动态| av在线播放精品| netflix在线观看网站| 亚洲国产欧美网| 欧美日韩av久久| 亚洲一区中文字幕在线| 999久久久精品免费观看国产| 亚洲国产精品成人久久小说| 9热在线视频观看99| 777久久人妻少妇嫩草av网站| 久久久国产精品麻豆| 国产深夜福利视频在线观看| 久久久久久久大尺度免费视频| av天堂在线播放| 欧美激情 高清一区二区三区| 人妻一区二区av| a级片在线免费高清观看视频| 成年动漫av网址| 国产91精品成人一区二区三区 | 在线观看人妻少妇| 久久久国产欧美日韩av| 美女午夜性视频免费| 深夜精品福利| 大型av网站在线播放| 波多野结衣一区麻豆| 午夜精品久久久久久毛片777| 免费观看a级毛片全部| 欧美在线一区亚洲| 可以免费在线观看a视频的电影网站| 中文字幕人妻丝袜制服| 久久精品成人免费网站| 波多野结衣一区麻豆| av网站在线播放免费| 亚洲欧洲精品一区二区精品久久久| 亚洲精品久久午夜乱码| 人妻人人澡人人爽人人| 在线十欧美十亚洲十日本专区| 丰满少妇做爰视频| 欧美另类一区| 日本vs欧美在线观看视频| 日韩欧美国产一区二区入口| 女人爽到高潮嗷嗷叫在线视频| 亚洲情色 制服丝袜| 国产亚洲精品一区二区www | 国产成人一区二区三区免费视频网站| 亚洲精品中文字幕一二三四区 | 亚洲精华国产精华精| 免费不卡黄色视频| 亚洲国产精品一区三区| 无限看片的www在线观看| 亚洲国产精品成人久久小说| 亚洲欧美激情在线| 亚洲 国产 在线| 亚洲精品一区蜜桃| 亚洲欧美色中文字幕在线| 久久狼人影院| 精品人妻熟女毛片av久久网站| 国产男女超爽视频在线观看| 叶爱在线成人免费视频播放| 视频在线观看一区二区三区| 后天国语完整版免费观看| 成人黄色视频免费在线看| 丝袜人妻中文字幕| 香蕉国产在线看| 亚洲五月婷婷丁香| 欧美黄色片欧美黄色片| 女人爽到高潮嗷嗷叫在线视频| 五月天丁香电影| 久久国产精品影院| 纯流量卡能插随身wifi吗| 久久精品aⅴ一区二区三区四区| 精品人妻熟女毛片av久久网站| 少妇裸体淫交视频免费看高清 | 久久久精品94久久精品| www.av在线官网国产| 亚洲,欧美精品.| 99re6热这里在线精品视频| 精品国产乱码久久久久久男人| 纵有疾风起免费观看全集完整版| 亚洲一区二区三区欧美精品| 国产一区二区三区av在线| 午夜激情久久久久久久| 一本综合久久免费| 欧美日韩亚洲高清精品| www.自偷自拍.com| 99精品欧美一区二区三区四区| 性色av乱码一区二区三区2| 午夜精品久久久久久毛片777| 自拍欧美九色日韩亚洲蝌蚪91| 性少妇av在线| av天堂久久9| 一本大道久久a久久精品| 国产一级毛片在线| 日韩欧美一区视频在线观看| 国产有黄有色有爽视频| 视频区图区小说| 丰满人妻熟妇乱又伦精品不卡| 两个人看的免费小视频| 国产免费一区二区三区四区乱码| 窝窝影院91人妻| 日韩欧美一区视频在线观看| 国产深夜福利视频在线观看| 午夜影院在线不卡| 久久久久精品人妻al黑| 亚洲性夜色夜夜综合| 日本a在线网址| 久久中文字幕一级| 亚洲专区字幕在线| 老熟妇仑乱视频hdxx| 亚洲精品一二三| 免费观看人在逋| 欧美人与性动交α欧美精品济南到| 日本一区二区免费在线视频| 国产国语露脸激情在线看| 嫁个100分男人电影在线观看| 亚洲美女黄色视频免费看| 美女扒开内裤让男人捅视频| 久久精品国产综合久久久| 欧美日韩中文字幕国产精品一区二区三区 | 69av精品久久久久久 | 满18在线观看网站| 久久久久久久久久久久大奶| 日韩制服骚丝袜av| 亚洲国产精品一区三区| 国产精品1区2区在线观看. | 在线av久久热| 亚洲国产欧美一区二区综合| 美女主播在线视频| 国产男女内射视频| 日日爽夜夜爽网站| 国产精品1区2区在线观看. | 在线观看一区二区三区激情| 精品少妇内射三级| 久久久久久免费高清国产稀缺| 国产精品国产av在线观看| 午夜精品久久久久久毛片777| 99香蕉大伊视频| 国产一区二区 视频在线| 午夜两性在线视频| 久久精品熟女亚洲av麻豆精品| 日韩精品免费视频一区二区三区| 国产精品九九99| 汤姆久久久久久久影院中文字幕| 国产熟女午夜一区二区三区| 亚洲伊人久久精品综合| 精品国内亚洲2022精品成人 | 涩涩av久久男人的天堂| 国产精品一二三区在线看| 亚洲精品国产一区二区精华液| 免费在线观看日本一区| a 毛片基地| 欧美 日韩 精品 国产| 在线观看人妻少妇| 一二三四社区在线视频社区8| 国产91精品成人一区二区三区 | 亚洲第一av免费看| 精品人妻熟女毛片av久久网站| 在线永久观看黄色视频| 又紧又爽又黄一区二区| 国产精品香港三级国产av潘金莲| 国产一区二区激情短视频 | 十分钟在线观看高清视频www| svipshipincom国产片| 国产在视频线精品| 丝袜在线中文字幕| 亚洲成人免费av在线播放| 精品少妇黑人巨大在线播放| 国产成人精品无人区| 欧美成狂野欧美在线观看| 国产在线观看jvid| 一边摸一边抽搐一进一出视频| 亚洲五月色婷婷综合| 无遮挡黄片免费观看| 天天添夜夜摸| 国产欧美日韩综合在线一区二区| 亚洲情色 制服丝袜| 国产视频一区二区在线看| 在线观看一区二区三区激情| 交换朋友夫妻互换小说| 国产成人av教育| 国产片内射在线| 我要看黄色一级片免费的| 成年av动漫网址| 国产精品二区激情视频| 最近最新中文字幕大全免费视频| 少妇人妻久久综合中文| 国产av国产精品国产| 中文字幕制服av| 精品乱码久久久久久99久播| 国产亚洲精品久久久久5区| 视频区欧美日本亚洲| 啦啦啦啦在线视频资源| 国产av一区二区精品久久| 丝袜美腿诱惑在线| 日本av免费视频播放| xxxhd国产人妻xxx| 老司机在亚洲福利影院| 伊人久久大香线蕉亚洲五| 一区二区日韩欧美中文字幕| 19禁男女啪啪无遮挡网站| 久久久精品国产亚洲av高清涩受| 亚洲欧美清纯卡通| 亚洲国产看品久久| 久久精品成人免费网站| 人人澡人人妻人| 黄色 视频免费看| 久久天堂一区二区三区四区| 国产又色又爽无遮挡免| 亚洲国产精品一区二区三区在线| 女人精品久久久久毛片| 啦啦啦视频在线资源免费观看| 性色av一级| 老汉色av国产亚洲站长工具| 国产成人av教育| 50天的宝宝边吃奶边哭怎么回事| 悠悠久久av| 亚洲,欧美精品.| 最近最新免费中文字幕在线| 成人免费观看视频高清| 精品国产超薄肉色丝袜足j| 人妻一区二区av| 啪啪无遮挡十八禁网站| 亚洲欧美成人综合另类久久久| 亚洲国产精品一区三区| 免费日韩欧美在线观看| 每晚都被弄得嗷嗷叫到高潮| 久久久国产欧美日韩av| 三上悠亚av全集在线观看| 桃花免费在线播放| 天堂8中文在线网| 免费在线观看视频国产中文字幕亚洲 | 丰满饥渴人妻一区二区三| 久久狼人影院| 欧美在线一区亚洲| 亚洲国产av新网站| 国产成人影院久久av| 亚洲成av片中文字幕在线观看| 中国美女看黄片| 青春草亚洲视频在线观看| 久久久精品区二区三区| 国产xxxxx性猛交| 国产一区二区三区在线臀色熟女 | 国产无遮挡羞羞视频在线观看| 99国产极品粉嫩在线观看| 久久久久久久国产电影| 午夜福利免费观看在线| 日本vs欧美在线观看视频| 女人爽到高潮嗷嗷叫在线视频| 精品人妻一区二区三区麻豆| 国产精品.久久久| 99久久国产精品久久久| 中国国产av一级| 两个人看的免费小视频| 欧美日本中文国产一区发布| 中文字幕人妻丝袜制服| 日韩大码丰满熟妇| 爱豆传媒免费全集在线观看| 9191精品国产免费久久| 亚洲专区中文字幕在线| 亚洲中文av在线| 精品欧美一区二区三区在线| 丝袜脚勾引网站| 91精品三级在线观看| 久久久精品国产亚洲av高清涩受| 一本久久精品| 国产日韩欧美亚洲二区| 黄色视频,在线免费观看| 亚洲第一欧美日韩一区二区三区 | 精品久久久久久电影网| 丁香六月欧美| 无限看片的www在线观看| 久久久久网色| 欧美一级毛片孕妇| 午夜日韩欧美国产| 成年av动漫网址| 国产三级黄色录像| 老司机福利观看| 纯流量卡能插随身wifi吗| 最近最新中文字幕大全免费视频| 我的亚洲天堂| 国产日韩欧美亚洲二区| 国产精品 国内视频| 正在播放国产对白刺激| 曰老女人黄片| 日本精品一区二区三区蜜桃| 夜夜夜夜夜久久久久| 久热爱精品视频在线9| 精品乱码久久久久久99久播| 最新的欧美精品一区二区| 国产日韩一区二区三区精品不卡| 秋霞在线观看毛片| 高清视频免费观看一区二区| 最近最新中文字幕大全免费视频| 两人在一起打扑克的视频| 岛国在线观看网站| 亚洲成人国产一区在线观看| 中文欧美无线码| 9191精品国产免费久久| 丁香六月天网| 亚洲七黄色美女视频| 久久影院123| 99久久人妻综合| 亚洲国产精品一区二区三区在线| 老司机午夜十八禁免费视频| av国产精品久久久久影院| 亚洲精品国产区一区二| 美女高潮到喷水免费观看| 叶爱在线成人免费视频播放| 精品人妻在线不人妻| 狠狠婷婷综合久久久久久88av| e午夜精品久久久久久久| 免费在线观看视频国产中文字幕亚洲 | 91大片在线观看| 精品福利观看| 91成人精品电影| 少妇裸体淫交视频免费看高清 | 热99re8久久精品国产| av电影中文网址| 宅男免费午夜| 国产极品粉嫩免费观看在线| 亚洲自偷自拍图片 自拍| 宅男免费午夜| 日韩制服骚丝袜av| 女性被躁到高潮视频| 国产精品二区激情视频| 两人在一起打扑克的视频| 欧美日韩精品网址| 人妻一区二区av| 日本撒尿小便嘘嘘汇集6| 曰老女人黄片| 性高湖久久久久久久久免费观看| 法律面前人人平等表现在哪些方面 | 999久久久国产精品视频| 久久久水蜜桃国产精品网| 亚洲av电影在线进入| av超薄肉色丝袜交足视频| 一区二区av电影网| 男男h啪啪无遮挡| 精品视频人人做人人爽| 欧美精品一区二区免费开放| 男男h啪啪无遮挡| 精品一区二区三卡| 亚洲美女黄色视频免费看| 黄色毛片三级朝国网站| av在线老鸭窝| 国产一区二区三区av在线| 久久 成人 亚洲| 精品国产一区二区三区四区第35| 国产成人影院久久av| xxxhd国产人妻xxx| 99久久人妻综合| 五月开心婷婷网| a在线观看视频网站| 啦啦啦视频在线资源免费观看| 欧美黑人精品巨大| 久久免费观看电影| 色婷婷av一区二区三区视频| 在线观看免费高清a一片| 建设人人有责人人尽责人人享有的| 亚洲欧美色中文字幕在线| 国产精品.久久久| 国产色视频综合| 夫妻午夜视频| 精品国产超薄肉色丝袜足j| 国产在线视频一区二区| 久久这里只有精品19| 精品福利观看| 叶爱在线成人免费视频播放| 黄片播放在线免费| 国产精品麻豆人妻色哟哟久久| 美女脱内裤让男人舔精品视频| 亚洲综合色网址| 一二三四在线观看免费中文在| 宅男免费午夜| 青草久久国产| 黑人欧美特级aaaaaa片| 男人舔女人的私密视频| 少妇粗大呻吟视频| 久久精品国产亚洲av高清一级| av天堂久久9| 亚洲全国av大片| 电影成人av| 丝袜美足系列| 亚洲成人国产一区在线观看| 精品久久久久久电影网| 亚洲精品成人av观看孕妇| 黑丝袜美女国产一区| 久久国产精品人妻蜜桃| 免费少妇av软件| 久久精品久久久久久噜噜老黄| 亚洲熟女毛片儿| 亚洲美女黄色视频免费看| 12—13女人毛片做爰片一| bbb黄色大片| 18禁观看日本| 69精品国产乱码久久久| 999久久久国产精品视频| 国产一区二区在线观看av| 十八禁高潮呻吟视频| 首页视频小说图片口味搜索| 久久精品熟女亚洲av麻豆精品| 一级毛片电影观看| 久久av网站| 日日夜夜操网爽| 免费高清在线观看日韩| 欧美 亚洲 国产 日韩一| 男女免费视频国产| 久热爱精品视频在线9| 久久性视频一级片| 少妇粗大呻吟视频| 少妇人妻久久综合中文| 久久久国产欧美日韩av| 免费久久久久久久精品成人欧美视频| 亚洲国产精品999| 国产高清国产精品国产三级| 欧美av亚洲av综合av国产av| 三级毛片av免费| 国产精品99久久99久久久不卡| 老汉色av国产亚洲站长工具| 老司机福利观看| 9热在线视频观看99| 午夜福利,免费看| 在线av久久热| 国产日韩欧美视频二区| 亚洲性夜色夜夜综合| 91老司机精品| 日韩视频在线欧美| 黄色片一级片一级黄色片| 亚洲欧美日韩另类电影网站| 日本a在线网址| av电影中文网址| 国产精品.久久久| 久久久久久久精品精品| 国产av一区二区精品久久| 天天影视国产精品| 国产成人啪精品午夜网站| 热99久久久久精品小说推荐| 日日爽夜夜爽网站| 成年美女黄网站色视频大全免费| 狂野欧美激情性bbbbbb| 久9热在线精品视频| 老熟女久久久| 一级片'在线观看视频| 两个人免费观看高清视频| 亚洲av电影在线观看一区二区三区| 国产欧美日韩精品亚洲av| 亚洲成人手机| 叶爱在线成人免费视频播放| 水蜜桃什么品种好| 久久九九热精品免费| 亚洲精品在线美女| 日韩制服骚丝袜av| avwww免费| 亚洲国产精品一区三区| 国产免费现黄频在线看| 色婷婷久久久亚洲欧美| 亚洲精品自拍成人| 亚洲国产欧美日韩在线播放| 亚洲欧美成人综合另类久久久| 狠狠精品人妻久久久久久综合| 波多野结衣一区麻豆| 热99re8久久精品国产| 精品国内亚洲2022精品成人 | 久久久精品国产亚洲av高清涩受| 免费日韩欧美在线观看| 亚洲七黄色美女视频| 亚洲一区中文字幕在线| 69av精品久久久久久 | 天堂俺去俺来也www色官网| 成年人黄色毛片网站| 国产无遮挡羞羞视频在线观看| 一级片免费观看大全| 男人爽女人下面视频在线观看| 99国产精品一区二区蜜桃av | 女人精品久久久久毛片| 国产一级毛片在线| 久久久国产成人免费| 少妇粗大呻吟视频| 99热国产这里只有精品6| 亚洲 国产 在线| 精品熟女少妇八av免费久了| 悠悠久久av| 在线观看免费午夜福利视频| 久久人人97超碰香蕉20202| 99精品久久久久人妻精品| 热re99久久精品国产66热6| 国产av又大| 老熟妇仑乱视频hdxx| 人人妻人人澡人人看| 嫩草影视91久久| 色婷婷av一区二区三区视频| 在线观看人妻少妇| 久久久久久亚洲精品国产蜜桃av| 日本91视频免费播放| 91麻豆av在线| 精品一品国产午夜福利视频| 午夜久久久在线观看| 日韩欧美一区视频在线观看| 丰满人妻熟妇乱又伦精品不卡| 国产又色又爽无遮挡免| 搡老乐熟女国产| 91精品三级在线观看| 亚洲精品av麻豆狂野| 国产免费现黄频在线看| 丰满少妇做爰视频| 日本a在线网址| 欧美精品啪啪一区二区三区 | 午夜免费鲁丝| 黄色视频不卡| 黑人操中国人逼视频| 久久国产精品大桥未久av| av国产精品久久久久影院| www.av在线官网国产| 中文字幕高清在线视频| 久久久国产精品麻豆| 一本久久精品| 69av精品久久久久久 | 亚洲成人免费av在线播放| 熟女少妇亚洲综合色aaa.| 在线观看一区二区三区激情| 亚洲第一欧美日韩一区二区三区 | 少妇 在线观看| 永久免费av网站大全| 丝袜脚勾引网站| 汤姆久久久久久久影院中文字幕| 亚洲欧美激情在线| 麻豆av在线久日| 午夜两性在线视频| 制服诱惑二区| 自线自在国产av| 99热网站在线观看| 免费少妇av软件| 丰满人妻熟妇乱又伦精品不卡| 久久毛片免费看一区二区三区| 一级毛片电影观看| 欧美午夜高清在线| 免费av中文字幕在线| 久久亚洲国产成人精品v| 亚洲精品国产色婷婷电影| 久久女婷五月综合色啪小说| 麻豆乱淫一区二区| 一本色道久久久久久精品综合| 欧美黄色片欧美黄色片| 精品国产国语对白av| a在线观看视频网站| 丝袜喷水一区| 淫妇啪啪啪对白视频 | a在线观看视频网站| 精品亚洲成a人片在线观看| 久久综合国产亚洲精品| 亚洲av日韩在线播放| 午夜视频精品福利| 午夜久久久在线观看| 一个人免费在线观看的高清视频 | 肉色欧美久久久久久久蜜桃| 国产成人欧美| 久久久国产一区二区| 欧美日韩中文字幕国产精品一区二区三区 | 伦理电影免费视频| 国内毛片毛片毛片毛片毛片| 丝袜在线中文字幕| √禁漫天堂资源中文www| 亚洲人成77777在线视频| 精品少妇一区二区三区视频日本电影| 成人国产av品久久久| 亚洲男人天堂网一区| 欧美人与性动交α欧美软件| 汤姆久久久久久久影院中文字幕| 欧美av亚洲av综合av国产av| 一级毛片精品| a级毛片在线看网站| 丁香六月天网| 啦啦啦中文免费视频观看日本| 久久久久久久久久久久大奶| 亚洲少妇的诱惑av| 9色porny在线观看| cao死你这个sao货| 老熟妇仑乱视频hdxx| 亚洲精品国产色婷婷电影| 国产亚洲精品久久久久5区| 蜜桃国产av成人99| √禁漫天堂资源中文www| 丝袜美腿诱惑在线| 少妇粗大呻吟视频| 国产人伦9x9x在线观看| 亚洲七黄色美女视频| 欧美+亚洲+日韩+国产| 高清在线国产一区| 亚洲av日韩精品久久久久久密| 亚洲欧美日韩另类电影网站| 日韩中文字幕视频在线看片| 国产精品九九99| 亚洲熟女毛片儿| 国产亚洲欧美精品永久| 国产免费现黄频在线看| 精品国产超薄肉色丝袜足j| 高清av免费在线| 久久女婷五月综合色啪小说| 欧美日韩黄片免|