    Electrochemical micromachining of microgroove arrays on phosphor bronze surface for improving the tribological performance

    2018-07-24 09:00:10XunZHOUNingsongQUZhiboHOUGiZHAO
    CHINESE JOURNAL OF AERONAUTICS 2018年7期

    Xun ZHOU,Ningsong QU,b,*,Zhibo HOU,Gi ZHAO

    aCollege of Mechanical and Electrical Engineering,Nanjing University of Aeronautics and Astronautics,Nanjing 210016,China

    bJiangsu Key Laboratory of Precision and Micro-Manufacturing Technology,Nanjing 210016,China

    cState Key Laboratory of Mechanics and Control of Mechanical Structures,Nanjing University of Aeronautics and Astronautics,Nanjing 210016,China

    KEYWORDS Friction coefficient;Microgrooves;Through-mask electrochemical micromachining;Ultrasonic motors;Wear

    Abstract A high friction coefficient and a low wear rate of contacted surfaces are essential elements to friction pairs between the stator and the rotor in ultrasonic motors.It has been shown that surface textures have a significant effect on improving the tribological performance of friction pairs.In this paper,microgroove arrays are introduced to the stator surface for improving the tribological performance of friction pairs between the stator and the rotor in ultrasonic motors.Microgrooves were fabricated on a phosphor bronze surface by through-mask electrochemical micromachining(TMEMM).Parameters,namely,the electrolyte inlet pressure,applied voltage,pulse duty cycle,and frequency,were varied to investigate their influences on the dimensions and morphology of the microgrooves.Results showed that the width and depth of the microgrooves were strongly affected by the applied voltage and frequency,while the morphology of the microgrooves was dependent on the electrolyte inlet pressure and the pulse duty cycle.Compared with a smooth surface,the friction coefficient increased from 0.245 to 0.334 and less abrasion was obtained when a surface was textured with microgrooves of which the width and depth were 185.6 and 57.6 μm,respectively.Microgroove arrays might play an important role in enhancing the performance of ultrasonic motors.

    1.Introduction

    Precision transmission components are essential to the performance of high-end equipment.Ultrasonic motors,as such a kind of components,have become widely used in medical equipment,semiconductor manufacturing,aerospace engineering,and other fields due to their excellent characteristics like a light weight,a large output torque,a rapid response speed,etc.An ultrasonic motor is typically driven by the ultrasonic vibration of an elastic stator,which is stimulated by piezoelectric ceramics and then transformed to an output force through the dry friction force between the rotor(or slider)and the stator.1The friction coefficient and the wear rate are two key measurements of the friction pairs’properties in ultrasonic motors,as the magnitude of the output torque and the working efficiency both increase with an increasing friction coefficient,and greater operating stability with a longer service life can be achieved at lower wear rates.2Till now,studies of enhancing and optimizing the performance of friction pairs in ultrasonic motors have mainly been focused on the choice and development of different materials.For example,Qiu et al.1investigated the main wear mechanisms and finally found the most promising material after testing four different engineering ceramics in an ultrasonic motor configuration.Li et al.3explored the wear process and the wear properties of contact surfaces between brass and PTFE-matrix composite at different wear stages in a traveling-wave ultrasonic motor.In order to choose the most suitable composite for practical applications,Qu et al.4conducted a comparative study of three kinds of polymer composites with duralumin stators for wear behaviors under different environmental conditions.However,an optimal choice of materials can only improve the tribological performance to a limited extent,and the cost of such materials is often very high.Therefore,it is of great importance to explore new methods to increase the friction coefficient while simultaneously decreasing the wear rate of the friction pair surfaces in ultrasonic motors.

    Surface texturing is an advanced technical means to improve the tribological performances of different contacted or moving friction pair surfaces.It has been widely used in the fields of aviation,machining,automobile manufacture,biomedicine,etc.In this technique,arrays of grooves,dimples,or pillars of appropriate sizes are generated on a workpiece surface.5The presence of such arrays shows notable effects by entrapping microscale grinding grains and reducing abrasive wear and furrows during a dry friction process.Surface textures,especially microgroove arrays,can meet the goals of increasing the friction coefficient while decreasing the wear rate.Song et al.6fabricated stripes on the surface of cast iron and verified that the abrasion resistance was more than doubled,and the friction coefficient was increased by 66%compared to the same material with a smooth surface.He et al.7reported that increasing the size of microgrooves on a poly(dimethyl siloxane)(PDMS)surface led to a higher friction coefficient.However,little research on ameliorating the tribological performance of ultrasonic motors by using the surface texturing technology has been reported.This paper proposes a method to increase the friction coefficient and decrease the wear rate of friction pairs in ultrasonic motors by applying microgroove arrays on the stator surface.

    Different ways of fabricating microgrooves have been found in recent years,such as microgrinding,8electrodischarge machining (EDM),9chemicaletching,10laser machining,11micro-abrasive jet machining(MAJM),12and electrochemical machining(ECM).13ECM is a material removal process based on an electrochemical reaction between the electrodes in an electrolytic cell.It shows significant advantages over most other machining methods in terms of the absences of cutting forces and tool wear and the fact that it does not generate any residual stress or a heat-affected zone in the material of a workpiece.14Over the years,there have been a number of investigations of microgrooves fabricated by ECM.Lee et al.15compared two types of electrolyte,aqueous sodium nitrate and aqueous sodium chloride,in an ECM process,and a better morphology of microgrooves was obtained in the former one.Liu et al.16manufactured microring grooves on the inner face of a metallic cylinder by pulse electrochemical sawing micro-machining.During this machining process,a rotational dentate cathode was applied to promote a uniform distribution of the electrolyte and facilitate the removal of electrolytic products.Rathod et al.17developed a tungsten microtool to fabricate microgrooves on stainless steel by ECM and studied various parameters affecting machining results.Lee et al.18simulated the electrolytic flow and then selected an operational parameter to generate microscale grooves of 200 μm in depth and 500 μm in width on SS316 stainless steel sheets.Natsu et al.19fabricated microgrooves on both a plate and a cylinder by electrolyte jet machining and found that the groove width remained the same while the depth varied with changes of the nozzle’s moving speed.Ghoshal and Bhattacharyya20fabricated complex microgrooves of‘U”and ‘S” shapes on SS-304 stainless steel by micro-electrochemical sinking and milling along the paths of micro features.Chen et al.21applied an electrolyte system with double nozzles to reduce the corner radius and taper of the side walls of microgrooves.However,in most of these studies,grooves were fabricated one by one with a reciprocating motion of the cathode of which the working efficiency was low.

    Through-mask electrochemical micromachining(TMEMM)is a common method adopted to machine surface texture in ECM.In TMEMM,a workpiece is covered with a patterned mask prepared by a lithographic process.When the electrolyte flows into the pattern,the exposed region is removed by electrochemical dissolution.With this method,a large number of microgrooves can be generated at the same time,which greatly increases the working efficiency.Research on fabricating micro-dimples by TMEMM has been widely reported,22–24although this technique is rarely used for machining microgrooves.

    It has been shown that the dissolution law varies greatly among different materials in an ECM process.Machining of stainless steel,25titanium alloy,26copper,27and other metallic materials has been studied,while there has been no report of any investigation of machining of phosphor bronze,a common material for friction pairs in ultrasonic motors.In this paper,the rotor and stator materials of the friction pairs were polyimide and phosphor bronze,respectively.Microgrooves were fabricated on the surface of phosphor bronze by TMEMM.Different machining parameters,namely,the electrolyte inlet pressure,applied voltage,pulse duty cycle,and frequency,which may influence results greatly,were investigated.The friction coefficients of both smooth and textured surfaces were obtained from a pin-on-disk dry friction test.The wear morphologies of the corresponding pins were also investigated to determine their effects on decreasing the wear rate of the contacted friction pair surfaces.

    2.Analysis of electric field and current density

    To investigate the profile of microgrooves in TMEMM,a mathematical model is set up,as shown in Fig.1,whereW0is the width of each microgroove on the mask,Gis the distance between the anode and the cathode,andH0is the thickness of the mask.

    The electric potential,φ,in the inter-electrode gap can be approximately described by Laplace’s equation as

    The boundary conditions are as follows:

    whereUis the applied voltage and n is the unit normal vector of surface.

    The current density,i,can be expressed by

    where κ is the conductivity of the electrolyte.In this paper,the COMSOL Multiphysics package was used to simulate the current density distribution over the workpiece surface under the following conditions: κ =10 S/m,G=2 mm,H0=50 μm,andW0=110 μm.The simulation results on the current density distribution at different applied voltages are shown in Fig.2.It can be seen that the current density increases with increasing applied voltage.Moreover,the maximum current density occurs at the edge of a microgroove and decreases to the center(see Fig.3).

    According to Faraday’s Law,the volume of material removed during the machining process can be calculated as

    where η is the current efficiency,ω is the volumetric electrochemical equivalent of the material(mm3/(A·s)),Iis the mean current intensity(A),andtis the machining time(s).Thus,the profiles of microgrooves can be predicted,and a central peak might be formed at the bottom of a microgroove.

    Fig.1 Electric potential distribution in the inter-electrode gap.

    Fig.2 Current density distribution at different applied voltages.

    Fig.3 Current density norm at an applied voltage of 25 V.

    3.Experimental procedures

    3.1.Electrochemical machining

    The experimental system is schematically shown in Fig.4.It consists of an electrolyte-circulating system,a power supply,electrodes,a PC-based digital acquisition system(PC-DAQ),and a time switch.Phosphor bronze samples with a diameter of 34 mm and a thickness of 5 mm were applied as the anodic workpiece for the machining process.The chemical composition of phosphor bronze is listed in Table 1.The samples were polished to a surface roughness of 0.16 μm and cleaned with absolute ethanol before experiments.

    Fig.4 Experimental system set-up.

    Table 1 Chemical composition of phosphor bronze.

    The machining process involved two steps.The first was lithography.A dry film(GPM220;DuPont,USA),which was a negative photoresist with a thickness of 50 μm,was employed as a mask,with patterned microgrooves being produced by a photolithographic procedure involving lamination,exposure,and development.Microgrooves with a width of 110 μm and a center distance of 667 μm were obtained on the mask.

    The second step was the ECM itself,in which the gap between electrodes was 2 mm.Fig.5 shows a schematic diagram of the TMEMM process.The electrolyte,sodium nitrate(NaNO3)solution,was at a concentration of 100 g/L and a temperature of 28°C, flowing along the patterned microgrooves on the workpiece surface.Back pressure was also introduced to make the electrolyte flow through the bottoms of the microgrooves and remove the electrolysis products from the working area completely.Thefixture’s detailed structure and the developed flow channel for the electrolyte are shown in Fig.6.The profiles of the microgrooves were measured by a three-dimensional profilometer(DVM5000;Leica,Germany)and a scanning electron microscope(SEM)(S-3400 N;Hitachi,Japan).

    The parameters of the microgrooves(see Fig.7)are calculated as follows.The average width of the microgrooves is

    whereWiis the microgroove width at theith measurement.The average depth of the microgrooves is

    whereHiis the microgroove depth at theith measurement.

    The standard deviations of the microgrooves’width and depth are

    SWandSHquantify the amount of dispersions of width and depth,and lower values are preferred to obtain a higher machining accuracy.In Eqs.(8)–(11),Nis the total number of measured microgrooves;in this experiment,N=30.

    The area ratio of microgrooves is

    Fig.5 Schematic of the TMEMM process.

    whereLis the distance between the microgrooves.The machining localization is

    whereW0=110 μm.EFevaluates the degree of lateral etching of microgrooves,and higher values are preferred.

    3.2.Friction tests

    In order to examine the friction performance of the microgroove array on the phosphor bronze samples,comparative dry friction tests on surfaces with and without microgrooves were carried out on a friction tester(HSR-2 M,China).A pin-on-disk friction test was used to simulate the working condition of the ultrasonic motor,in which the square pin was made of polyimide with a width of 8 mm and the disk was a machined phosphor bronze sample.The sliding direction was perpendicular to the microgrooves,and the length was 16 mm,with a motor speed of 300 r/min.Each friction test was conducted for 30 min at a normal load of 120 N,which was calculated according to the working status of the ultrasonic motor.In order to ensure the stability of the testing system,the load was detected and controlled by load cells.

    4.Results and discussion

    The electrolyte inlet pressure,P,applied voltage,U,pulse duty cycle,D,and frequency,f,were varied to reveal their effects on the electrochemical machining of microgrooves on phosphor bronze.The machining parameters and results are given in Table 2.

    4.1.Effect of the electrolyte inlet pressure on microgrooves

    The electrolyte inlet pressure affects the machining results to a certain extent.It is important to choose an appropriate value for this pressure before evaluating the effects of other parameters.According to our previous investigation on generating micro-dimple arrays,parameters with a voltage of 20 V,a frequency of 0.12 kHz,and a duty cycle of 20%were applied.14Fig.8 shows the changes in the width and depth of microgrooves generated at inlet pressures of 0.1,0.2,0.3,and 0.4 MPa and an effective machining time of 10 s.Standard deviations of the width are 2.64,2.43,1.83,and 1.83 μm,while the depth standard deviations are 1.88,1.66,1.33,and 1.32 μm,respectively.There is no obvious change in the sizes of the microgrooves,which ranges from 175.0 to 180.5 μm in width and from 44.5 to 45.7 μm in depth.profiles of the microgrooves in Fig.9 shows that a smoother bottom can be achieved in microgrooves generated at an inlet pressure of 0.3 and 0.4 MPa instead of 0.1 and 0.2 MPa.A similar conclu-sion can also be drawn by the standard deviations of microgrooves’width and depth.In TMEMM,machining products block the electrochemical reaction and greatly affect the uniformity of machining once they accumulate at the bottom of microgrooves.With the application of a high electrolyte inlet pressure,machining products can be removed from the electrolyte easily,and microgrooves with smooth bottoms can be obtained.Compared with an inlet pressure of 0.4 MPa,the sealing performance of thefixture might be maintained more easily at an inlet pressure of 0.3 MPa.Thus,an electrolyte inlet pressure of 0.3 MPa is appropriate for generating microgrooves by TMEMM.

    Fig.6 Detailed structure of thefixture.

    Fig.7 Schematic diagram showing the definitions of the parameters.

    4.2.Effect of the applied voltage on microgrooves

    It has been verified that the machining voltage exerts a great influence on machining results in TMEMM.24Experiments 3 and 5–7 were conducted to identify the effects of the applied voltage on microgrooves.Fig.10 plots the variations in the width and depth of the microgrooves at applied voltages of 10,15,20,and 25 V,a frequency of 0.12 kHz,a duty cycle of 20%,an electrolyte inlet pressure of 0.3 MPa,and an effective machining time of 10 s.It is obvious that the width and depth of the microgrooves increase with an increase of the applied voltage.A high applied voltage leads to a high current intensity,which increases the volume of material removed according to Eq.(7).In addition,Fig.11(a)shows that a central peak remains at the bottom of a microgroove when the applied voltage is 10 V.According to the simulation results,a higher current density occurs at the edge other than the center of the electric field,and therefore the edge material removal volume is larger.However,when the applied voltage exceeds 15 V,the central peak disappears,and smooth microgrooves can be obtained(see Fig.11(b)–(d)).This can be explained by the fact that at a high applied voltage,the current density is way too high at the edge of the electric field,which results in a creation of excessive amounts of machining products(see Fig.12).Therefore,the electrical resistance increases at the edge and uniforms the distribution of the current density.Finally,microgrooves with smooth morphology are obtained.

    Table 2 Machining parameters and results.

    Fig.8 Effect of electrolyte inlet pressure on width and depth of microgrooves.

    Usually,machining products need to be removed timely for improving the machining accuracy in ECM.However,in this paper,a new method is proposed to generate smooth microgrooves with an accumulation of machining products.Furthermore,it can be seen that the machining localization EF is enhanced,as shown in Fig.13.This is because the mask limits the lateral etching of the material while the microgroove depth still increases with increasing applied voltage.

    4.3.Effect of the pulse duty cycle on microgrooves

    To investigate the effects of pulse parameters on microgrooves machining,experiments with various pulse duty cycles were performed.Considering the capacity of our developed current acquisition system,experiments were conducted at a voltage of 15 V,a frequency of 0.12 kHz,an electrolyte inlet pressure of 0.3 MPa,and an effective machining time of 10 s.Fig.14 plots changes in the width and depth of microgrooves generated at different pulse duty cycles.The dimensions of the microgrooves vary little with increasing pulse duty cycle,ranging from 164.1 to 167.9 μm in width and from 33.8 to 37.0 μm in depth.However,there is an obvious variation in their threedimensional topography(see Fig.15).The standard deviations of microgrooves’width and depth are the smallest at a pulse duty cycle of 20%,so that the bottoms of these microgrooves are the smoothest.Since the pulse interval time is longer at a pulse duty cycle of 20%than those of any other pulse duty cycles,machining productscan be removed thoroughly through the flowing electrolyte.Therefore,a pulse duty cycle of 20%is suitable for generating microgrooves with a highquality three-dimensional topography.

    Fig.10 Effect of applied voltage on width and depth of microgrooves.

    4.4.Effect of the frequency on microgrooves

    The effect of the frequency during TMEMM with a dry- film mask was investigated.Figs.16 and 17 respectively show variations in the dimensions and machining localizationEFof microgrooves generated at frequencies of 0.12,2,4,and 6 kHz,an applied voltage of 20 V,a duty cycle of 20%,an effective machining time of 10 s,and an electrolyte inlet pressure of 0.3 MPa.The width and depth of the microgrooves decrease while the machining localization grows with increasing frequency.Furthermore,the microgroove morphology becomes poor at high frequencies(see Fig.18).In order to illustrate this phenomenon,the current signal was collected during the machining process by the PC-DAQ and is shown in Fig.19.It is evident that the current decreases with increasing frequency.At a high frequency,the pulse interval time is too short to update the electrolyte in a single pulse duty cycle,which blocks the removal of machining products.The resulting accumulation of these products leads to an increased electrical resistance during machining,and therefore the current intensity decreases.According to Eq.(7),the volume of material removed decreases and shows a reduction of the microgrooves’dimensions.Meanwhile,the accumulated products are nonuniform,so that the dissolution of each area is uneven.As a result,microgrooves’morphology becomes poor,and the bottoms are no longer smooth.Similar conclusions regarding reduced width and depth were obtained in a previous report on the influences of the pulse frequency on machining accuracy and surfacefinish.17

    Fig.9 profiles of microgrooves generated at different inlet pressures.

    Fig.11 profiles of microgrooves generated at different applied voltages.

    Fig.12 Distribution of reaction products with high applied voltages.

    Fig.13 Effect of the applied voltage on machining localization EF.

    4.5.Friction properties

    It was found that the friction coefficient varied little with a change of the microgrooves’depths,but was affected greatly by the area ratio in our previous investigation.A high friction coefficient could be obtained with a microgroove area ratio over 20%.28,29specifically,in the friction tests of this paper,microgrooves of different widths and the average depth about 58 μm at an area ratio of about 25%were machined with the optimized machining parameters:an electrolyte inlet pressure of 0.3 MPa,an applied voltage of 20 V,a duty cycle of 20%,a frequency of 0.12 kHz,and an effective machining time of 10 s.Fig.20 shows a typical SEM image of a machined workpiece with microgrooves.

    Fig.14 Effect of pulse duty cycle on width and depth of microgrooves.

    The results of friction tests are shown in Table 3.It can be seen that the friction coefficients of surfaces with microgroove arrays are greater than that of a smooth surface,which is only about 0.245.The highest friction coefficient,0.334,is obtained when the average width of microgrooves is 188.6 μm.That is,the distance between the microgrooves is 750 μm.Fig.21 shows the optical images of wear track on the phosphor bronze surface.No obvious difference can be observed between surfaces with and without microgrooves.Since the hardness of polyimide is lower than that of phosphor bronze,polyimide was worn and adhered on the surface of phosphor bronze(see the gray zone in Fig.21).Therefore,the wear morphology of pins can be observed after the friction tests.SEM images of the corresponding pin surfaces are shown in Fig.22.A large area of material is detached from the substrate surface,and severe abrasion can be seen when a pin is rubbed with an untextured phosphor bronze surface.However,less abrasion and a better wear morphology of the pin surface are obtained when a pin is rubbed with a microgrooved surface.This can be attributed to the microgroove arrays.During a dry friction process,solid-solid contact inevitably occurs owing to the roughness and inaccurate morphology of contacted surfaces,which produces wear particles and promotes wear30(see Fig.22(b)).However,when the surface is textured,wear particles are captured into microgrooves,resulting in a reduction of abrasive wear(see Fig.22(c)–(f)).Thus,microgroove arrays have a beneficial effect on decreasing the wear rate while increasing the friction coefficient.Microgroove arrays can thus improve the magnitude of the output torque and service life of ultrasonic motors.

    Fig.15 profiles of microgrooves generated at different pulse duty cycles.

    Fig.16 Effect of frequency on width and depth of microgrooves.

    Fig.17 Effect of frequency on the machining localization EF.

    Fig.18 profiles of microgrooves generated at different frequencies.

    Fig.19 Current signal at different frequencies.

    Fig.20 SEM image of microgrooves machined with the optimized parameters.

    Table 3 Friction coefficients of surfaces with different widths of microgrooves.

    Fig.22 SEM images of pin surfaces under different conditions.

    5.Conclusions

    This paper has described an experimental investigation of a procedure for generating microgrooves on phosphor bronze material,in which the effects of different machining parameters were studied.Microgrooves ranging from 148.5 to 258.6 μm in width and from 17.6 to 58.0 μm in depth were successfully fabricated by TMEMM.Friction tests were also carried out.The following conclusions can be drawn from experimental results:

    (1)A high inlet pressure and a low pulse duty cycle have the advantageofimproving themorphology ofthe microgrooves.

    (2)The width and depth of the microgrooves were greatly affected by the applied voltage and the frequency.Moreover,a new method was proposed to generate smooth microgrooves with the accumulation of machining products.

    (3)High-quality microgroove arrays can be well achieved with optimized machining parameters:an electrolyte inlet pressure of 0.3 MPa,an applied voltage of 20 V,a duty cycle of 20%,and a frequency of 0.12 kHz.

    (4)Compared with a smooth surface,the friction coefficient increased from 0.245 to 0.334 and less abrasion was obtained when a surface was textured with microgrooves of which the width and depth were 185.6 and 57.6 μm,respectively.Microgroove arrays exhibit a good application prospect in improving the tribological performance of friction pairs in ultrasonic motors.

    Acknowledgements

    The work described in this study was supported by the National Basic Research Program of China(973 Program,No.2015CB057502)and the Fundamental Research Funds for the Central Universities(No.NZ2016106).

    国产精品成人在线| 国产av一区二区精品久久| 久久国产亚洲av麻豆专区| 观看美女的网站| 最新的欧美精品一区二区| 亚洲精品一区蜜桃| 侵犯人妻中文字幕一二三四区| 又粗又硬又长又爽又黄的视频| 亚洲在久久综合| 亚洲伊人色综图| 亚洲成人手机| 黄网站色视频无遮挡免费观看| 午夜91福利影院| 热re99久久国产66热| 99久国产av精品国产电影| 欧美 亚洲 国产 日韩一| 男男h啪啪无遮挡| 国产片特级美女逼逼视频| 老熟女久久久| 青春草视频在线免费观看| 亚洲成色77777| 叶爱在线成人免费视频播放| 欧美黑人欧美精品刺激| 秋霞伦理黄片| 蜜桃在线观看..| 中文字幕人妻丝袜制服| 纵有疾风起免费观看全集完整版| 波野结衣二区三区在线| 久热爱精品视频在线9| 天堂8中文在线网| 少妇被粗大猛烈的视频| 国产在视频线精品| 国产99久久九九免费精品| 可以免费在线观看a视频的电影网站 | 免费久久久久久久精品成人欧美视频| 飞空精品影院首页| 国产高清国产精品国产三级| 免费高清在线观看视频在线观看| 大陆偷拍与自拍| 午夜福利乱码中文字幕| 成年人午夜在线观看视频| 中文字幕高清在线视频| 天天躁日日躁夜夜躁夜夜| 精品一区二区三区av网在线观看 | av国产久精品久网站免费入址| 人人澡人人妻人| 国产1区2区3区精品| 黄色毛片三级朝国网站| 黄色视频在线播放观看不卡| 中文字幕亚洲精品专区| 国产又爽黄色视频| 精品少妇黑人巨大在线播放| 人体艺术视频欧美日本| 免费女性裸体啪啪无遮挡网站| 老鸭窝网址在线观看| 啦啦啦啦在线视频资源| 免费少妇av软件| 久久婷婷青草| 搡老岳熟女国产| 国产精品一国产av| 国产不卡av网站在线观看| 青春草视频在线免费观看| 三上悠亚av全集在线观看| 9热在线视频观看99| 热99国产精品久久久久久7| 国产精品嫩草影院av在线观看| 秋霞在线观看毛片| 国产精品久久久久久精品古装| 国产xxxxx性猛交| 国产伦理片在线播放av一区| 大陆偷拍与自拍| 精品国产露脸久久av麻豆| 久久99精品国语久久久| 超色免费av| 涩涩av久久男人的天堂| 久久 成人 亚洲| 丝袜美足系列| 又黄又粗又硬又大视频| 蜜桃国产av成人99| 美女午夜性视频免费| 日韩电影二区| 人人妻,人人澡人人爽秒播 | 国产日韩一区二区三区精品不卡| 精品少妇久久久久久888优播| 亚洲综合精品二区| 亚洲熟女毛片儿| 免费少妇av软件| 99国产精品免费福利视频| 美女脱内裤让男人舔精品视频| 色94色欧美一区二区| 亚洲国产精品999| 亚洲男人天堂网一区| 伦理电影大哥的女人| 亚洲中文av在线| 国产一区二区三区综合在线观看| 美女高潮到喷水免费观看| videosex国产| 久久国产精品大桥未久av| 免费观看人在逋| 亚洲精品久久成人aⅴ小说| 久久久欧美国产精品| 久久鲁丝午夜福利片| 美女高潮到喷水免费观看| 久久精品人人爽人人爽视色| 国产一卡二卡三卡精品 | 在线观看免费视频网站a站| 亚洲四区av| 高清av免费在线| 99国产综合亚洲精品| 视频在线观看一区二区三区| 制服诱惑二区| 日韩一卡2卡3卡4卡2021年| 国产精品免费大片| 午夜福利乱码中文字幕| 日本欧美视频一区| 亚洲久久久国产精品| 伊人亚洲综合成人网| 欧美日韩福利视频一区二区| 一区二区av电影网| 亚洲精品国产一区二区精华液| 色视频在线一区二区三区| 欧美人与性动交α欧美软件| 免费看av在线观看网站| 亚洲熟女毛片儿| 九九爱精品视频在线观看| 熟妇人妻不卡中文字幕| 成人午夜精彩视频在线观看| 高清av免费在线| 黑人猛操日本美女一级片| 一区二区三区乱码不卡18| 麻豆精品久久久久久蜜桃| 波多野结衣av一区二区av| www.av在线官网国产| 一级,二级,三级黄色视频| 一本—道久久a久久精品蜜桃钙片| 人人澡人人妻人| 亚洲熟女毛片儿| 成人午夜精彩视频在线观看| 国产女主播在线喷水免费视频网站| 亚洲第一区二区三区不卡| 在线观看免费午夜福利视频| www.熟女人妻精品国产| 久久精品国产a三级三级三级| 亚洲第一区二区三区不卡| 丰满乱子伦码专区| 新久久久久国产一级毛片| 国产成人精品久久二区二区91 | 黄片播放在线免费| 午夜福利视频在线观看免费| 如日韩欧美国产精品一区二区三区| 欧美精品av麻豆av| 极品少妇高潮喷水抽搐| av在线观看视频网站免费| 国产av国产精品国产| 新久久久久国产一级毛片| 欧美精品人与动牲交sv欧美| 毛片一级片免费看久久久久| 午夜福利一区二区在线看| 国产一区二区三区av在线| 丝袜美足系列| 熟女av电影| 国产精品秋霞免费鲁丝片| 超碰成人久久| 国产一区二区三区综合在线观看| 国产成人欧美在线观看 | 十分钟在线观看高清视频www| 亚洲婷婷狠狠爱综合网| 美女中出高潮动态图| av在线观看视频网站免费| 精品少妇内射三级| 亚洲精华国产精华液的使用体验| 最新在线观看一区二区三区 | 欧美成人精品欧美一级黄| 色网站视频免费| xxx大片免费视频| 性色av一级| 性高湖久久久久久久久免费观看| 午夜激情久久久久久久| 久久人人97超碰香蕉20202| 制服丝袜香蕉在线| 啦啦啦在线免费观看视频4| 无遮挡黄片免费观看| 亚洲精品自拍成人| netflix在线观看网站| avwww免费| 观看av在线不卡| 毛片一级片免费看久久久久| 尾随美女入室| 熟女少妇亚洲综合色aaa.| 亚洲精品在线美女| 交换朋友夫妻互换小说| 99九九在线精品视频| 国产日韩欧美在线精品| 成人国产麻豆网| a级毛片黄视频| 精品人妻熟女毛片av久久网站| 桃花免费在线播放| 黄网站色视频无遮挡免费观看| 亚洲人成77777在线视频| 午夜激情久久久久久久| 黄色 视频免费看| 肉色欧美久久久久久久蜜桃| 高清不卡的av网站| 成年动漫av网址| 免费观看a级毛片全部| 欧美国产精品va在线观看不卡| 亚洲第一青青草原| 色吧在线观看| 亚洲欧美精品综合一区二区三区| 国产熟女欧美一区二区| 大码成人一级视频| 国产成人欧美| 亚洲欧美精品自产自拍| 9191精品国产免费久久| 亚洲第一青青草原| 亚洲欧洲日产国产| 国产成人系列免费观看| 亚洲一卡2卡3卡4卡5卡精品中文| 一边摸一边做爽爽视频免费| 女性生殖器流出的白浆| 黑人欧美特级aaaaaa片| 精品一品国产午夜福利视频| 日韩一卡2卡3卡4卡2021年| 欧美成人午夜精品| 亚洲av日韩在线播放| 日韩成人av中文字幕在线观看| 精品亚洲成国产av| av福利片在线| 丰满饥渴人妻一区二区三| 叶爱在线成人免费视频播放| 久久久久精品国产欧美久久久 | av国产久精品久网站免费入址| 18禁国产床啪视频网站| 亚洲国产中文字幕在线视频| 国产亚洲av片在线观看秒播厂| 免费高清在线观看视频在线观看| 五月天丁香电影| 日韩熟女老妇一区二区性免费视频| 亚洲伊人久久精品综合| 青春草国产在线视频| 九草在线视频观看| av一本久久久久| 亚洲精品一区蜜桃| 国产欧美日韩综合在线一区二区| 亚洲欧美日韩另类电影网站| 高清黄色对白视频在线免费看| 中文字幕av电影在线播放| 成人午夜精彩视频在线观看| 亚洲av男天堂| 日韩制服丝袜自拍偷拍| 制服诱惑二区| 国产亚洲av高清不卡| 在线天堂最新版资源| 看免费av毛片| 亚洲男人天堂网一区| 高清av免费在线| av中文乱码字幕在线| 午夜精品在线福利| 在线观看66精品国产| 免费看美女性在线毛片视频| 久久 成人 亚洲| 18禁国产床啪视频网站| 国产精品久久电影中文字幕| 亚洲欧美日韩无卡精品| av片东京热男人的天堂| 亚洲av成人不卡在线观看播放网| 午夜福利视频1000在线观看 | 国产色视频综合| 成人国产综合亚洲| 亚洲精品中文字幕一二三四区| 可以在线观看毛片的网站| avwww免费| 欧美黄色淫秽网站| 精品人妻1区二区| 国产熟女午夜一区二区三区| 激情视频va一区二区三区| 免费高清在线观看日韩| 很黄的视频免费| 国产亚洲精品久久久久久毛片| 亚洲中文av在线| 九色国产91popny在线| 中文字幕人成人乱码亚洲影| 国产成人欧美在线观看| 波多野结衣高清无吗| 波多野结衣一区麻豆| 天天一区二区日本电影三级 | 丁香六月欧美| 老汉色av国产亚洲站长工具| 久久人妻av系列| 人人妻人人澡欧美一区二区 | 午夜免费成人在线视频| 波多野结衣一区麻豆| 黑人巨大精品欧美一区二区mp4| 午夜福利免费观看在线| 丁香六月欧美| 亚洲精品国产精品久久久不卡| 久久午夜综合久久蜜桃| 一进一出好大好爽视频| 黄色丝袜av网址大全| 美女午夜性视频免费| 亚洲人成伊人成综合网2020| 天天躁夜夜躁狠狠躁躁| 国产国语露脸激情在线看| 亚洲一区二区三区色噜噜| 亚洲精品久久国产高清桃花| 亚洲欧美精品综合一区二区三区| 亚洲国产欧美一区二区综合| 九色亚洲精品在线播放| 高清黄色对白视频在线免费看| 精品国产国语对白av| 天堂√8在线中文| 欧美大码av| 男女做爰动态图高潮gif福利片 | 亚洲精品在线观看二区| 极品人妻少妇av视频| 日韩免费av在线播放| 电影成人av| 美国免费a级毛片| АⅤ资源中文在线天堂| 怎么达到女性高潮| 亚洲熟妇熟女久久| 国产aⅴ精品一区二区三区波| 一a级毛片在线观看| 久久精品国产99精品国产亚洲性色 | 亚洲国产毛片av蜜桃av| e午夜精品久久久久久久| 精品电影一区二区在线| cao死你这个sao货| 国产精品99久久99久久久不卡| 久久精品国产亚洲av高清一级| 香蕉久久夜色| 久久人妻熟女aⅴ| 一区二区三区国产精品乱码| 成人亚洲精品一区在线观看| 一区二区三区国产精品乱码| 亚洲av电影在线进入| 一级毛片精品| 亚洲av电影在线进入| 男男h啪啪无遮挡| www.999成人在线观看| 国产在线精品亚洲第一网站| 亚洲视频免费观看视频| 国产在线精品亚洲第一网站| 免费高清视频大片| 日日摸夜夜添夜夜添小说| 国产欧美日韩精品亚洲av| 黄片播放在线免费| 人人妻人人爽人人添夜夜欢视频| 中文字幕久久专区| 国产精品九九99| 国产99久久九九免费精品| 亚洲熟妇中文字幕五十中出| 丁香六月欧美| 国产一区二区三区在线臀色熟女| 搡老熟女国产l中国老女人| 久久久久久大精品| 香蕉久久夜色| 亚洲七黄色美女视频| 天天一区二区日本电影三级 | 久久久久久免费高清国产稀缺| 日韩高清综合在线| 999久久久精品免费观看国产| 久久性视频一级片| 麻豆久久精品国产亚洲av| 亚洲成av人片免费观看| 久久久久久人人人人人| 中文字幕人妻熟女乱码| 亚洲全国av大片| 热99re8久久精品国产| 好男人电影高清在线观看| 三级毛片av免费| www.自偷自拍.com| 亚洲人成伊人成综合网2020| 欧美av亚洲av综合av国产av| 亚洲国产中文字幕在线视频| 亚洲成人国产一区在线观看| 人妻丰满熟妇av一区二区三区| 中文字幕人妻丝袜一区二区| 怎么达到女性高潮| 久久久久久大精品| 一本大道久久a久久精品| 日韩欧美免费精品| 757午夜福利合集在线观看| 国产成人精品久久二区二区91| 757午夜福利合集在线观看| 69av精品久久久久久| 激情在线观看视频在线高清| 电影成人av| 精品少妇一区二区三区视频日本电影| 男人的好看免费观看在线视频 | 国产精品99久久99久久久不卡| 亚洲精华国产精华精| 老司机在亚洲福利影院| 亚洲五月婷婷丁香| 一区二区三区高清视频在线| 热99re8久久精品国产| 精品人妻1区二区| 在线av久久热| 欧美黑人精品巨大| 精品第一国产精品| 亚洲精品粉嫩美女一区| 女人爽到高潮嗷嗷叫在线视频| 久久中文字幕人妻熟女| 国产精品国产高清国产av| 国产精品久久久久久人妻精品电影| 97人妻天天添夜夜摸| 在线观看午夜福利视频| 亚洲成人久久性| 三级毛片av免费| 最好的美女福利视频网| 美女扒开内裤让男人捅视频| 精品乱码久久久久久99久播| 日日摸夜夜添夜夜添小说| 免费高清在线观看日韩| 欧美激情久久久久久爽电影 | 亚洲国产欧美日韩在线播放| 老司机午夜十八禁免费视频| 国产真人三级小视频在线观看| 成人三级做爰电影| 黄片小视频在线播放| 高潮久久久久久久久久久不卡| 国产精品九九99| 韩国av一区二区三区四区| 日本a在线网址| 九色亚洲精品在线播放| 久久午夜亚洲精品久久| 亚洲精品在线观看二区| 亚洲av电影不卡..在线观看| 国产私拍福利视频在线观看| 久久影院123| 国产高清激情床上av| xxx96com| 亚洲av电影在线进入| 超碰成人久久| 99riav亚洲国产免费| 亚洲国产欧美日韩在线播放| 亚洲免费av在线视频| 男人舔女人下体高潮全视频| 两个人看的免费小视频| 国产一区二区激情短视频| 久久久久久久久中文| 一夜夜www| 国产精品1区2区在线观看.| 黄片大片在线免费观看| 日本免费一区二区三区高清不卡 | 成人三级黄色视频| 日韩欧美国产在线观看| 国产精品日韩av在线免费观看 | 久久久久国内视频| 午夜视频精品福利| 亚洲成a人片在线一区二区| 国产激情欧美一区二区| 国产免费av片在线观看野外av| 欧美久久黑人一区二区| 亚洲中文av在线| 国产免费男女视频| 这个男人来自地球电影免费观看| 女人被躁到高潮嗷嗷叫费观| 日本vs欧美在线观看视频| 久久狼人影院| 日韩大尺度精品在线看网址 | 国产精品98久久久久久宅男小说| 久久九九热精品免费| 午夜福利高清视频| 女人精品久久久久毛片| 国产欧美日韩一区二区三| 中文字幕最新亚洲高清| 色综合站精品国产| 欧美日韩瑟瑟在线播放| 亚洲成av人片免费观看| 国产三级在线视频| 亚洲精品国产色婷婷电影| 啦啦啦 在线观看视频| 欧美乱色亚洲激情| 在线观看午夜福利视频| 韩国精品一区二区三区| 国产精品久久电影中文字幕| 变态另类丝袜制服| 国产免费男女视频| 国产亚洲av嫩草精品影院| 波多野结衣高清无吗| 国产亚洲欧美精品永久| 亚洲av成人av| 亚洲一区二区三区不卡视频| www.www免费av| 自线自在国产av| 99久久综合精品五月天人人| 午夜福利,免费看| 国产亚洲精品综合一区在线观看 | 国内毛片毛片毛片毛片毛片| 在线观看免费视频日本深夜| 热99re8久久精品国产| 国产不卡一卡二| 亚洲欧美日韩高清在线视频| 亚洲性夜色夜夜综合| 亚洲va日本ⅴa欧美va伊人久久| 又大又爽又粗| 国产精品久久久久久亚洲av鲁大| 日本三级黄在线观看| 免费高清视频大片| 天天一区二区日本电影三级 | 欧美日本亚洲视频在线播放| 国内久久婷婷六月综合欲色啪| 亚洲精品美女久久久久99蜜臀| netflix在线观看网站| 亚洲五月天丁香| 久久久久久免费高清国产稀缺| 亚洲成a人片在线一区二区| 日韩欧美一区二区三区在线观看| 热re99久久国产66热| av视频在线观看入口| 国产午夜福利久久久久久| 国产97色在线日韩免费| 在线免费观看的www视频| 91九色精品人成在线观看| 视频在线观看一区二区三区| 波多野结衣高清无吗| 久久伊人香网站| 亚洲中文av在线| 老熟妇乱子伦视频在线观看| 在线观看日韩欧美| 国产不卡一卡二| 国产激情欧美一区二区| 亚洲黑人精品在线| 女人被躁到高潮嗷嗷叫费观| 一卡2卡三卡四卡精品乱码亚洲| 老汉色av国产亚洲站长工具| 757午夜福利合集在线观看| 麻豆国产av国片精品| 国产真人三级小视频在线观看| 怎么达到女性高潮| 国产成人精品无人区| 老汉色∧v一级毛片| 精品无人区乱码1区二区| 日韩欧美一区视频在线观看| 麻豆一二三区av精品| 最近最新免费中文字幕在线| 999精品在线视频| 国产97色在线日韩免费| 男女床上黄色一级片免费看| 老司机深夜福利视频在线观看| 香蕉国产在线看| 搡老岳熟女国产| 一级毛片女人18水好多| 国产成人精品久久二区二区91| 国产高清视频在线播放一区| 性欧美人与动物交配| 天堂动漫精品| 亚洲一区中文字幕在线| 免费在线观看黄色视频的| 巨乳人妻的诱惑在线观看| 亚洲 欧美一区二区三区| 色播亚洲综合网| 韩国精品一区二区三区| 中文字幕最新亚洲高清| 免费观看人在逋| 国产成人欧美| www.精华液| 亚洲av电影在线进入| 中文亚洲av片在线观看爽| 欧美色欧美亚洲另类二区 | 亚洲国产日韩欧美精品在线观看 | 欧美最黄视频在线播放免费| 国产精品久久久久久人妻精品电影| 亚洲全国av大片| 级片在线观看| 制服丝袜大香蕉在线| 每晚都被弄得嗷嗷叫到高潮| 法律面前人人平等表现在哪些方面| 久久久久久久午夜电影| 国产精品亚洲一级av第二区| 国产单亲对白刺激| 19禁男女啪啪无遮挡网站| 亚洲午夜精品一区,二区,三区| 无人区码免费观看不卡| 精品乱码久久久久久99久播| 少妇熟女aⅴ在线视频| 国产精品美女特级片免费视频播放器 | 久久久精品国产亚洲av高清涩受| av视频免费观看在线观看| 欧美日本视频| 久久久久国内视频| 国产在线观看jvid| 99精品在免费线老司机午夜| 18禁美女被吸乳视频| 欧美亚洲日本最大视频资源| 老司机午夜福利在线观看视频| 国产午夜精品久久久久久| 又紧又爽又黄一区二区| 国产亚洲欧美98| 亚洲熟妇熟女久久| 侵犯人妻中文字幕一二三四区| 操美女的视频在线观看| 亚洲av美国av| 亚洲av五月六月丁香网| aaaaa片日本免费| 亚洲久久久国产精品| 国语自产精品视频在线第100页| 97超级碰碰碰精品色视频在线观看| 中文字幕人妻丝袜一区二区| 欧美日韩精品网址| 国产区一区二久久| 啦啦啦 在线观看视频| 黑人巨大精品欧美一区二区mp4| 成年女人毛片免费观看观看9| 国产午夜精品久久久久久| 久久国产精品影院| 国产成人欧美在线观看| 久久久久久国产a免费观看| 久久国产精品影院| 久久久久国产一级毛片高清牌| 国产一区二区激情短视频| 夜夜看夜夜爽夜夜摸| 亚洲男人的天堂狠狠| 免费高清在线观看日韩|